By using an electrolyte that combines fluoroaryl sulfone and carboxylic acid ester solvents in lithium-ion batteries, a highly stable LiF interface film is formed, which solves the problem of SEI film instability caused by volume expansion of silicon-based anode materials and improves efficiency. Dynamic performance and safety performance of lithium-ion batteries.

CN118738567APending Publication Date: 2024-10-01EVE ENERGY CO LTD

Patent Information

Application Number
CN202411067239.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The volume expansion of silicon-based anode materials in lithium-ion batteries causes instability of the SEI film, which affects cycle stability and kinetic performance. The SEI film formed by existing electrolyte solvents has a high content of organic components, resulting in poor performance.

Method used

Fluorinated aryl sulfone is used as the main component of the electrolyte, combined with low-viscosity carboxylic acid ester solvents, to form a highly stable LiF interface film, reduce the viscosity of the electrolyte, increase the lithium ion transmission rate, and add fluorine-containing lithium salts such as LiPF6 , LiBF4 and LiTFSI to enhance conductivity and flame retardant properties.

Benefits of technology

It improves the first Coulomb efficiency, cycle performance, rate performance and safety performance of lithium-ion batteries, enhances the stability of the SEI film, reduces the internal resistance of the battery, and improves the lithium-ion transmission rate and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738567A_ABST
    Figure CN118738567A_ABST
Patent Text Reader

Abstract

The invention discloses an electrolyte, the electrolyte comprises fluoroaryl sulfone and a carboxylic ester solvent, the structural general formula of the fluoroaryl sulfone is as shown in the following formula (I), at least one of R1-R10 is an F atom, and R1-R10 are respectively and independently H atoms, methyl or methoxyl; in the electrolyte, the mass fraction of the fluoro aryl sulfone is greater than 15%. According to the electrolyte, through the synergistic effect of the fluoro aryl sulfone and the carboxylic ester solvent, the stability of an SEI film and the dynamic performance of the lithium ion battery are both improved, the first coulombic efficiency, the cycle performance and the rate capability of the lithium ion battery are effectively improved, and the electrolyte has a flame-retardant function and can be widely applied to the field of lithium ion batteries. And the safety performance of the lithium ion battery is improved. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of lithium ion batteries, and in particular relates to an electrolyte and a lithium ion battery. Background Art

[0002] Anode materials with high specific capacity are an important breakthrough in improving the energy density of lithium-ion batteries. Silicon-based materials are considered to be the most likely anode materials to replace graphite because of their high theoretical specific capacity (Si: 4200mAh / g, SiO: 2650mAh / g), suitable discharge potential and relatively abundant reserves in nature. However, there are many problems in the commercial application of single silicon in lithium-ion batteries. First, silicon-based materials as anodes will have volume expansion problems during battery cycles, and may cause the rupture of active particles, pulverization of pole pieces and the shedding of active materials. Secondly, the silicon anode is accompanied by a large volume expansion during the first cycle. Due to the change in silicon volume, the solid electrolyte interface film (SEI) will rupture. The newly exposed silicon on the surface will produce a new SEI film, and at the same time, it will continuously consume lithium ions in the electrolyte, reducing the first coulomb efficiency. More seriously, due to the volume change of the electrode material during the cycle, the SEI film at the silicon anode interface repeatedly grows and ruptures, greatly affecting the cycle stability.

[0003] Due to the volume effect of silicon-based negative electrode materials, it is difficult for silicon-based negative electrodes to form stable solid electrolyte interface films in the electrolyte, and the electrode structure is destroyed during the battery cycle. New solid electrolyte interface films will continue to form on the exposed silicon-based surface, leading to corrosion of the negative electrode material and capacity attenuation.

