Zinc ion battery electrolyte for increasing ion solvation structure entropy as well as preparation method and application of zinc ion battery electrolyte
By using zinc ion electrolyte with the synergistic participation of polyanions in zinc ion batteries, the solvation structure entropy and interface characteristics are adjusted, the problems of dendrite growth and side reactions in zinc ion batteries are solved, the conductivity and cycle life are improved, and Costs are reduced and more efficient electrochemical performance is achieved.
Patent Information
- Application Number
- CN202411102929.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-10-01
AI Technical Summary
In existing aqueous zinc-ion batteries, the thermodynamic instability of solvated zinc ions and unstable electrode/electrolyte interface lead to side reactions such as dendrite growth, hydrogen evolution reaction, and corrosion, resulting in low zinc utilization, low Coulombic efficiency, and short cycle life. .
Using a zinc-ion battery electrolyte with the synergistic participation of multiple anions, a combination of soluble zinc salts such as zinc sulfate, inorganic anionic zinc salts and organic anionic zinc salts is used to form strong coupling, adjust the solvation structure entropy, reduce the size of zinc ion clusters, and enhance migration. kinetics, and modify the solid electrolyte interface through polyanion adsorption, reducing strong hydrogen bonds and active water.
It significantly improves the migration kinetics and conductivity of zinc ions, inhibits dendrite growth and side reactions, extends the cycle life and electrochemical performance stability of zinc-ion batteries, reduces processing costs, and is compatible with industrial applications.
Smart Images

Figure CN118738600A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a zinc ion battery electrolyte, in particular to a zinc ion battery electrolyte capable of increasing ion solvation structural entropy and improving ion conductivity, and a preparation method and application thereof, belonging to the technical field of zinc ion batteries. Background Art
[0002] The development of lithium-ion batteries has been limited by the high cost of preparation and safety issues caused by the flammability of organic electrolytes. In contrast, aqueous zinc-ion batteries have attracted increasing attention due to the inherent safety and environmental characteristics of their electrolytes and their economic advantages.
[0003] Metal zinc has a high specific capacity (820mAh g -1 ), low redox potential (-0.76V relative to standard hydrogen electrode), abundant resources, and non-flammability, and are considered to be ideal negative electrode materials for aqueous zinc-ion batteries. However, due to the thermodynamic instability of solvated zinc ions and the unstable electrode / electrolyte interface causing side reactions such as dendrite growth, hydrogen evolution reaction, and corrosion, low zinc utilization, low Coulombic efficiency, and short cycle life.
[0004] Strategies such as electrolyte optimization, interface engineering, and Zn electrode architecture have been developed to address these challenges, among which electrolyte regulation is widely regarded as a promising approach due to its feasibility and effectiveness. However, this approach still has some disadvantages. In particular, while the use of organic additives has shown significant effects in stabilizing Zn anodes by correlating electric double layer capacitance and optimizing solvation structure and hydrogen bonding network, these solutions often lead to poor ionic conductivity, sluggish diffusion rate kinetics, insufficient cycle life under harsh conditions, and increased flammability risk. The use of metal salt additives can produce dendrite-free Zn anodes through interfacial absorption or electrostatic screening. However, the introduction of metal ions not only has limited improvement on the stability of Zn anode under aqueous conditions, but more importantly, the potential deposition / stripping mechanism of the introduced cations remains elusive. In addition, while designing high-concentration electrolytes can reduce water activity by disrupting hydrogen bonding networks, it also leads to increased viscosity, reduced ion diffusion kinetics, and other economic defects, greatly limiting its practical applicability. Therefore, creating a new aqueous electrolyte composed only of Zn salts is essential to enhance highly reversible Zn anodes, extend service life, and improve cost-effectiveness. Summary of the invention
[0005] The main purpose of the present invention is to provide an aqueous zinc ion battery electrolyte and a preparation method thereof which can increase the ion solvation structural entropy and improve the ion conductivity, so as to overcome the deficiencies in the prior art.
[0006] Another object of the present invention is to provide an application of the zinc ion battery electrolyte.
[0007] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:
[0008] An embodiment of the present invention provides a zinc ion battery electrolyte for increasing ion solvation structural entropy, comprising: a soluble zinc salt and a solvent, wherein the soluble zinc salt comprises a combination of zinc sulfate, an inorganic anion zinc salt and an organic anion zinc salt, wherein the inorganic anion zinc salt comprises any one or a combination of two or more of zinc chloride, zinc bromide, zinc nitrate, zinc phosphate, zinc perchlorate, and zinc fluoroborate, and the organic anion zinc salt comprises any one or a combination of two or more of zinc trifluoromethanesulfonate, zinc bis(trifluoromethylsulfonyl)imide, zinc bis(difluoromethylsulfonyl)(trifluoromethylxanthyl)imide, zinc undecylenate, zinc N-(benzenesulfonyl)benzenesulfonamide, zinc tetrakis(hexafluoroisopropoxy)borate, zinc gluconate, and zinc carbonate, and the types of the soluble zinc salt are five or more.
