Transfer sheet, method for manufacturing exterior member, and exterior member
By using a transfer sheet with a release film, a first protective layer, and a second protective layer on a metal component, combined with the transfer method, the problem of both gloss utilization and weather resistance in exterior components is solved, and high weather resistance is achieved and improvement of design effects.
Patent Information
- Application Number
- CN202380021879.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-22
- Filing Date
- 2023-03-15
- Publication Date
- 2024-10-01
AI Technical Summary
The existing technology is difficult to effectively utilize the glossiness of metal components in exterior components while meeting high weather resistance requirements, and is particularly deficient in inhibiting deterioration under ultraviolet exposure.
Using a transfer sheet with a release film, a first protective layer, a second protective layer and a pattern layer, the pattern layer and protective layer are provided on the metal component by a transfer method, preferably with low ultraviolet transmittance and visible light transmittance in the covering area Taking into account both weather resistance and gloss.
The design of exterior components with good weather resistance and effective use of the gloss of metal components has been achieved, improving the weather resistance and design performance of exterior components.
Smart Images

Figure CN118742437A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a transfer sheet, a method for producing an exterior member, and the exterior member. Background Art
[0002] For example, as an interior component or exterior component of a building, a decorative component having a substrate and a decorative sheet is used. In the case where the substrate is a metal component, a unique design can be obtained by effectively utilizing the glossiness of the metal. In addition, the range of variations in the design that can be expressed is expanded. However, the decorative sheet usually has a substrate layer, which is sometimes colored. For example, Patent Document 1 describes a decorative sheet, which is sequentially laminated with a printing layer, an adhesive layer, an anchoring layer, and a covering film layer on one surface of a colored substrate layer containing a thermoplastic resin. In addition, regarding the decorative sheet, since the thickness of the decorative sheet itself is relatively thick, it sometimes affects the design. Therefore, when using a decorative sheet, there is room for improvement in the design expression of effectively utilizing the glossiness of the metal component. In addition, for the exterior component, in order to suppress the degradation caused by exposure to the outdoors, especially the degradation caused by the influence of ultraviolet rays, a higher weather resistance than the interior component is required.
[0003] Prior Art Literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2016-168785 Summary of the invention
[0006] Problems to be solved by the invention
[0007] In order to effectively utilize the glossiness of a metal component as a base, the inventors of the present application have studied a scheme of providing a pattern layer on a metal component by a transfer method using a transfer sheet having a release film and a transfer layer including at least a pattern layer. When a transfer sheet is used, since a base material layer in a decorative sheet is not required, the glossiness of the metal component is not easily impaired.
[0008] In addition, in order to obtain excellent weather resistance, the inventors of the present application have studied a scheme of configuring a protective layer (weather-resistant layer) on the transfer layer in the transfer sheet in addition to the pattern layer. That is, they have studied a scheme of using a transfer sheet having a release film, a protective layer and a pattern layer in sequence, and providing a pattern layer and a protective layer on a metal component by a transfer method.
[0009] Since high weather resistance is required for the exterior components, it is preferred that the ultraviolet transmittance of the transfer layer is as low as possible. In order to reduce the ultraviolet transmittance of the transfer layer, it is effective to increase the amount of weathering agent used in the protective layer. If the amount of weathering agent used is increased, yellowing caused by the weathering agent is likely to occur. Therefore, the visible light transmittance of the transfer layer decreases, and it is difficult to obtain a design that effectively utilizes the gloss of the metal component. On the other hand, if the visible light transmittance of the transfer layer is increased in order to effectively utilize the gloss of the metal component, it is difficult to fully reduce the ultraviolet transmittance of the transfer layer. As a result, it is difficult to obtain good weather resistance.
[0010] The present invention has been made in view of the above-mentioned actual situation, and a main object of the present invention is to provide a transfer sheet capable of manufacturing an exterior member having excellent weather resistance and a design that effectively utilizes the glossiness of a metal member.
[0011] Means for solving problems
[0012] In the present invention, a transfer sheet is provided, which is a transfer sheet for manufacturing an exterior component having a metal component, the transfer sheet having a release film and a transfer layer arranged on one surface of the release film, the transfer layer having a first protective layer, a second protective layer and a pattern layer in sequence in the thickness direction from the release film side, the first protective layer and the second protective layer having a weathering agent, the transfer layer having a low hiding area with a hiding rate of less than 50% measured in accordance with JIS K 5600-4-1, in which the ultraviolet transmittance is less than 1% and the visible light transmittance is greater than 40%.
[0013] In the present invention, a method for manufacturing an exterior component is provided, which is a method for manufacturing an exterior component having a metal component, and the manufacturing method comprises: a preparation step of preparing the above-mentioned transfer sheet; and a stacking step of stacking the above-mentioned transfer sheet on the above-mentioned metal component with the aid of an adhesive layer in a manner such that the surface of the above-mentioned pattern layer side of the above-mentioned transfer sheet faces the above-mentioned metal component.
[0014] In the present invention, an exterior component is provided, which is an exterior component having a metal component, and the exterior component has a first protective layer, a second protective layer, a pattern layer, an adhesive layer and the above-mentioned metal component in sequence in the thickness direction, the above-mentioned first protective layer and the above-mentioned second protective layer have a weathering agent, the FI value of the surface of the above-mentioned metal component is greater than 20 and less than 25, and the above-mentioned exterior component has an area where the FI value measured from the side of the above-mentioned first protective layer is greater than 10.
[0015] Effects of the Invention
[0016] In the present invention, there is achieved an effect of being able to obtain an exterior member having good weather resistance and having a design that effectively utilizes the glossiness of a metal member. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is a schematic cross-sectional view illustrating a transfer sheet in the present invention.
[0018] Figure 2 This is a schematic cross-sectional view illustrating a method for producing an exterior member in the present invention.
[0019] Figure 3 It is a schematic cross-sectional view illustrating an exterior member in the present invention.