[0004] Currently, commonly used electrolyte solvents are linear carbonates and cyclic carbonates, such as dimethyl carbonate, ethyl methyl carbonate, ethylene carbonate and propylene carbonate. The SEI film formed by these solvents has a high content of organic components, resulting in poor SEI film stability and lithium-ion battery kinetic performance. Summary of the invention

[0005] In order to solve the technical problem in the above-mentioned prior art that when the electrolyte solvent is linear carbonate and cyclic carbonate, the formed SEI film has a high organic component content, resulting in poor SEI film stability and lithium ion battery kinetic performance, the purpose of the present invention is to provide an electrolyte and a lithium ion battery.

[0006] The present invention provides an electrolyte, the electrolyte comprising a fluoroaryl sulfone and a carboxylic acid ester solvent, the general structural formula of the fluoroaryl sulfone being the following formula (I):

[0007]

[0008] Among them, R1~R 10 At least one of them is a F atom, R1~R10 are each independently an H atom, a methyl group or a methoxy group;

[0009] The electrolyte includes an organic solvent, in which the mass fraction of the fluoroaryl sulfone is ≥15%.

[0010] The electrolyte of the present invention comprises fluoroaryl sulfone. In a first aspect, the fluoroaryl sulfone is a fluorinated solvent, which not only has low Li + Solvation ability, thereby improving the kinetic performance of lithium-ion batteries. On the second hand, fluoroaryl sulfones are also easy to promote the formation of LiF interface films. The formed LiF interface films have high stability and high ionic conductivity, which can improve the initial coulomb efficiency, cycle performance and rate performance of lithium-ion batteries. On the third hand, sulfones have good thermal stability, which can improve the safety performance of lithium-ion batteries. On the fourth hand, the fluorine and sulfone groups in the fluoroaryl sulfones of the present invention are directly connected to the aromatic groups, and the aromatic groups have large π bonds. The fluorine and sulfone groups are directly connected to the aromatic groups, and there is a conjugation effect, and the solvent is more stable, thereby reducing the participation of organic solvents in the formation of SEI films. Furthermore, since the fluoroaryl sulfone has a high viscosity, the present invention uses a low-viscosity carboxylic acid ester solvent and a fluoroaryl sulfone to significantly reduce the viscosity of the electrolyte, thereby increasing the lithium ion transmission rate, which can effectively improve the rate performance of lithium-ion batteries. The electrolyte of the present invention improves the stability of the SEI film and the kinetic performance of the lithium ion battery through the synergistic effect of the fluoroaryl sulfone and the carboxylic acid ester solvent, effectively improving the first cycle coulombic efficiency, cycle performance and rate performance of the lithium ion battery. The electrolyte of the present invention also has a flame retardant function, thereby improving the safety performance of the lithium ion battery.

[0011] Preferably, the fluorinated aryl sulfone comprises at least one of the following structural formulas:

[0012]

[0013]

[0014] The fluoroaryl sulfone described in this embodiment includes at least one of the above structural formulas. The above fluoroaryl sulfone can further improve the stability of the SEI film, the kinetic performance of the lithium-ion battery and the safety performance of the lithium-ion battery.

[0015] Preferably, the carboxylate solvent includes at least one of methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), methyl butyrate (MB), and methyl propionate (MP).

[0016] The carboxylic acid ester solvent described in this scheme includes at least one of methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), methyl butyrate (MB), and methyl propionate (MP), which can not only reduce the viscosity of the electrolyte and increase the lithium ion transmission rate, but also has good heat resistance, stable properties at high temperatures, low volatility, is not prone to spontaneous combustion, and is relatively safe to use.

[0017] Preferably, the electrolyte further comprises linear carbonate and cyclic carbonate.

[0018] Preferably, the mass ratio of the linear carbonate to the cyclic carbonate is 20:(15-25).

[0019] Preferably, the linear carbonate includes at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and methyl propyl carbonate (MPC).

[0020] Preferably, the cyclic carbonate includes at least one of ethylene carbonate (EC), fluoroethylene carbonate (FEC), and propylene carbonate (PC).