[0009] An embodiment of the present invention also provides a method for preparing the aforementioned zinc ion battery electrolyte for increasing the ion solvation structural entropy, which comprises: dissolving a soluble zinc salt as an electrolyte in a solvent, stirring and mixing evenly, and obtaining the zinc ion battery electrolyte for increasing the ion solvation structural entropy.
[0010] The embodiments of the present invention also provide the use of the aforementioned zinc ion battery electrolyte for increasing the ion solvation structural entropy in an aqueous zinc ion battery or a zinc ion electrochemical energy storage device.
[0011] Correspondingly, an embodiment of the present invention further provides an aqueous zinc ion battery, which includes: a positive electrode, a negative electrode, a separator and an electrolyte, wherein the electrolyte is the aforementioned zinc ion battery electrolyte that increases the ion solvation structural entropy.
[0012] Compared with the prior art, the present invention has the following beneficial effects:
[0013] 1) The zinc ion battery electrolyte provided by the present invention increases the solvation structural entropy of zinc ions through the synergistic participation of multiple anions, reduces the size of zinc ion clusters, enhances the migration kinetics of zinc ions, and improves ionic conductivity; at the same time, the number of strong hydrogen bonds in the system is reduced, and the activity of bound water and free water is reduced; further, the multiple anions adsorb and modify the solid electrolyte interface film protective layer, which can effectively reduce the desolvation ability of zinc ions, uniformly distribute the interface current density, and promote the uniform distribution of zinc ions at the interface; thereby inhibiting uncontrollable dendrite growth, significantly reducing the occurrence of side reactions such as hydrogen evolution and corrosion, extending the cycle life of the zinc ion battery and improving the electrochemical performance stability of the full battery;
[0014] 2) The preparation method of the zinc ion battery electrolyte provided by the present invention is simple and easy, has low processing cost, and has strong universality and industrial application compatibility. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0016] Figure 1 It is a schematic diagram of the ionic conductivity test results of the zinc ion battery electrolyte obtained using Example 1 of the present invention and Comparative Example 1;
[0017] Figure 2 The Zn||Zn symmetric button cells assembled using the zinc ion battery electrolytes obtained in Example 1, Comparative Example 1, Comparative Example 2, Comparative Example 3, and Comparative Example 4 of the present invention were subjected to an electrochemical reaction at 10 mA cm -2 and 5mAh cm -2 Time-voltage curve under test conditions;
[0018] Figure 3 The Zn||Zn symmetrical button cells assembled using the zinc ion battery electrolytes obtained in Examples 1, 2, 3, 4, and Comparative Example 1 of the present invention were subjected to an electrochemical reaction at 10 mA cm -2 and 5mAh cm -2 Time-voltage curve under test conditions;
[0019] Figure 4 The Zn||Zn symmetric button cells assembled using the zinc ion battery electrolytes obtained in Example 1 and Comparative Example 1 of the present invention were tested at 1 mA cm -2 and 0.5 mAh cm -2 Time-voltage curve under test conditions;
[0020] Figure 5a , Figure 5b The scanning electron microscope comparison images of the zinc negative electrode surface of the Zn||Zn symmetrical button cells assembled with the zinc ion battery electrolytes in Example 1 of the present invention and Comparative Example 1 after 100 hours of circulation;
[0021] Figure 6 Zn||MnO assembled in Example 1 of the present invention and Comparative Example 1 2 Comparison of the discharge specific capacity-cycle number curves of aqueous zinc-ion full batteries. DETAILED DESCRIPTION
[0022] In view of the defects of the prior art, the inventors of this case have proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution mainly provides an aqueous zinc ion battery electrolyte that increases the structural entropy of ion solvation, which can effectively improve the ionic conductivity, inhibit the uncontrollable growth of zinc dendrites, and reduce the occurrence of hydrogen evolution and corrosion side reactions, thereby improving the electrochemical cycle life of the zinc ion battery.
[0023] The technical solution, its implementation process and principle are further explained as follows. However, it should be understood that within the scope of the present invention, the above-mentioned technical features of the present invention and the technical features specifically described in the following (embodiments) can be combined with each other to form a new or preferred technical solution. Due to space limitations, they will not be described one by one here.