[0020] Figure 4 It is a schematic diagram explaining the method of measuring the FI value. DETAILED DESCRIPTION
[0021] Hereinafter, the embodiments will be described with reference to the accompanying drawings, etc. However, the present invention can be implemented in many different ways and should not be limited to the contents of the embodiments described below. In addition, in order to make the description clearer, the drawings sometimes schematically show the width, thickness, and shape of each part compared to the actual method, but this is only an example and should not be interpreted as limiting.
[0022] In this specification, when expressing the manner of arranging other members on a certain member, if it is simply expressed as "above" or "below", unless otherwise specified, it includes both the case where the other member is arranged directly above or directly below in a manner of contacting with the certain member, and the case where the other member is arranged above or below the certain member with another member further interposed therebetween. In addition, in this specification, when expressing the manner of arranging other members on the surface of a certain member, if it is simply expressed as "on the surface", unless otherwise specified, it includes both the case where the other member is arranged directly above or directly below in a manner of contacting with the certain member, and the case where the other member is arranged above or below the certain member with another member further interposed therebetween.
[0023] Hereinafter, the transfer sheet, the method for producing the exterior member, and the exterior member in the present invention will be described in detail.
[0024] A. Transfer film
[0025] Figure 1 This is a schematic cross-sectional view illustrating a transfer sheet in the present invention. Figure 1 The transfer sheet 10 shown in the figure comprises a release film 1 and a transfer layer 2 disposed on one surface of the release film 1. The transfer layer 2 extends in a thickness direction D from the release film 1 side. T The transfer layer 2 has a first protective layer 3, a second protective layer 4 and a pattern layer 5 in this order. In the present invention, the transfer layer 2 has a low hiding area with a hiding rate of 50% or less as measured according to JIS K5600-4-1, and in the low hiding area, the ultraviolet transmittance is 1% or less, and the visible light transmittance is 40% or more.
[0026] Figure 2 This is an example of using Figure 1 A schematic cross-sectional view of a method for manufacturing an exterior member having a metal member and a transfer sheet 10 shown in FIG. Figure 2 As shown in (a), the transfer sheet 10 is prepared. Figure 2 As shown in (b), the transfer sheet 10 is laminated on the metal member 20 via the adhesive layer 30 in such a manner that the surface of the transfer sheet 10 on the pattern layer 5 side faces the metal member 20. The "surface of the transfer sheet 10 on the pattern layer 5 side" refers to the surface of the transfer sheet 10 located on the pattern layer 5 side when the release film 1 is used as a reference. Next, as Figure 2 As shown in (c), the release film 1 is peeled off from the transfer sheet 10. As a result, the transfer layer 2 in the transfer sheet 10 is transferred to the metal member 20 side, and a thickness direction D is obtained. T The exterior member 100 has the first protective layer 3, the second protective layer 4, the pattern layer 5, the adhesive layer 30 and the metal member 20 in this order.
[0027] According to the present invention, in the low-covering area of the transfer layer, the ultraviolet transmittance is less than 1% and the visible light transmittance is more than 40%, so that it becomes an exterior component with good weather resistance and a design that effectively utilizes the gloss of the metal component. As mentioned above, since high weather resistance is required for the exterior component, it is preferred that the ultraviolet transmittance of the transfer layer is as low as possible. In order to reduce the ultraviolet transmittance of the transfer layer, it is effective to increase the amount of weathering agent used in the protective layer. If the amount of weathering agent used is increased, yellowing caused by the weathering agent is likely to occur. Therefore, the visible light transmittance of the transfer layer decreases, and it will be difficult to obtain a design that effectively utilizes the gloss of the metal component. On the other hand, if the visible light transmittance of the transfer layer is increased in order to effectively utilize the gloss of the metal component, it is difficult to fully reduce the ultraviolet transmittance of the transfer layer. As a result, it is difficult to obtain good weather resistance.
[0028] In the present invention, the present invention has conducted intensive studies with a view to achieving a balance between improved weather resistance and effective use of the gloss of metal components, and has found that the above balance can be achieved by setting the ultraviolet transmittance and visible light transmittance in the low shielding area to a predetermined range.
[0029] In addition, the transfer sheet in the present invention is generally used to manufacture exterior components having metal components. For exterior components (components for outdoor use), higher weather resistance is required than that for interior components (components for indoor use). For example, when a decorative sheet is used to manufacture an exterior component, a transparent resin layer is sometimes provided on the decorative sheet in order to increase the strength. In this case, the transparent resin layer is a relatively thick layer, and therefore, high weather resistance is imparted, for example, by adding a sufficient amount of weathering agent to the transparent resin layer. In contrast, it is technically difficult to impart high weather resistance to a transfer sheet that does not have a layer equivalent to a transparent resin layer. In the present invention, generally both the first protective layer and the second protective layer contain a weathering agent. As a result, the properties required for the first protective layer (such as surface properties such as wear resistance) and the properties required for the second protective layer (such as adhesion) can be maintained, and high weather resistance can be imparted.
[0030] In addition, in the case of a transfer sheet, the adhesion of the first protective layer and the second protective layer is easily insufficient. Here, in the case of a decorative sheet, a pattern layer is usually formed on the substrate layer, and then a second protective layer is formed on the pattern layer, and then a first protective layer is formed on the second protective layer. The first protective layer is typically made by curing the first protective layer formed on the second protective layer with a resin composition, so the adhesion of the first protective layer and the second protective layer becomes good. In contrast, in the case of a transfer sheet, a first protective layer is usually formed on a release film, and then a second protective layer is formed on the first protective layer, and then a pattern layer is formed on the second protective layer. The first protective layer is typically made by curing the first protective layer formed on the release film with a resin composition. Since the second protective layer is formed on the cured first protective layer, the adhesion of the first protective layer and the second protective layer is easily insufficient. In the present invention, the second protective layer is preferably a layer with higher softness than the first protective layer. Thus, the adhesion of the first protective layer and the second protective layer can be improved.