[0021] Preferably, the mass ratio of the fluoroaryl sulfone to the carboxylate solvent is (20-50):(10-25).

[0022] The mass ratio of the fluoroaryl sulfone to the carboxylate solvent in this embodiment is (20-50):(10-25). The mass ratio of the fluoroaryl sulfone to the carboxylate solvent within this range can further improve the flame retardancy of the electrolyte, the stability of the SEI film and the kinetic performance of the lithium-ion battery, and can fully reduce the viscosity of the electrolyte, increase the lithium ion transfer rate, and thus reduce the internal resistance of the lithium-ion battery.

[0023] Preferably, the electrolyte further comprises a fluorine-containing lithium salt, and the fluorine-containing lithium salt comprises LiPF6, LiBF4 and LiTFSI.

[0024] The fluorine-containing lithium salts described in this scheme include LiPF6, LiBF4 and LiTFSI. These three fluorine-containing lithium salts can form dense and high-strength LiF; LiBF4 has a wide operating temperature range, good stability at high temperatures and excellent low-temperature performance, and LiTFSI can improve Li + The degree of dissociation makes the electrolyte have high conductivity, thereby improving the rate performance of lithium-ion batteries. It also has good flame retardant properties, thereby improving the safety of lithium-ion batteries. Therefore, the three fluorine-containing lithium salts LiPF6, LiBF4 and LiTFSI work synergistically in the electrolyte of this scheme, so that the electrolyte of this scheme has both a wide operating temperature range and high conductivity and good flame retardant properties.

[0025] Preferably, in the electrolyte, the concentration of LiPF6 is 1-1.5 mol / L, the mass fraction of LiTFSI is 1%-3%, and the mass fraction of LiBF4 is 0.1%-0.5%.

[0026] In the electrolyte of this scheme, the concentration of LiPF6 is 1-1.5 mol / L, the mass fraction of LiTFSI is 1-3%, and the mass fraction of LiBF4 is 0.1-0.5%. In the electrolyte of this scheme, the concentrations of these three fluorine-containing lithium salts are within this range, which can not only make the electrolyte have a wide operating temperature range and high conductivity, but also make the fluorine-containing lithium salt fully dissolved and reduce the corrosion of the current collector aluminum foil.

[0027] The present invention also provides a lithium ion battery comprising the electrolyte. DETAILED DESCRIPTION

[0028] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only embodiments of a part of the present invention, rather than all embodiments.

[0029] Example 1

[0030] The structural formula of the fluorinated aryl sulfone used in the electrolyte of this embodiment is as follows:

[0031]

[0032] 4-Fluorophenyl sulfone

[0033] Preparation of electrolyte

[0034] S1. Dimethyl carbonate (DMC), fluoroethylene carbonate (FEC), ethylene carbonate (EC), fluoroaryl sulfone, and methyl acetate (MA) were mixed in a mass ratio of 20:10:10:40:20, and the mixture was stirred to obtain a first mixture;

[0035] S2. Add lithium hexafluorophosphate LiPF6 to the first mixture and stir, and after stirring and mixing evenly, obtain a second mixture;

[0036] S3. Add lithium salt additives lithium tetrafluoroborate LiBF4 and lithium bis(trifluoromethanesulfonyl)imide LiTFSI to the second mixture and stir. After stirring and mixing evenly, an electrolyte is obtained. In the electrolyte of this embodiment, the concentration of LiPF6 is 1 mol / L, the mass fraction of LiTFSI is 2%, and the mass fraction of LiBF4 is 0.3%.

[0037] Example 2

[0038] The structural formula of the fluorinated aryl sulfone used in the preparation of the electrolyte of this embodiment is as follows:

[0039] Other than that, the same as in Example 1.

[0040] Example 3

[0041] The structural formula of the fluorinated aryl sulfone used in the preparation of the electrolyte of this embodiment is as follows:

[0042] Other than that, the same as in Example 1.