[0024] As one aspect of the technical solution of the present invention, a zinc ion battery electrolyte for increasing the structural entropy of ion solvation comprises a soluble zinc salt and a solvent.
[0025] In some specific embodiments, the soluble zinc salt includes a combination of zinc sulfate, an inorganic anion zinc salt and an organic anion zinc salt, and the soluble zinc salt contains five or more inorganic anions and organic anions, which can induce a weak solvation structure. The two types of anions used in the present invention can form a strong coupling with zinc ions, adjust the diversity of solvation structures, enhance ion dissociation and reduce the size of ion clusters, improve ion migration kinetics and increase ion conductivity, and achieve uniform and reversible deposition of zinc. Organic anions participate in the regulation of hydrogen bond networks in free water, reduce the reactivity of water through dipole, hydrogen bond and other effects, and inhibit hydrogen evolution reaction.
[0026] In some preferred embodiments, the inorganic anion zinc salt may include any one or a combination of two or more of zinc chloride, zinc bromide, zinc nitrate, zinc phosphate, zinc perchlorate, zinc fluoroborate, etc., but is not limited thereto.
[0027] In some preferred embodiments, the organic anion zinc salt can be any one of zinc trifluoromethanesulfonate, zinc bis(trifluoromethylsulfonyl)imide, zinc bis(difluoromethylsulfonyl)(trifluoromethylxanthoxy)imide, zinc undecylenate, zinc N-(benzenesulfonyl)benzenesulfonamide, zinc tetrakis(hexafluoroisopropoxy)borate, zinc gluconate, zinc carbonate, zinc acetate, etc., or a combination of two or more thereof, but is not limited thereto.
[0028] In some specific embodiments, the solvent includes water, preferably ultrapure water, but not limited thereto.
[0029] In some specific embodiments, the zinc ion battery electrolyte includes: zinc sulfate, and four or more of inorganic anion zinc salts and organic anion zinc salts. That is, from another perspective, the soluble zinc salt combination is based on zinc sulfate salt, and at least one of inorganic anion zinc salts, at least one of organic anion zinc salts, etc., a total of four or more zinc salt combinations are added.
[0030] In some specific embodiments, the concentration of soluble zinc salt (ie, zinc ions) in the zinc ion battery electrolyte is 1 to 3 mol / L.
[0031] In some specific embodiments, the concentration of zinc sulfate in the zinc ion battery electrolyte is 0.2-2.0 mol / L, and the sum of the concentrations of the other four or more soluble zinc salts is 0.8-2.8 mol / L.
[0032] In some more preferred embodiments, the concentration of zinc sulfate in the zinc ion battery electrolyte is 0.4 to 1.6 mol / L, preferably 0.8 to 1.6 mol / L, and the concentration of the other four or more soluble zinc salts is 0.4 to 1.6 mol / L. For example, the concentration of zinc sulfate is independently selected from any value selected from 0.4 mol / L, 0.8 mol / L, 1.2 mol / L, 1.6 mol / L, or a range between any two values.
[0033] Furthermore, the molar ratios of the other four or more soluble zinc salts in the zinc ion battery electrolyte are equal.
[0034] In some more preferred embodiments, the other four or more soluble zinc salts in the zinc ion battery electrolyte may include a combination of zinc chloride, zinc bromide, zinc trifluoromethanesulfonate and zinc perchlorate.
[0035] In a preferred embodiment, the zinc ion battery electrolyte comprises zinc sulfate, zinc chloride, zinc bromide, zinc trifluoromethanesulfonate and zinc perchlorate.
[0036] Furthermore, the molar ratio of the soluble zinc salts zinc chloride, zinc bromide, zinc trifluoromethanesulfonate and zinc perchlorate in the zinc ion battery electrolyte is equal to 1:1:1:1.
[0037] Furthermore, the concentrations of the other four or more soluble zinc salts in the zinc ion battery electrolyte can all independently be 0.1 to 0.5 mol / L. More specifically, the concentrations of the soluble zinc salts zinc chloride, zinc bromide, zinc trifluoromethanesulfonate and zinc perchlorate are independently selected from any value selected from 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L or any range value between two of them.