[0031] 1. Transfer layer
[0032] The transfer layer in the present invention includes at least a first protective layer, a second protective layer, and a pattern layer in this order from the release film side.
[0033] (1) Coverage
[0034] The transfer layer in the present invention has a low hiding region with a hiding rate of 50% or less as measured in accordance with JIS K 5600-4-1. For example, the transfer layer in the present invention has both a low hiding region with a hiding rate of 50% or less and a region with a hiding rate of more than 50% when viewed from above. The region with a hiding rate of more than 50% is a region where the pattern layer is dense and the base does not need to be effectively utilized.
[0035] The hiding power of the transfer layer in the present invention is measured as follows.
[0036] 1) Cut the portion of the transfer sheet where you want to measure the coverage into a specified size.
[0037] 2) A tape is attached to the upper end of the transfer surface (the surface on the pattern layer side) of the cut transfer sheet to peel the transfer layer from the release film. Then, the tape is removed to obtain a single transfer layer.
[0038] 3) The above transfer layer was stacked on a hiding test paper according to JIS K 5600-4-1, and the tristimulus values YW and YB were measured using a spectrocolorimeter (Spectrocolorimeter CM-3700A manufactured by Konica Minolta), and the hiding ratio YB / YW was calculated as a percentage.
[0039] The proportion of the low covering area to the top view area of the transfer layer varies according to the coloring degree of the pattern layer and the pattern of the pattern layer, and can be, for example, 5% or more, 10% or more, 15% or more, or 30% or more. On the other hand, the proportion of the low covering area to the top view area of the transfer layer can be, for example, 95% or less, 90% or less, or 80% or less. In addition, the coverage rate in the low covering area can be 40% or less, or 35% or less.
[0040] (2) Visible light transmittance
[0041] In the low-coverage area, the visible light transmittance is usually 40% or more, and can be 45% or more, or 50% or more. If the visible light transmittance of the transfer layer is within the above range, a design expression that effectively utilizes the glossiness of the metal component can be achieved. The above visible light transmittance refers to the average transmittance in the visible light region (for example, above 380 mm and below 780 nm).
[0042] In addition, when the shielding rate in the low shielding region is 40% or less, the visible light transmittance of the low shielding region may be, for example, 45% or more, or 50% or more.
[0043] (3) UV transmittance
[0044] In the low-covering area, the ultraviolet transmittance is usually less than 1%, can be less than 0.5%, can be less than 0.2%, and can be less than 0.1%. If the ultraviolet transmittance of the transfer layer is within the above range, the weather resistance is excellent. The above ultraviolet transmittance refers to the average transmittance in the ultraviolet region (for example, more than 280nm and less than 350nm).
[0045] When the shielding rate in the low shielding region is 40% or less, the ultraviolet transmittance in the low shielding region may be, for example, 1% or less, 0.5% or less, 0.2% or less, or 0.1% or less.
[0046] The ultraviolet transmittance in the area where the coverage of the transfer layer in the present invention is greater than 50% can be 1% or less, or 0.5% or less, or 0.2% or less, or 0.1% or less. That is, with respect to the transfer layer, in the entire area when viewed from above, the ultraviolet transmittance can be 1% or less, or 0.5% or less, or 0.2% or less, or 0.1% or less. In addition, the visible light transmittance in the area where the coverage of the transfer layer in the present invention is greater than 50% varies depending on the degree of coloring of the pattern layer, for example, less than 40%, or less than 20%.
[0047] It should be noted that in the present invention, the visible light transmittance and ultraviolet transmittance do not need to be within the above ranges over the entire area of the above-mentioned low covering area, as long as the visible light transmittance and ultraviolet transmittance measured at least at the same location as the location where the covering rate is measured to be less than 50% are less than the above values. On the other hand, the ratio of the area where the visible light transmittance and ultraviolet transmittance are within the above ranges to the total area of the above-mentioned low covering area can be 10% or more, 20% or more, or 30% or more. On the other hand, the ratio of the area where the visible light transmittance and ultraviolet transmittance are within the above ranges to the total area of the above-mentioned low covering area can be 100% or less, 90% or less, or 80% or less.
[0048] (3) Thickness
[0049] The thickness of the transfer layer is, for example, 10 μm or more, 12 μm or more, or 14 μm or more. If the transfer layer is thin, sufficient weather resistance may not be obtained. On the other hand, the thickness of the transfer layer is preferably 30 μm or less, 25 μm or less, or 20 μm or less. If the transfer layer is thick, it may be difficult to effectively utilize the gloss of the metal component. Specifically, the thickness of the transfer layer is the total thickness of the first protective layer, the second protective layer and the pattern layer.
[0050] (4) Layer composition
[0051] The transfer layer in the present invention may include only the first protective layer, the second protective layer, and the pattern layer, or may include other layers.
[0052] (i) 1st protective layer
[0053] The transfer sheet in the present invention has a first protective layer. The first protective layer contributes to improved weather resistance by including a weathering agent. In addition, the first protective layer also contributes to improved surface properties (such as scratch resistance and stain resistance) of the outer packaging member. In addition, if the hardness of the first protective layer is increased in order to improve the surface properties of the outer packaging member, the adhesion of the first protective layer and the pattern layer is easily reduced. The first protective layer and the release film can be configured in a direct contact manner or through other layers.
[0054] The first protective layer preferably contains a cured product (cross-linked structure) of a curable resin composition as a resin component. The proportion of the cured product of the curable resin composition relative to the total resin components constituting the first protective layer is, for example, 70% by mass or more, 90% by mass or more, 95% by mass or more, or 100% by mass.
[0055] As the cured product of the curable resin composition, for example, a cured product of an ionizing radiation curable resin composition can be mentioned. As the ionizing radiation curable resin composition, for example, an electron beam curable resin composition and an ultraviolet curable resin composition can be mentioned. Among them, the electron beam curable resin composition is preferred because it does not require a polymerization initiator, has little odor, and is not easy to be colored.