[0043] Example 4

[0044] The structural formula of the fluorinated aryl sulfone used in the preparation of the electrolyte of this embodiment is as follows:

[0045] Other than that, the same as in Example 1.

[0046] Example 5

[0047] The preparation of the electrolyte in this example is the same as in Example 1, except that dimethyl carbonate (DMC), fluoroethylene carbonate (FEC), ethylene carbonate (EC), fluoroaryl sulfone, and methyl acetate (MA) are in a mass ratio of 20:10:10:55:5.

[0048] Example 6

[0049] The preparation of the electrolyte in this example is the same as in Example 1, except that dimethyl carbonate (DMC), fluoroethylene carbonate (FEC), ethylene carbonate (EC), fluoroaryl sulfone, and methyl acetate (MA) are in a mass ratio of 20:10:10:15:45.

[0050] Example 7

[0051] The preparation of the electrolyte of this embodiment is the same as that of Embodiment 1 except that the mass of LiTFSI in Embodiment 1 is replaced by the base solvent (DMC, FEC, and EC are configured as the base solvent in a mass ratio of 20:10:10).

[0052] Example 8

[0053] The preparation of the electrolyte in this embodiment is the same as that in Embodiment 1 except that the mass of LiBF4 in Embodiment 1 is replaced by the base solvent (DMC, FEC, and EC are configured as the base solvent in a mass ratio of 20:10:10).

[0054] Example 9

[0055] The preparation of the electrolyte in this embodiment is the same as that in Embodiment 1 except that the mass fraction of LiTFSI is 3.5% and the mass fraction of LiBF4 is 0.8%.

[0056] Example 10

[0057] The preparation of the electrolyte in this embodiment is the same as that in Embodiment 1 except that the mass fraction of LiTFSI is 0.7% and the mass fraction of LiBF4 is 0.05%.

[0058] Comparative Example 1

[0059] The preparation of the electrolyte of this comparative example is the same as that of Example 1, except that the mass of methyl acetate (MA) in Example 1 is replaced by the base solvent (DMC, FEC, and EC are configured as the base solvent in a mass ratio of 20:10:10).

[0060] Comparative Example 2

[0061] The preparation of the electrolyte in this comparative example is the same as that in Example 1 except that 1,3-difluoro-5-methylsulfonylbenzene is used to replace the fluoroaryl sulfone in Example 1. The structural formula of 1,3-difluoro-5-methylsulfonylbenzene is as follows:

[0062]

[0063] Comparative Example 3

[0064] The preparation of the electrolyte in this comparative example is the same as that in Example 1 except that (trifluoromethanesulfonyl)methane is used to replace the fluoroaryl sulfone in Example 1. The structural formula of (trifluoromethanesulfonyl)methane is as follows:

[0065]

[0066] Comparative Example 4

[0067] The electrolyte used in this comparative example is fluorobenzene and diphenyl sulfone, and the structural formula is as follows:

[0068]

[0069] S1. Dimethyl carbonate (DMC), fluoroethylene carbonate (FEC), ethylene carbonate (EC), fluorobenzene, diphenyl sulfone, and methyl acetate (MA) were mixed in a mass ratio of 20:10:10:38:42:20, and the mixture was stirred to obtain a first mixture;

[0070] S2. Add lithium hexafluorophosphate LiPF6 to the first mixture and stir, and after stirring and mixing evenly, obtain a second mixture;

[0071] S3. Add lithium salt additives lithium tetrafluoroborate LiBF4 and lithium bis(trifluoromethanesulfonyl)imide LiTFSI to the second mixture and stir. After stirring and mixing evenly, an electrolyte is obtained. In the electrolyte of this embodiment, the concentration of LiPF6 is 1 mol / L, the mass fraction of LiTFSI is 2%, and the mass fraction of LiBF4 is 0.3%.