[0038] The zinc ion battery electrolyte provided by the present invention increases the solvation structural entropy of zinc ions through the synergistic participation of multiple anions. Two types of anions form a strong coupling with zinc ions due to electrostatic action and participate in the construction of ion solvation shells, thereby enriching the diversity of solvation structures, increasing structural entropy, reducing the size of zinc ion clusters, enhancing the migration kinetics of zinc ions, and improving ion conductivity; at the same time, organic anions reduce the number of strong hydrogen bonds in the system and reduce the activity of bound water and free water; further, multiple anions adsorb and modify the solid electrolyte interface film protective layer, effectively reduce the desolvation ability of zinc ions, uniformly distribute the interface current density, and promote the uniform distribution of zinc ions at the interface; thereby inhibiting uncontrollable dendrite growth, significantly reducing the occurrence of side reactions such as hydrogen evolution and corrosion, extending the cycle life of the zinc ion battery, and improving the electrochemical performance stability of the full battery.
[0039] As another aspect of the technical solution of the present invention, it also relates to a method for preparing the aforementioned zinc ion battery electrolyte for increasing the ion solvation structural entropy, which comprises: dissolving a soluble zinc salt as an electrolyte in a solvent, stirring and mixing evenly, and obtaining the zinc ion battery electrolyte for increasing the ion solvation structural entropy.
[0040] In summary, the preparation method of the zinc ion battery electrolyte of the present invention is simple and easy, has low processing cost, and has strong universality and industrial application compatibility.
[0041] As another aspect of the technical solution of the present invention, it also relates to the application of the aforementioned zinc ion battery electrolyte that increases the ion solvation structural entropy in an aqueous zinc ion battery or a zinc ion electrochemical energy storage device.
[0042] Correspondingly, as another aspect of the technical solution of the present invention, it also relates to an aqueous zinc ion battery, which comprises: a positive electrode, a negative electrode, a separator and an electrolyte, wherein the electrolyte is the aforementioned zinc ion battery electrolyte that increases the ion solvation structural entropy.
[0043] In some embodiments, the active material contained in the positive electrode may include at least one of vanadium oxide compounds, manganese oxide compounds, Prussian blue compounds, etc., preferably manganese oxide compounds, such as MnO 2 , but not limited to this.
[0044] In some embodiments, the negative electrode may include at least any one of zinc foil, zinc sheet, zinc wire, zinc powder, zinc foam, zinc plate, zinc alloy, etc., but is not limited thereto.
[0045] In some embodiments, the membrane may be a commercially available membrane, for example, may preferably include a glass fiber membrane.
[0046] In summary, the aqueous zinc ion battery electrolyte provided by the present invention that increases the ion solvation structural entropy can effectively improve the ionic conductivity and ion migration number during the charge and discharge process, homogenize the local current density distribution at the electrode-electrolyte interface and reduce the ion concentration polarization, modify the solid electrolyte interface film, prevent the formation and growth of dendrites, and the occurrence of corrosion reactions, and extend the battery cycle life. In addition, experiments have shown that the zinc ion battery prepared using the zinc ion battery electrolyte of the present application and the vanadium oxide positive electrode material has obvious improvements in terms of capacity retention, cycle performance and rate performance.
[0047] The present application is further described in detail below in conjunction with a series of preferred embodiments and the accompanying drawings, and the described embodiments are only a part of embodiments of the present invention, and are not limited to these embodiments when selected in practical applications. It should be noted in addition that the embodiments described below are intended to facilitate the understanding of the present invention, and do not play any limiting role thereto. All other embodiments obtained by those skilled in the relevant art without making any creative work, all belong to the scope of protection of the present invention. The experimental materials adopted in the embodiments used below, if not otherwise specified, can all be purchased by conventional reagent companies.
[0048] Example 1
[0049] The invention discloses a preparation step of a zinc ion battery electrolyte for increasing ion solvation structural entropy, comprising: adding zinc sulfate, zinc chloride, zinc bromide, zinc perchlorate and zinc trifluoromethanesulfonate to water at room temperature, stirring the water until the water is completely dissolved, and obtaining 20 mL of zinc ion battery electrolyte, wherein the concentrations of zinc sulfate, zinc chloride, zinc bromide, zinc perchlorate and zinc trifluoromethanesulfonate are 1.2 mol / L, 0.2 mol / L, 0.2 mol / L, 0.2 mol / L and 0.2 mol / L, respectively.
[0050] Example 2
[0051] The invention discloses a preparation step of a zinc ion battery electrolyte for increasing ion solvation structural entropy, comprising: adding zinc sulfate, zinc chloride, zinc bromide, zinc perchlorate and zinc trifluoromethanesulfonate to water at room temperature, stirring the water until the water is completely dissolved, and obtaining 20 mL of zinc ion battery electrolyte, wherein the concentrations of zinc sulfate, zinc chloride, zinc bromide, zinc perchlorate and zinc trifluoromethanesulfonate are 1.0 mol / L, 0.5 mol / L, 0.5 mol / L, 0.5 mol / L and 0.5 mol / L, respectively.