[0056] The ionizing radiation curable resin composition is a composition containing a compound having an ionizing radiation curable functional group (hereinafter, also referred to as an "ionizing radiation curable compound"). As the ionizing radiation curable functional group, it is a group that is crosslinked and cured by irradiation with ionizing radiation, for example, functional groups having olefinic double bonds such as (meth) acryloyl, vinyl, and allyl can be cited. It should be noted that in the present invention, (meth) acryloyl refers to acryloyl or methacryloyl. In addition, in the present invention, (meth) acrylate refers to acrylate or methacrylate.
[0057] Ionizing radiation refers to radiation with energy quanta that can polymerize or crosslink molecules in electromagnetic waves or charged particle beams. Examples of ionizing radiation include electron beams (EB) and ultraviolet rays (UV). Other examples of ionizing radiation include electromagnetic waves such as X-rays and gamma rays, and charged particle beams such as alpha rays and ion rays.
[0058] The ionizing radiation curable compound preferably includes, for example, one or more selected from urethane (meth) acrylate, epoxy (meth) acrylate, polyester (meth) acrylate, polyether (meth) acrylate, polycarbonate (meth) acrylate, and acrylic (meth) acrylate. Among them, the ionizing radiation curable compound preferably includes at least urethane (meth) acrylate. The urethane (meth) acrylate is preferably a caprolactone-based urethane acrylate. This is because it is easy to improve the weather resistance and scratch resistance of the first protective layer.
[0059] In addition, the ionizing radiation curable compound may include caprolactone-based urethane acrylate and urethane (meth) acrylate not modified with caprolactone. In this case, the content of the caprolactone-based urethane acrylate contained in the first protective layer is M CLUA , the content of urethane (meth) acrylate not modified by caprolactone is set as M UA . M CLUA Relative to M UA and M CLUA The total mass ratio (M CLUA / (M UA +M CLUA )) is, for example, 40 mass % to 90 mass % inclusive, may be 45 mass % to 80 mass % inclusive, or may be 50 mass % to 70 mass % inclusive.
[0060] Caprolactone urethane acrylate can be generally obtained by reacting caprolactone polyol, organic isocyanate and hydroxy (meth) acrylate. As a synthesis method, for example, a method of reacting a polycaprolactone polyol with an organic polyisocyanate to generate a polyurethane prepolymer containing -NCO groups (isocyanate groups) at both ends, and then reacting with hydroxy (meth) acrylate can be cited.
[0061] As the caprolactone polyol, commercially available caprolactone polyols can be used, and preferably, caprolactone polyols having two hydroxyl groups and a number average molecular weight of preferably 500 to 3000, more preferably 750 to 2000 can be mentioned. In addition, one or more of polyols other than the caprolactone series, such as ethylene glycol, diethylene glycol, 1,4-butanediol, 1,6-hexanediol, etc., can also be mixed and used in any proportion. As the organic polyisocyanate, diisocyanates having two isocyanate groups are preferred. From the viewpoint of suppressing yellowing, isophorone diisocyanate, hexamethylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, trimethylhexamethylene diisocyanate, etc. can be preferably mentioned. As (meth) hydroxy acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, caprolactone-modified 2-hydroxyethyl acrylate, etc. can be preferably mentioned.
[0062] When the ionizing radiation curable resin composition contains a caprolactone polyol, the caprolactone urethane acrylate is preferably a caprolactone diol urethane acrylate. Caprolactone diol urethane acrylate refers to a urethane acrylate having a diethylene glycol terminal in the caprolactone urethane acrylate. By using the caprolactone diol urethane acrylate, cracks and whitening in the first protective layer can be suppressed.
[0063] The number average molecular weight of the ionizing radiation curable compound is, for example, 300 to 10000, 1000 to 10000, or 2000 to 10000. The number average molecular weight is measured by GPC analysis and is calculated in terms of standard polystyrene.
[0064] For example, when the ionizing radiation curable compound is an ultraviolet curable compound, the ionizing radiation curable compound preferably contains at least one of a photopolymerization initiator and a photopolymerization accelerator.
[0065] Examples of the photopolymerization initiator include acetophenone, benzophenone, α-hydroxyalkylphenone, Michler's ketone, benzoin, benzyl dimethyl ketal, benzoyl benzoate, α-acyl oxime ester, acylphosphine oxide, and thioxanthones. Examples of the photopolymerization accelerator include isopentyl p-dimethylaminobenzoate and ethyl p-dimethylaminobenzoate.
[0066] The first protective layer contains a weathering agent. Examples of the weathering agent include ultraviolet absorbers and light stabilizers. The first protective layer preferably contains at least one of the ultraviolet absorbers and light stabilizers. The first protective layer may contain one or more ultraviolet absorbers. Similarly, the first protective layer may contain one or more light stabilizers.
[0067] Examples of the ultraviolet absorber contained in the first protective layer include organic ultraviolet absorbers such as triazine ultraviolet absorbers, benzotriazole ultraviolet absorbers, benzophenone ultraviolet absorbers, oxybenzophenone ultraviolet absorbers, salicylate ultraviolet absorbers, and cyano(meth)acrylate ultraviolet absorbers, and inorganic ultraviolet absorbers such as titanium dioxide, cerium oxide, and zinc oxide. Among them, triazine ultraviolet absorbers are more preferred.
[0068] Examples of the triazine ultraviolet absorber include hydroxyphenyl triazine ultraviolet absorbers. Examples of the hydroxyphenyl triazine ultraviolet absorber include 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2,4-bis[2-hydroxy-4-butoxyphenyl]-6-(2,4-dibutoxyphenyl)-1,3,5-triazine, triazine, 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-(2'-ethyl)hexyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[2-(2-ethylhexanoyloxy)ethoxy]phenol.