[0072] Comparative Example 5

[0073] The preparation of the electrolyte in this comparative example is the same as that in Example 1 except that dimethyl sulfone is used to replace the fluoroaryl sulfone in Example 1. The structural formula of dimethyl sulfone is as follows:

[0074]

[0075] Comparative Example 6

[0076] The preparation of the electrolyte in this comparative example is the same as in Example 1 except that ethylene glycol dibutyl ether (DME) is used to replace methyl acetate (MA) in Example 1.

[0077] Preparation of lithium-ion batteries

[0078] (1) Preparation of positive electrode sheet

[0079] The positive electrode active material LiNi 0.8 Co 0.1 Mn 0.1 O2, conductive agent acetylene black and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3 and added to a solvent N-methylpyrrolidone (NMP). The mixture is evenly mixed to obtain a positive electrode slurry with a solid content of 45%. The positive electrode slurry is coated on both surfaces of the positive electrode current collector aluminum foil to form a positive electrode active coating. After vacuum drying, a positive electrode sheet is obtained.

[0080] (2) Preparation of negative electrode sheet

[0081] Silicon-carbon negative electrode material (SiC), conductive agent conductive carbon black (SP), single-walled carbon nanotubes (SWCNT) and binder polyacrylic acid (PAA) are mixed in a mass ratio of 80:9:1:10 and added to a solvent deionized water, mixed evenly, to prepare a negative electrode slurry with a solid content of 25%, and the negative electrode slurry is coated on both surfaces of the negative electrode current collector copper foil to form a negative electrode active coating, and after vacuum drying, a negative electrode sheet is prepared.

[0082] (3) Selection of electrolyte

[0083] The electrolytes obtained in the above-mentioned embodiments and comparative examples and the common electrolyte of the control group (EC:DMC:DEC mass ratio of 30:40:30, LiPF6 1 mol / L) were selected to prepare lithium-ion batteries.

[0084] (4) Selection of isolation membrane

[0085] The isolation film includes a polyethylene (PE) film and ceramic layers respectively arranged on two surfaces of the PE film, wherein the total thickness of the two ceramic layers is 3 μm, the thickness of the PE film is 9 μm, and the total thickness of the isolation film is 12 μm.

[0086] (5) Preparation of lithium-ion batteries

[0087] The positive electrode sheet, the isolation film, and the negative electrode sheet are stacked in order, and the isolation film is placed between the positive electrode sheet and the negative electrode sheet to play an isolating role, so as to prepare a bare battery cell; the bare battery cell is placed in an outer packaging shell, and after drying, an electrolyte is injected, and a lithium-ion battery is obtained through vacuum packaging, standing, forming, shaping and other processes.

[0088] Performance Testing

[0089] The rate performance of the battery was tested under lithium-ion battery test conditions, and the test was conducted on the LAND battery test system of Wuhan Jinnuo Electronics Co., Ltd. at room temperature (25°C), with the charge and discharge voltage limited to 2.5V to 4.2V. The first coulomb efficiency (first efficiency), cycle performance and rate performance are shown in Table 1 below.

[0090] 1) First Coulomb efficiency

[0091] At 25°C, the lithium-ion battery was charged to 4.2V at a constant current and constant voltage rate of 0.33C and allowed to stand for 10 minutes. Then, the lithium-ion battery was discharged to 2.5V at a constant current rate of 0.33C and allowed to stand for 10 minutes. The first coulombic efficiency of the lithium-ion battery was calculated.

[0092] First coulombic efficiency (%) = total capacity of the lithium-ion battery discharged at 0.33C for the first time / total capacity of the lithium-ion battery charged at 0.33C for the first time × 100%.

[0093] 2) Capacity retention rate after 900 cycles at room temperature 1C / 1C

[0094] At 25°C, the lithium-ion battery is charged to 4.2V at a constant current and constant voltage rate of 1C, with a cut-off current of 0.05C, and allowed to stand for 10 minutes. Then, the lithium-ion battery is discharged to 2.5V at a constant current rate of 1C and allowed to stand for 10 minutes. This is considered one charge and discharge cycle. The lithium-ion battery is charged and discharged for 900 cycles according to the above method, and the capacity retention rate of the lithium-ion battery after 900 cycles of charge and discharge at 1C / 1C is calculated.