[0052] Example 3
[0053] The invention discloses a preparation step of a zinc ion battery electrolyte for increasing ion solvation structural entropy, comprising: adding zinc sulfate, zinc chloride, zinc bromide, zinc perchlorate and zinc trifluoromethanesulfonate to water at room temperature, stirring the water until the water is completely dissolved, and obtaining 20 mL of zinc ion battery electrolyte, wherein the concentrations of zinc sulfate, zinc chloride, zinc bromide, zinc perchlorate and zinc trifluoromethanesulfonate are 0.8 mol / L, 0.3 mol / L, 0.3 mol / L, 0.3 mol / L and 0.3 mol / L, respectively.
[0054] Example 4
[0055] The invention discloses a preparation step of a zinc ion battery electrolyte for increasing ion solvation structural entropy, comprising: adding zinc sulfate, zinc chloride, zinc bromide, zinc perchlorate and zinc trifluoromethanesulfonate to water at room temperature, stirring the water until the water is completely dissolved, and obtaining 20 mL of zinc ion battery electrolyte, wherein the concentrations of zinc sulfate, zinc chloride, zinc bromide, zinc perchlorate and zinc trifluoromethanesulfonate are 0.4 mol / L, 0.4 mol / L, 0.4 mol / L, 0.4 mol / L and 0.4 mol / L, respectively.
[0056] Example 5
[0057] The invention discloses a preparation step of a zinc ion battery electrolyte for increasing the structural entropy of ion solvation, comprising: adding zinc sulfate, zinc nitrate, zinc phosphate, zinc trifluoromethanesulfonate and zinc perchlorate to water at room temperature, stirring the water until the water is completely dissolved, and obtaining 20 mL of zinc ion battery electrolyte, wherein the concentrations of zinc sulfate, zinc nitrate, zinc phosphate, zinc perchlorate and zinc trifluoromethanesulfonate are 0.2 mol / L, 0.2 mol / L, 0.2 mol / L, 0.2 mol / L and 0.2 mol / L, respectively.
[0058] Example 6
[0059] The invention discloses a preparation step of a zinc ion battery electrolyte for increasing the structural entropy of ion solvation, comprising: adding zinc sulfate, zinc chloride, zinc nitrate, zinc phosphate, zinc fluoroborate and zinc trifluoromethanesulfonate to water at room temperature, stirring the water until the water is completely dissolved, and obtaining 20 mL of zinc ion battery electrolyte, wherein the concentrations of zinc sulfate, zinc chloride, zinc nitrate, zinc phosphate, zinc fluoroborate and zinc trifluoromethanesulfonate are 0.5 mol / L, 0.5 mol / L, 0.5 mol / L, 0.5 mol / L, 0.5 mol / L and 0.5 mol / L, respectively.
[0060] Example 7
[0061] The invention discloses a preparation step of a zinc ion battery electrolyte for increasing the structural entropy of ion solvation, comprising: adding zinc sulfate, zinc chloride, zinc trifluoromethanesulfonate, zinc bis(difluoromethylsulfonyl)(trifluoromethylxanthoxy)imide and zinc undecylenate to water at room temperature, stirring the mixture until the mixture is completely dissolved, and obtaining 20 mL of zinc ion battery electrolyte, wherein the concentrations of zinc sulfate, zinc chloride, zinc trifluoromethanesulfonate, zinc bis(difluoromethylsulfonyl)(trifluoromethylxanthoxy)imide and zinc undecylenate are 2.0 mol / L, 0.2 mol / L, 0.2 mol / L, 0.2 mol / L and 0.2 mol / L, respectively.
[0062] Example 8
[0063] The invention discloses a preparation step of a zinc ion battery electrolyte for increasing ion solvation structural entropy, comprising: adding zinc sulfate, zinc nitrate, zinc fluoroborate, zinc trifluoromethanesulfonate, zinc undecylenate, zinc N-(phenylsulfonyl)benzenesulfonamide, and zinc tetrakis(hexafluoroisopropoxy)borate to water at room temperature, and stirring the mixture until the mixture is completely dissolved to obtain 20 mL of zinc ion battery electrolyte, wherein the concentrations of zinc sulfate, zinc nitrate, zinc fluoroborate, zinc trifluoromethanesulfonate, zinc undecylenate, zinc N-(phenylsulfonyl)benzenesulfonamide, and zinc tetrakis(hexafluoroisopropoxy)borate are 1.2 mol / L, 0.1 mol / L, 0.1 mol / L, 0.2 mol / L, 0.2 mol / L, 0.2 mol / L, and 0.2 mol / L, respectively.