[0069] The content of the ultraviolet absorber contained in the first protective layer is, for example, 0.5 to 10 parts by mass, 0.8 to 8 parts by mass, or 1 to 5 parts by mass, relative to 100 parts by mass of the ionizing radiation curable compound. If the content of the ultraviolet absorber is high, the ultraviolet absorber may bleed out, and if the content of the ultraviolet absorber is low, sufficient ultraviolet absorption performance may not be obtained.
[0070] Examples of the light stabilizer contained in the first protective layer include hindered amine light stabilizers. Examples of the hindered amine light stabilizer include 1,2,2,6,6-pentamethyl-4-piperidinyl methacrylate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate, bis(2,2,6,6-pentamethyl-4-piperidinyl) sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate, methyl(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate, and 2,4-bis[N-butyl-N-(1-cyclohexyloxy-2,2,6,6-tetramethylpiperidin-4-yl)amino]-6-(2-hydroxyethylamine)-1,3,5-triazine).
[0071] The content of the light stabilizer contained in the first protective layer is, for example, 1 part by mass or more and 10 parts by mass or less, 1.5 parts by mass or more and 8 parts by mass or less, or 2 parts by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the ionizing radiation curable compound. If the content of the light stabilizer is high, bleeding of the light stabilizer may occur, and if the content of the light stabilizer is low, sufficient light stability may not be obtained.
[0072] The first protective layer may contain additives such as an organosilicon compound, a polymerization inhibitor, a crosslinking agent, an antistatic agent, an adhesion enhancer, an antioxidant, a leveling agent, a thixotropy imparting agent, a coupling agent, a plasticizer, an antifouling agent, and a defoaming agent. The first protective layer may contain a filler (filler) or may not contain a filler (filler). As fillers, for example, organic fillers and inorganic fillers may be cited. As inorganic fillers, silicon dioxide may be cited. In addition, by making the first protective layer free of fillers, the reduction in transparency is suppressed. As a result, the reduction in designability is suppressed.
[0073] In addition, the thickness of the first protective layer is, for example, 2 μm or more, 3 μm or more, or 4 μm or more. If the first protective layer is thin, sufficient weather resistance may not be obtained. On the other hand, the thickness of the first protective layer is, for example, 20 μm or less, 15 μm or less, or 10 μm or less. If the first protective layer is thick, the hardness of the first protective layer increases, the followability of the first protective layer to the second protective layer decreases, the first protective layer is prone to cracks, and good weather-resistant adhesion may not be obtained.
[0074] (ii) Second protective layer
[0075] The transfer sheet of the present invention has a second protective layer. The second protective layer contains a weathering agent, thereby contributing to improved weather resistance and improved adhesion with the pattern layer. The second protective layer and the first protective layer may be arranged in direct contact or via other layers.
[0076] The second protective layer contains a resin. Examples of the resin include (meth) acrylic resins, urethane resins, butyral resins, polyolefins, chlorinated polyolefins, vinyl chloride-vinyl acetate copolymers, and polyesters. Among them, urethane resins are preferred. The second protective layer preferably contains a cured product (cross-linked structure) of the above resins.
[0077] The second protective layer preferably comprises a cured product of a curable resin composition (particularly a cured product of a thermosetting resin composition). A thermosetting resin composition is a composition comprising at least a thermosetting resin, and is a resin composition that is cured by heating. Examples of thermosetting resins include: (meth) acrylic resins, urethane resins, urethane acrylic resins, phenolic resins, urea melamine resins, epoxy resins, unsaturated polyester resins, and silicone resins. In addition, the thermosetting resin composition may be a composition obtained by adding a curing agent such as an isocyanate curing agent or an epoxy curing agent to these resins.
[0078] The cured product of the thermosetting resin composition is preferably a cured product of a thermosetting resin composition comprising a (meth) acrylic resin, a carbamate resin or a carbamate acrylic resin, and more preferably a cured product of a thermosetting resin composition comprising a carbamate acrylic resin. In addition, in order to make the structure of the cured product more rigid, the thermosetting resin composition preferably comprises an isocyanate curing agent or an epoxy curing agent, and more preferably comprises an isocyanate curing agent. Among them, from the viewpoint of suppressing yellowing, HDI (hexamethylene diisocyanate) curing agent is preferred.
[0079] In addition, when the second protective layer contains a urethane acrylic resin, the urethane acrylic resin is preferably a urethane acrylic copolymer, and more preferably a polycarbonate urethane acrylic copolymer. The polycarbonate urethane acrylic copolymer is a resin obtained by free radical polymerization of an acrylic monomer and a polycarbonate polyurethane polymer obtained by reacting a polycarbonate diol with a (di)isocyanate.
[0080] Examples of the (di)isocyanate include aromatic isocyanates such as 4,4′-diphenylmethane diisocyanate, 2,4-toluene diisocyanate, 1,5-naphthalene diisocyanate, orthoisocyanate phenylsulfonyl isocyanate, orthoisocyanate phenylsulfonyl isocyanate, and paraisocyanate phenylsulfonyl isocyanate; aliphatic isocyanates such as 1,6-hexamethylene diisocyanate; and alicyclic isocyanates such as isophorone diisocyanate, hydrogenated xylylene diisocyanate, and hydrogenated diphenylmethane diisocyanate.
[0081] Examples of the acrylic monomer include alkyl (meth)acrylates such as (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, and isobutyl (meth)acrylate.
[0082] The mass ratio of the carbamate component to the total of the acrylic component and the carbamate component in the polycarbonate-based carbamate acrylic copolymer ([carbamate component] / ([acrylic component]+[carbamate component]) is, for example, 70% by mass or more and 95% by mass or less, 75% by mass or more and 95% by mass or more, or 80% by mass or more and 90% by mass or less. By making the above-mentioned mass ratio 70% by mass or more, the proportion of the polycarbonate structure in the polycarbonate-based carbamate acrylic copolymer can be increased, so that the structure of the polycarbonate-based carbamate acrylic copolymer becomes more rigid. Therefore, deformation with respect to temperature changes can be reduced. In addition, by making the above-mentioned mass ratio 95% by mass or less, it is easy to ensure the flexibility of the second protective layer, and the adhesion with the pattern layer is improved.