[0095] The capacity retention rate (%) of a lithium-ion battery after N cycles = (discharge capacity at the Nth cycle / initial discharge capacity) × 100%, where N is the number of cycles of the lithium-ion battery.

[0096] 3) 1C / 8C discharge capacity retention rate at room temperature

[0097] At 25°C, the divided lithium-ion battery is charged to 4.2V at a constant current and constant voltage rate of 1C, with a cut-off current of 0.05C; it is left to stand for 10 minutes; then the lithium-ion battery is discharged to 2.5V at a constant current rate of 1C, and its discharge capacity Q is recorded. 1C As the initial discharge capacity; then charge the lithium-ion battery to 4.2V at 1C rate at 25°C, with a cut-off current of 0.05C; let it stand for 10 minutes; then discharge the fully charged battery to 2.5V at 8C rate, and record its discharge capacity Q 8C ; Calculate the discharge capacity retention rate (%) of the lithium-ion battery at 1C / 8C rate = discharge capacity Q at 8C rate 8C / Discharge capacity at 1C rate Q 1C ×100%.

[0098] 4) Battery thermal runaway ARC (adiabatic accelerated calorimeter) test

[0099] The lithium-ion battery is heated from room temperature to 45±2℃ in the chamber. After being left for 90 minutes, the temperature rise rate of the battery is detected. If the temperature rise exceeds 0.2℃ within 10 minutes (i.e., the self-heating temperature rise rate SHR>0.02℃ / min), it is considered that a self-exothermic reaction occurs inside the lithium-ion battery, and the adiabatic environment is maintained until the lithium-ion battery has thermal runaway; if the temperature rise does not exceed 0.2℃ within 10 minutes (i.e., the self-heating temperature rise rate SHR≤0.02℃ / min), continue to the next step temperature rise test; each temperature step is 5℃, and the steps are repeated on each step. The ARC test temperature range is 45-300℃, the self-heating starting temperature is T1 (temperature rise rate SHR>0.02℃ / min), and the thermal runaway starting temperature is T2 (temperature rise rate SHR>1℃ / min).

[0100] Table 1

[0101]

[0102]

[0103] From the analysis of Table 1, we can see that:

[0104] After the electrolytes of Examples 1 to 10 of the present invention are used to prepare lithium-ion batteries, they show good performance in the first coulombic efficiency, cycle capacity retention rate, high-rate discharge capacity retention rate (fast charge and discharge) and battery thermal runaway ARC test (self-heating starting temperature T1 and thermal runaway starting temperature T2), while Comparative Examples 1 to 6 and the control group do not belong to the technical scheme of the present invention, so their performance in the above four aspects is significantly deteriorated. This shows that the electrolyte prepared using the technical scheme of the present invention is applied to lithium batteries, which can effectively improve the first coulombic efficiency, cycle performance, rate performance and flame retardant performance (i.e. safety performance) of lithium-ion batteries.

[0105] Compared with the fluoroaryl sulfone used in Example 1, the fluorine content of the fluoroaryl sulfone and the substitution site of the F atom on the phenyl group in the electrolytes of Examples 2 and 3 are different. The fluoroaryl sulfone in Example 4 contains other non-F substituents on the aromatic group, namely, methoxy. Comparative Example 2 is 1,3-difluoro-5-methylsulfonylbenzene, Comparative Example 3 is (trifluoromethylsulfonyl) methane, which is a fluoroalkyl sulfone, and Comparative Example 5 is dimethyl sulfone. The fluoroaryl sulfones used in Examples 1 to 4 meet the general structural formula of the fluoroaryl sulfone of the present invention. From the test results in Table 1, the lithium ion batteries prepared using the electrolytes of Examples 1 to 4 also show good technical effects in the first coulomb efficiency, cycle capacity retention rate, high rate discharge capacity retention rate and battery thermal runaway ARC test. However, the structural formulas of the other solvents used in Comparative Examples 2, 3 and 5 to replace the fluoroaryl sulfone in Example 1 do not satisfy the general structural formula of the fluoroaryl sulfone of the present invention. From the test results in Table 1, the technical effects of the lithium ion batteries prepared using the electrolytes of Comparative Examples 2, 3 and 5 in the first coulombic efficiency, cycle capacity retention rate, high-rate discharge capacity retention rate and battery thermal runaway ARC test are significantly reduced.