[0064] Example 9
[0065] The invention discloses a preparation step of a zinc ion battery electrolyte for increasing ion solvation structural entropy, comprising: adding zinc sulfate, zinc chloride, zinc nitrate, zinc trifluoromethanesulfonate, zinc gluconate, zinc carbonate and zinc acetate to water at room temperature, and stirring the water until the water is completely dissolved to obtain 20 mL of zinc ion battery electrolyte, wherein the concentrations of the zinc sulfate, zinc chloride, zinc nitrate, zinc trifluoromethanesulfonate, zinc gluconate, zinc carbonate and zinc acetate are 1.6 mol / L, 0.2 mol / L, 0.2 mol / L, 0.2 mol / L, 0.2 mol / L, 0.2 mol / L and 0.2 mol / L, respectively.
[0066] Comparative Example 1
[0067] The invention discloses a preparation step of a zinc ion battery electrolyte, comprising: adding zinc sulfate into water at room temperature, stirring the water until the water is completely dissolved, and obtaining 20 mL of the zinc ion battery electrolyte, wherein the concentration of the zinc sulfate is 2 mol / L.
[0068] Comparative Example 2
[0069] The invention discloses a preparation step of a zinc ion battery electrolyte, comprising: adding zinc sulfate and zinc trifluoromethanesulfonate to water at room temperature, stirring the water until the water is completely dissolved, and obtaining 20 mL of the zinc ion battery electrolyte, wherein the concentrations of zinc sulfate and zinc chloride are 1.2 mol / L and 0.8 mol / L, respectively.
[0070] Comparative Example 3
[0071] The invention discloses a preparation step of a zinc ion battery electrolyte, comprising: adding zinc sulfate, zinc chloride and zinc trifluoromethanesulfonate to water at room temperature, stirring the mixture until the mixture is completely dissolved, and obtaining 20 mL of the zinc ion battery electrolyte, wherein the concentrations of the zinc sulfate, zinc chloride and zinc trifluoromethanesulfonate are 1.2 mol / L, 0.4 mol / L and 0.4 mol / L respectively.
[0072] Comparative Example 4
[0073] The invention discloses a preparation step of a zinc ion battery electrolyte, comprising: adding zinc sulfate, zinc chloride, zinc trifluoromethanesulfonate and zinc perchlorate to water at room temperature, and stirring the water until the water is completely dissolved to obtain 20 mL of the zinc ion battery electrolyte, wherein the concentrations of the zinc sulfate, zinc chloride, zinc trifluoromethanesulfonate and zinc perchlorate are 1.2 mol / L, 0.2 mol / L, 0.2 mol / L and 0.2 mol / L respectively.
[0074] Under the conditions of the above-mentioned comparative examples 1-4, due to the small number of anion types, the regulating effect on the solvation structure of zinc ions is not obvious, and the weakening effect of organic anions on the strength of hydrogen bonds in water is not prominent, so it is not conducive to slowing down the dehydrogenation reaction and inhibiting dendrite growth at the electrode-electrolyte interface during charging.
[0075] The present invention performs an ionic conductivity test on the zinc ion battery electrolytes obtained in Example 1 and Comparative Example 1. Figure 1 The results show that enriching the types of zinc salts in the electrolyte can increase the ion solvation structure entropy and significantly improve its ion conductivity. The ion conductivity of Example 1 increased by nearly 1.3 times to 10.15 S m -1 .
[0076] The present invention performs zinc ion half-cell cycle performance test on the zinc ion battery electrolytes obtained in Examples 1-4 and Comparative Examples 1-4:
[0077] Assembly of Zn||Zn symmetric button half-cell. Zinc foil was used as the positive electrode and negative electrode, commercial glass fiber was used as the separator, and the electrolytes prepared in the above-mentioned Example 1, Example 2, Example 3, Example 4, Comparative Example 1, Comparative Example 2, Comparative Example 3, and Comparative Example 4 were added to assemble the Zn||Zn symmetric button half-cell.
[0078] For the Zn||Zn symmetric button half-cells assembled with the electrolytes prepared in Example 1, Comparative Example 1, Comparative Example 2, Comparative Example 3, and Comparative Example 4, the 10 mA / cm 2 The current density and 5 mAh / cm 2 The deposition capacity was tested by electrochemical charge-discharge cycle test, and the electrochemical cycle life results were shown in Figure 2 As shown, the cycle life of the Zn||Zn symmetric button half-cells assembled with the electrolytes prepared in Example 1, Comparative Example 1, Comparative Example 2, Comparative Example 3, and Comparative Example 4 are 920 hours, 105 hours, 242 hours, 255 hours, and 432 hours, respectively. The above results show that the aqueous zinc ion electrolyte has excellent electrochemical properties compared to the low-component zinc ion battery electrolyte, stabilizes the zinc electrode-electrolyte interface, inhibits dendrite growth, hydrogen evolution, and corrosion side reactions, and prolongs the cycle life of the Zn||Zn half-cell.