[0083] The second protective layer contains a weathering agent. Examples of the weathering agent include ultraviolet absorbers and light stabilizers. The second protective layer preferably contains at least one of the ultraviolet absorbers and light stabilizers. The preferred types and forms of the weathering agent are the same as those described in the above-mentioned "(i) First protective layer", so the description here is omitted. In particular, the second protective layer preferably contains a triazine-based ultraviolet absorber. In addition, the second protective layer preferably contains a hindered amine-based light stabilizer.
[0084] The content of the ultraviolet absorber contained in the second protective layer is, for example, 0.1 mass parts or more and 50 mass parts or less, 3 mass parts or more and 40 mass parts or less, or 10 mass parts or more and 35 mass parts or less relative to 100 mass parts of the resin component. In addition, the content of the ultraviolet absorber contained in the second protective layer (relative to the content of 100 mass parts of the resin component) may be greater than the content of the ultraviolet absorber contained in the first protective layer (relative to the content of 100 mass parts of the resin component).
[0085] The content of the light stabilizer contained in the second protective layer is, for example, 0.1 parts by mass or more and 15 parts by mass or less, 1 part by mass or more and 15 parts by mass or less, or 3 parts by mass or more and 10 parts by mass or less, relative to 100 parts by mass of the resin component. In addition, the content of the light stabilizer contained in the second protective layer (relative to 100 parts by mass of the resin component) may be greater than the content of the light stabilizer contained in the first protective layer (relative to 100 parts by mass of the resin component).
[0086] The second protective layer may contain additives such as organic silicon compounds, polymerization inhibitors, crosslinking agents, antistatic agents, adhesion improvers, antioxidants, leveling agents, thixotropy imparting agents, coupling agents, plasticizers, antifouling agents, defoaming agents, fillers, etc. In addition, the second protective layer may contain fillers or may not contain fillers.
[0087] The thickness of the second protective layer may be, for example, 2 μm or more, or 3 μm or more.
[0088] If the second protective layer is thin, the adhesion to the pattern layer may be insufficient. On the other hand, the thickness of the second protective layer is, for example, 10 μm or less, 8 μm or less, or 5 μm or less. If the second protective layer is thick, the movement of the second protective layer caused by heat becomes large, the first protective layer is prone to cracking, and good weather-resistant adhesion may not be obtained.
[0089] (iii) Pattern layer
[0090] The transfer sheet of the present invention has a pattern layer on the surface of the second protective layer opposite to the first protective layer. By providing the pattern layer, the design of the exterior member is improved. The pattern layer and the second protective layer can be arranged in direct contact or through other layers.
[0091] The pattern layer is a layer printed with ink. Examples of the pattern (pattern) in the pattern layer include: wood grain pattern, stone grain pattern, sand grain pattern, tile pattern, brickwork pattern, cloth pattern, leather grain pattern, geometric figures, letters, symbols, abstract pattern, floral pattern, wavy pattern, striped pattern, metallic pattern, and rust pattern.
[0092] The pattern layer usually contains a colorant and a binder resin. Examples of the colorant include inorganic pigments such as carbon black (ink), iron black, titanium white, antimony white, chrome yellow, titanium yellow, red iron oxide, cadmium red, ultramarine, and cobalt blue, organic pigments (including dyes) such as quinacridone red, isoindolinone yellow, nickel azo complex, phthalocyanine blue, and azomethine azo black (Japanese: アゾメチンアゾブラック), metal pigments such as aluminum and brass, and pearlescent pigments such as titanium dioxide-coated mica and basic lead carbonate.
[0093] Examples of the binder resin include urethane resins, acrylic polyol resins, (meth)acrylic resins, ester resins, amide resins, butyral resins, styrene resins, urethane-acrylic copolymers, vinyl chloride-vinyl acetate copolymers, vinyl chloride-vinyl acetate-acrylic copolymers, chlorinated propylene resins, nitrocellulose resins, and cellulose acetate resins.
[0094] The pattern layer may contain additives such as ultraviolet absorbers, light stabilizers, curing agents, plasticizers, catalysts, etc. as needed. The thickness of the pattern layer is, for example, 0.5 μm to 20 μm, 1 μm to 10 μm, or 2 μm to 5 μm.
[0095] (iv) Others
[0096] The transfer layer in the present invention preferably does not have a solid layer (a layer where ink is applied solidly). The solid layer is, for example, an opaque solid layer. This is because it is easy to obtain a low-masking area by not having a solid layer.
[0097] 2. Release film
[0098] The transfer sheet in the present invention has a release film (first release film) on the surface of the first protective layer opposite to the second protective layer. The release film and the first protective layer may be disposed in direct contact or with another layer interposed therebetween.
[0099] The release film is preferably a resin film. Examples of the resin contained in the resin film include ester resins, olefin resins, styrene resins, vinyl resins, (meth)acrylic resins, amide resins, imide resins, and carbonate resins.
[0100] The release film preferably contains an ester resin or an olefin resin.
[0101] Examples of the ester resin include polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), and polyethylene terephthalate-isophthalate copolymers. Among them, PET or PBT is preferred, and PET is more preferred, from the viewpoint of being less susceptible to thermal shrinkage during the production of the transfer sheet and shrinkage due to irradiation with ionizing radiation.
[0102] Examples of the olefin resin include polyethylene, polypropylene, polybutene, ethylene-propylene copolymers, and ethylene-propylene-butene copolymers. Among them, polypropylene is preferred because it is less likely to shrink due to heat during the production of the transfer sheet and shrinkage due to ionizing radiation.