[0106] Compared with Example 1, the electrolyte of Example 5 uses more fluoroaryl sulfones - the mass ratio of fluoroaryl sulfones to carboxylic acid ester solvents is 55:5, and the electrolyte of Example 6 uses less fluoroaryl sulfones - the mass ratio of fluoroaryl sulfones to carboxylic acid ester solvents is 15:45. Both Example 5 and Example 6 are not within the further preferred range of the mass ratio of fluoroaryl sulfones to carboxylic acid ester solvents of (20-50):(10-25). In Example 5, a large amount of fluoroaryl sulfones is used, and the viscosity of the prepared electrolyte is large, and the lithium ion transmission rate is reduced. From the test results in Table 1, the technical effect of the lithium ion battery prepared using the electrolyte of Example 5 is reduced in terms of the high-rate discharge capacity retention rate. In Example 6, a small amount of fluoroaryl sulfones is used, which promotes the formation of less LiF interface film with high stability and ionic conductivity, reduces the thermal stability of the electrolyte and the stability of the fluoroaryl sulfone solvent, and reduces Li +The solvation capacity is also reduced, and the technical effect of the lithium-ion battery prepared using the electrolyte of Example 5 in the battery thermal runaway ARC test is reduced.

[0107] Compared with Example 1, no LiTFSI is added to the electrolyte of Example 7, and no LiBF4 is added to the electrolyte of Example 8. The mass fractions of LiTFSI and LiBF4 in the electrolytes of Examples 9 and 10 are not in the preferred range - the mass fraction of LiTFSI is 1% to 3%, and the mass fraction of LiBF4 is 0.1% to 0.5%, that is, the mass fractions of LiTFSI and LiBF4 in the electrolyte of Example 9 are both greater than the preferred range, and the mass fractions of LiTFSI and LiBF4 in the electrolyte of Example 10 are both less than the preferred range. From the test results in Table 1, the technical effects of the lithium-ion battery prepared using the electrolyte of Example 7 in the first coulomb efficiency, cycle capacity retention rate and battery thermal runaway ARC test are better than those of Example 9. The mass fractions of LiTFSI and LiBF4 in the electrolyte of Example 9 are not in the preferred range, and the technical effect is not as good as that of Example 7 (without adding LiTFSI), which shows that in the electrolyte, the combination of LiTFSI and LiBF4 and their respective mass fractions within the preferred range can achieve unexpected synergistic technical effects.

[0108] Compared with Example 1, Comparative Example 1 does not use a carboxylic acid ester solvent, and the viscosity of the prepared electrolyte is very high, the movement of lithium ions is hindered, the insertion and extraction of lithium ions on the negative electrode surface breaks the equilibrium state, and lithium ions are deposited on the negative electrode surface to cause lithium precipitation. At the same time, the obstruction of the movement of lithium ions will also generate heat. Therefore, compared with Example 1, the lithium ion battery prepared using the electrolyte of Comparative Example 1 has significantly reduced technical effects in the first coulomb efficiency, cycle capacity retention rate, high-rate discharge capacity retention rate and battery thermal runaway ARC test.