[0079] For the Zn||Zn symmetric button half-cells assembled with the electrolytes prepared in Examples 1, 2, 3, 4, and Comparative Example 1, the current was 10 mA / cm 2 The current density and 5 mAh / cm 2 The deposition capacity was tested by electrochemical charge-discharge cycle test, and the electrochemical cycle life results were shown in Figure 3 As shown, the cycle life of the Zn||Zn symmetric button half-cells assembled with the electrolytes prepared in Example 1, Example 2, Example 3, Example 4, and Comparative Example 1 are 920 hours, 397 hours, 430 hours, and 105 hours, respectively. The above results show that the aqueous zinc ion battery electrolyte containing the concentration described in Example 1 exhibits excellent electrochemical properties compared to the zinc ion battery electrolytes with the concentrations described in Example 2, Example 3, and Example 4, stabilizes the zinc electrode-electrolyte interface, inhibits dendrite growth, hydrogen evolution, and corrosion side reactions, and prolongs the cycle life of the Zn||Zn half-cell.
[0080] For the Zn||Zn symmetric button half-cells assembled with the zinc ion battery electrolytes prepared in Example 1 and Comparative Example 1, the 2 The current density and 0.5 mAh / cm 2 The deposition capacity was tested by electrochemical charge-discharge cycle test, and the electrochemical cycle life results were as follows: Figure 4 As shown in the figure, the cycle life of the Zn||Zn symmetric button half-cell assembled with the zinc ion battery electrolyte prepared in Example 1 and Comparative Example 1 is 3000 hours and 125 hours respectively. The results show that at 1 mA / cm 2Under low current density conditions, the cycle life of the Zn||Zn symmetric button half-cell containing the zinc ion battery electrolyte of Example 1 is significantly higher than that of the electrolyte containing a single component of zinc sulfate. The Zn||Zn symmetric button half-cell containing Comparative Example 1 short-circuited after 125 hours of cycling.
[0081] Scanning electron microscope images of zinc electrodes after cycling in different electrolytes Figure 5a and Figure 5b As shown, Figure 5a The zinc electrode after circulating in the zinc ion battery electrolyte of Example 1 for 100 hours, Figure 5b The zinc electrode after 100 hours of circulation in the single zinc sulfate electrolyte of Comparative Example 1. The results show that after the zinc electrode circulates in the zinc ion battery electrolyte, the surface is flat and uniform, and no obvious dendrites and corrosion products are produced. In the electrolyte containing a single zinc sulfate, the zinc electrode presents an extremely uneven surface, indicating that it has experienced severe dendrite growth during the electrochemical charge and discharge cycle, showing petal-shaped byproducts.
[0082] The present invention also carried out a zinc ion full battery performance test, which is as follows:
[0083] Assembly of aqueous zinc-ion full battery:
[0084] MnO 2 The powder, conductive carbon and binder are mixed evenly in a mass ratio of 7:2:1, and N-methylpyrrolidone is added to prepare a slurry, which is then coated on a carbon cloth and dried to obtain a positive electrode. The positive electrode shell, positive electrode sheet, diaphragm, electrolyte, negative electrode sheet, gasket, spring, and negative electrode shell are assembled in this order, commercial zinc foil is used as the negative electrode, commercial glass fiber is used as the diaphragm, and the electrolyte prepared in the above-mentioned Example 1, Example 2, Example 3, Example 4, and Comparative Example 1 is added respectively, and the battery is compacted by a battery press to obtain an aqueous zinc ion full battery.
[0085] For the Zn||MnO prepared by the electrolyte in Example 1 and Comparative Example 1, 2 The full battery was subjected to electrochemical charge and discharge cycle tests at a current density of 5A / g. The electrochemical cycle life results are shown in Figure 6 As shown, the capacity retention rate and average coulombic efficiency of the full battery containing the electrolyte of Example 1 after 1000 cycles reached 84.6% and 99.96%, respectively. However, the capacity retention rate of the full battery assembled with the electrolyte of Comparative Example 1 dropped sharply after 100 cycles, and the capacity retention rate after 850 cycles was 14.7%, further indicating that the zinc ion battery electrolyte containing Example 1 has a more stable cycle performance than Comparative Example 1.