[0103] In addition, from the viewpoint of obtaining an exterior component with a release film having a design that effectively utilizes the glossiness of a metal component, the 60° gloss (Japanese: グロス) value of the release film is preferably 25% or more. The above-mentioned 60° gloss value may be 30% or more, or 35% or more. The 60° gloss value of the release film is a value measured using a gloss meter (micro-TRI-gloss gloss meter manufactured by BYK) according to the method of JIS Z8741:1997. Specifically, the surface of the release film opposite to the transfer surface (the surface on which the transfer layer is arranged) is faced upward, the gloss meter is placed, and the gloss value at 60° is read. It should be noted that the 60° gloss value is, for example, the average value of the values measured at any 10 locations of the release film.
[0104] The arithmetic mean surface roughness Sa of the surface of the release film opposite to the transfer layer is preferably 0.5 μm or less. This is because an exterior member with a release film having a design that effectively utilizes the glossiness of the metal member can be obtained. The arithmetic mean surface roughness Sa may be 0.4 μm or less.
[0105] The arithmetic mean surface roughness Sa is obtained by expanding Ra, a two-dimensional roughness parameter described in JIS B0601:1994, to three dimensions, and placing the orthogonal coordinate axes X and Y axes on the reference plane, setting the roughness surface to Z (x, y), and setting the size of the reference plane to Lx and Ly, and calculating the arithmetic mean surface roughness Sa by the following formula (i). It should be noted that in formula (i), A = Lx × Ly.
[0106] [Mathematical formula 1]
[0107]
[0108] The measurement of the arithmetic mean surface roughness Sa of the surface of the release film on the opposite side to the transfer layer was specifically performed using the following measuring equipment and measuring conditions.
[0109] ·Measurement equipment
[0110] KEYENCE 3D shape measuring machine VK-X1000
[0111] Analysis software
[0112] Shape Measurement Laser Microscope VK-X100 / X200 Series Analysis Applications
[0113] ·Measurement conditions
[0114] 5x lens
[0115] ·Measurement area
[0116] Horizontal width 500μm × vertical width 500μm
[0117] The release film may be a stretched film or an unstretched film. The stretching ratio in the machine direction (MD) of the stretched film is, for example, 5 times or more and 30 times or less. The stretching ratio in the width direction (TD) of the stretched film is, for example, 5 times or more and 30 times or less. In addition, the thickness of the release film is, for example, 10 μm or more and 200 μm or less, 15 μm or more and 150 μm or less, or 20 μm or more and 100 μm or less.
[0118] 3. Transfer film
[0119] The transfer sheet in the present invention has a release film and a transfer layer (at least a first protective layer, a second protective layer, and a pattern layer) in this order in the thickness direction.
[0120] The transfer sheet in the present invention may have a second release film on the surface of the pattern layer opposite to the second protective layer. For example, when the transfer sheet is wound into a roll and manufactured, the occurrence of adhesion can be suppressed. The second release film is usually peeled off from the transfer sheet before the lamination process described later. The details of the second release film are the same as those described in the first release film, so the description here is omitted.
[0121] 4. Method for manufacturing transfer sheet
[0122] The method for manufacturing the transfer sheet in the present invention is not particularly limited, and for example, the following method can be cited: forming a first protective layer on the surface of a release film, then forming a second protective layer on the surface of the first protective layer opposite to the release film, and then forming a pattern layer on the surface of the second protective layer opposite to the first protective layer.
[0123] As a method for forming the first protective layer, for example, there can be mentioned a method of applying a composition for forming the first protective layer on the surface of the release film and curing it. As a method for applying the above composition, for example, there can be mentioned a gravure printing method, a rod coating method, a roller coating method, a reverse roller coating method, and a comma coating method. As the above curing method, for example, there can be mentioned a method of irradiating ionizing radiation such as electron beams and ultraviolet rays.
[0124] As a method for forming the second protective layer, for example, there can be mentioned a method of applying a composition for forming the second protective layer on the surface of the first protective layer on the opposite side to the release film, and curing it as needed. As a method for applying the above-mentioned composition, for example, there can be mentioned a gravure printing method, a rod coating method, a roller coating method, a reverse roller coating method, and a comma coating method. As the above-mentioned curing method, for example, there can be mentioned heat. In addition, as a method for forming a pattern layer, for example, there can be mentioned a method of applying an ink containing a colorant, a binder resin and a solvent on the surface of the second protective layer on the opposite side to the first protective layer.
[0125] 5. Purpose
[0126] The transfer sheet in the present invention is used to manufacture an exterior component having a metal component. Using the transfer sheet in the present invention, the above-mentioned transfer layer is provided on the metal component by a transfer method, thereby obtaining an exterior component having good weather resistance and a design that effectively utilizes the glossiness of the metal component. Specifically, when the FI value of the metal component is greater than or equal to 20 and less than or equal to 25, when the transfer sheet is laminated on the metal component with the surface on the pattern layer side facing the metal component via an adhesive layer, and the release film is peeled off to form a laminate, an exterior component having an FI value (measured from the transfer layer side) of greater than or equal to 10 in the low covering area of the laminate can be obtained. The FI value of such an exterior component is the same as that described in "C. Exterior component" described later, so the description here is omitted.
[0127] B. Method for manufacturing exterior components
[0128] In the present invention, a method for manufacturing an exterior member is provided, which is a method for manufacturing an exterior member having a metal member, the method comprising: a preparation step of preparing the transfer sheet; and a lamination step of laminating the transfer sheet on the metal member via an adhesive layer in a manner that the surface of the transfer sheet on the pattern layer side becomes the metal member side. According to the present invention, an exterior member having good weather resistance and a design that effectively utilizes the glossiness of the metal member can be obtained.
[0129] Figure 2 This is a schematic cross-sectional view illustrating a method for manufacturing an exterior member in the present invention. Figure 2 , since it has been explained in the above-mentioned “A. Transfer sheet”, the explanation here is omitted.
[0130] 1. Preparation process
[0131] The preparation step in the present invention is a step of preparing a transfer sheet having a release film, a first protective layer, a second protective layer, and a pattern layer in this order in the thickness direction. The transfer sheet is the same as the above-mentioned "A. transfer sheet", so the description here is omitted.