[0109] The fluorobenzene and diphenyl sulfone used in Comparative Example 4, the combination of fluorobenzene and diphenyl sulfone meets the functional group characteristics of the fluoroaryl sulfone in Example 1, that is, the F atom is connected to the phenyl group, and there is also a symmetrical diphenyl sulfone. From the test results in Table 1, the lithium ion battery prepared using the electrolyte of Comparative Example 4 has significantly reduced technical effects in the first coulomb efficiency, cycle capacity retention rate, high-rate discharge capacity retention rate and battery thermal runaway ARC test. This shows that even if the solvent used simultaneously meets the functional group characteristics of the structural formula of the fluoroaryl sulfone in the technical solution of the present invention, it is not possible to simultaneously achieve the above four technical effects by replacing the fluoroaryl sulfone in the technical solution of the present invention.

[0110] Comparative Example 6 uses ethylene glycol dibutyl ether (DME) to replace methyl acetate (MA) in Example 1, that is, the low-viscosity carboxylic acid ester solvent in the technical solution of the present invention is not used, but a low-viscosity ether solvent is used. From the test results in Table 1, the lithium ion battery prepared using the electrolyte of Comparative Example 6 has significantly reduced technical effects in the first coulombic efficiency, cycle capacity retention rate, high-rate discharge capacity retention rate and battery thermal runaway ARC test. This shows that even if other low-viscosity ether solvents are used, the technical effects of the above four aspects cannot be achieved at the same time. The fluoroaryl sulfone in the technical solution of the present invention needs to be matched with a carboxylic acid ester solvent, which is a necessary technical feature to achieve the technical effects of the present invention.

[0111] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. An electrolyte, characterized in that: The electrolyte comprises a fluoroaryl sulfone and a carboxylic acid ester solvent, and the general structural formula of the fluoroaryl sulfone is the following formula (I): Among them, R1~R 10 At least one of them is a F atom, R1~R 10 are each independently an H atom, a methyl group or a methoxy group; The electrolyte includes an organic solvent, and the mass fraction of the fluoroaryl sulfone in the organic solvent is ≥15%.

2. The electrolyte according to claim 1, characterized in that The fluoroaryl sulfone includes at least one of the following structural formulas:

3. The electrolyte according to claim 1, characterized in that The carboxylate solvent includes at least one of methyl formate, methyl acetate, ethyl acetate, methyl butyrate, and methyl propionate.

4. The electrolyte according to claim 1, characterized in that The electrolyte also includes linear carbonate and cyclic carbonate.

5. The electrolyte according to claim 4, characterized in that The linear carbonate includes at least one of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, and methyl propyl carbonate.

6. The electrolyte according to claim 4, characterized in that The cyclic carbonate includes at least one of ethylene carbonate, fluoroethylene carbonate, and propylene carbonate.

7. The electrolyte according to claim 1, characterized in that The mass ratio of the fluoroaryl sulfone to the carboxylate solvent is (20-50):(10-25).

8. The electrolyte according to claim 1, characterized in that The electrolyte further includes a fluorine-containing lithium salt, and the fluorine-containing lithium salt includes LiPF6, LiBF4 and LiTFSI.

9. The electrolyte according to claim 8, characterized in that In the electrolyte, the concentration of LiPF6 is 1-1.5 mol / L, the mass fraction of LiTFSI is 1%-3%, and the mass fraction of LiBF4 is 0.1%-0.5%.

10. A lithium ion battery, characterized in that: The electrolyte comprises the electrolyte according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Separators, articles and methods of making thereof

    CN109565015A

  • Lithium ion battery electrolyte and lithium ion battery containing same

    CN111146499A

  • Lithium ion battery electrolyte and lithium ion battery

    CN114284558A

  • Wide-temperature-range high-voltage sodium-ion battery electrolyte and sodium-ion battery

    CN118315668A

  • Electrolyte for rechargeable lithium battery andrechargeable lithium battery comprising same

    KR1020050029971A

Cited By

  • Safe lithium ion battery for unmanned aerial vehicle and preparation method of safe lithium ion battery