[0086] In addition, the inventor of this case also used other raw materials and other process conditions listed above to replace the various raw materials and corresponding process conditions in Examples 1-4 to conduct corresponding experiments, and the content that needed to be verified was close to the target product of Examples 1-4.
[0087] It should be understood that the above description and the embodiments shown in the drawings cannot be interpreted as limiting the design concept of the present invention. Those with the same knowledge in the technical field of the present invention can improve and change the technical concept of the present invention in various forms, and such improvements and changes should be understood to fall within the scope of protection of the present invention.
Claims
1. A zinc ion battery electrolyte that increases the ion solvation structural entropy, It is characterized in that include: A soluble zinc salt and a solvent, wherein the soluble zinc salt comprises a combination of zinc sulfate, an inorganic anion zinc salt and an organic anion zinc salt, wherein the inorganic anion zinc salt comprises any one of zinc chloride, zinc bromide, zinc nitrate, zinc phosphate, zinc perchlorate and zinc fluoroborate or a combination of two or more thereof, and the organic anion zinc salt comprises any one of zinc trifluoromethanesulfonate, zinc bis(trifluoromethylsulfonyl)imide, zinc bis(difluoromethylsulfonyl)(trifluoromethylxanthoxy)imide, zinc undecylenate, zinc N-(benzenesulfonyl)benzenesulfonamide, zinc tetrakis(hexafluoroisopropoxy)borate, zinc gluconate, zinc carbonate and zinc acetate or a combination of two or more thereof, and the soluble zinc salt comprises five or more kinds.
2. The zinc ion battery electrolyte for increasing the ion solvation structural entropy according to claim 1, It is characterized in that include: Zinc sulfate, and four or more of inorganic anion zinc salts and organic anion zinc salts.
3. The zinc ion battery electrolyte for increasing ion solvation structural entropy according to claim 1, Features: The concentration of the soluble zinc salt in the zinc ion battery electrolyte is 1-3 mol / L.
4. The zinc ion battery electrolyte for increasing ion solvation structural entropy according to claim 2, Features: The concentration of zinc sulfate in the zinc ion battery electrolyte is 0.2-2.0 mol / L, and the sum of the concentrations of the other four or more soluble zinc salts is 0.8-2.8 mol / L.
5. The zinc ion battery electrolyte for increasing ion solvation structural entropy according to claim 4, Features: The concentration of zinc sulfate in the zinc ion battery electrolyte is 0.4 to 1.6 mol / L, preferably 0.8 to 1.6 mol / L, and the concentration of the other four or more soluble zinc salts is 0.4 to 1.6 mol / L.
6. The zinc ion battery electrolyte for increasing ion solvation structural entropy according to claim 4, Features: The molar ratios of the other four or more soluble zinc salts in the zinc ion battery electrolyte are equal; preferably, the other four or more soluble zinc salts in the zinc ion battery electrolyte include a combination of zinc chloride, zinc bromide, zinc trifluoromethanesulfonate and zinc perchlorate; Preferably, the concentrations of the other four or more soluble zinc salts in the zinc ion battery electrolyte are independently 0.1 to 0.5 mol / L, and particularly preferably 0.1 to 0.3 mol / L; And / or, the solvent comprises water, preferably ultrapure water.
7. A method for preparing a zinc ion battery electrolyte for increasing ion solvation structural entropy as claimed in any one of claims 1 to 6, It is characterized in that include: A soluble zinc salt serving as an electrolyte is dissolved in a solvent, and the mixture is stirred and mixed uniformly to prepare a zinc ion battery electrolyte with increased ion solvation structural entropy.
8. Use of the zinc ion battery electrolyte for increasing ion solvation structural entropy according to any one of claims 1 to 6 in an aqueous zinc ion battery or a zinc ion electrochemical energy storage device.
9. An aqueous zinc ion battery, It is characterized in that include: A positive electrode, a negative electrode, a separator and an electrolyte, wherein the electrolyte is the zinc ion battery electrolyte with increased ion solvation structural entropy as described in any one of claims 1 to 6.
10. The aqueous zinc ion battery according to claim 9, Features: The negative electrode comprises at least any one of zinc foil, zinc sheet, zinc wire, zinc powder, zinc foam, zinc plate and zinc alloy; And / or, the active material contained in the positive electrode includes at least any one of vanadium oxide compounds, manganese oxide compounds, and Prussian blue compounds, preferably manganese oxide compounds, and particularly preferably MnO 2 ; And / or, the diaphragm comprises a glass fiber diaphragm.
Citation Information
Cited By
Electrolysis process based on high-entropy electrolyte and application of electrolysis process
CN120844150A