[0132] 2. Lamination process
[0133] The lamination step in the present invention is a lamination step of laminating the transfer sheet on the metal member via the adhesive layer so that the surface of the transfer sheet on the pattern layer side faces the metal member.
[0134] (1) Metal components
[0135] The metal component in the present invention is a component containing a metal as a main component. Examples of the metal contained in the metal component include aluminum, iron, etc., preferably aluminum. That is, the metal component is preferably an aluminum component. The shape of the metal component is not particularly limited, and examples thereof include a plate-like, sheet-like, and three-dimensional shape. In addition, the metal component may have a planar portion, a curved portion, or both a planar portion and a curved portion. In addition, the metal component may have at least one of a convex portion, a concave portion, a convex stripe portion, a concave stripe portion, and a through portion.
[0136] The surface of the metal component presents different hues depending on the angle of illumination and the angle of observation. As an indicator of the hue unique to the metal, there is an angle-dependent chromatic aberration index (FI value). The angle-dependent chromatic aberration is expressed by the size of the hue difference when the surface of the metal component is observed from different angles. In the present invention, the angle-dependent chromatic aberration index value (FI value) of the metal component is preferably greater than 20 and less than 25. The FI value can be calculated by the following formula.
[0137] like Figure 4 As shown in the figure, a metal member is arranged as a sample S, and a light beam C is irradiated from a first direction inclined at 45° relative to a vertical direction perpendicular to the surface of the metal member to obtain specular reflected light of the light. At the deflection angles of 15°, 45°, and 110° from the specular reflected light, the L value specified in JIS Z 8729 is measured. * a * b * Lightness index L of the color system * For color measurement, for example, a multi-angle spectrophotometer MA68II manufactured by X-Rite Corporation can be used. The measurement conditions are light source D65 and a 10° field of view.
[0138] Next, by substituting each lightness index into the following formula, the flop index (FI) can be calculated.
[0139] [Mathematical formula 2]
[0140]
[0141] (Where L * 15°, L * 45°, L * 110° respectively, the deflection angles of 15°, 45°, and 110° from the mirror reflected light are L specified in JISZ 8729 * a * b * L * , the specularly reflected light is the specularly reflected light of the light incident at an angle of 45° relative to the perpendicular direction of the stacked surface. )
[0142] (2) Adhesive layer
[0143] In order to obtain adhesion between the transfer sheet and the metal member, the adhesive layer in the present invention is disposed between the surface of the transfer sheet on the pattern layer side and the metal member. In order to obtain a design that effectively utilizes the gloss of the metal member, the adhesive layer is preferably transparent.
[0144] As the adhesive used in the adhesive layer, there is no particular limitation, and known adhesives can be used. For example, adhesives such as heat-sensitive adhesives and pressure-sensitive adhesives can be preferably cited. As the resin used in the adhesive constituting the adhesive layer, for example, acrylic resins, polyurethane resins, vinyl chloride resins, vinyl acetate resins, vinyl chloride-vinyl acetate copolymer resins, styrene-acrylic copolymer resins, polyester resins, polyamide resins, etc. can be cited, and they can be used alone or in combination. In addition, polyurethane-based adhesives and polyester-based adhesives of two-component curing type using isocyanate compounds etc. as curing agents can also be used.
[0145] In addition, an adhesive may be used in the adhesive layer. As the adhesive, various adhesives such as acrylic, urethane, silicone, and rubber can be appropriately selected and used.
[0146] In the present invention, the thickness of the adhesive layer is not particularly limited. From the viewpoint of obtaining excellent adhesion, it is preferably 1 μm or more, more preferably 5 μm or more, and further preferably 10 μm or more. On the other hand, in order to obtain a design that effectively utilizes the gloss of the metal component, it is preferably 30 μm or less, more preferably 25 μm or less, and further preferably 20 μm or less.
[0147] (3) Lamination method
[0148] In the lamination process, the transfer sheet is laminated on the metal component via the adhesive layer in such a manner that the surface of the transfer sheet on the pattern layer side faces the metal component. Specifically, the adhesive layer is arranged between the surface of the transfer sheet on the pattern layer side and the metal component so that the transfer sheet, the adhesive layer and the metal component are closely attached. The adhesive layer may be integrated with the transfer sheet in advance, or may be integrated with the metal component in advance.
[0149] As a method for making the transfer sheet, adhesive layer and metal component close together, for example, a lamination method can be cited. In the lamination method, for example, the stack of the transfer sheet, adhesive layer and metal component is heated and pressurized from the transfer sheet side. As a method for heating and pressurizing, for example, a method using a roller transfer device can be cited. When a hot melt adhesive (thermosensitive adhesive) is used as an adhesive, although it also depends on the type of resin constituting the adhesive, the heating temperature is preferably above 160°C and below 200°C, and in the case of a reactive hot melt adhesive, the heating temperature is preferably above 100°C and below 130°C. In addition, in the case of vacuum forming, it is usually carried out while heating, preferably above 80°C and below 130°C, and more preferably above 90°C and below 120°C.
[0150] Furthermore, the method for producing an exterior member in the present invention may include a peeling step of peeling the release film from the first protective layer after the lamination step.
[0151] 3. External components
[0152] The exterior component manufactured in the present invention is a component having a first protective layer, a second protective layer, a pattern layer, an adhesive layer, and a metal component in this order. The exterior component may be an exterior component with a release film having a release film on the surface of the first protective layer opposite to the second protective layer, or an exterior component without a release film.
[0153] The exterior component manufactured in the present invention has good weather resistance and has a design that effectively utilizes the glossiness of the metal component. Specifically, when the FI value of the surface of the metal component is greater than 20 and less than 25, when the transfer sheet is laminated to the metal component with the surface of the pattern layer facing the metal component by means of an adhesive layer, and the release film is peeled off to form a laminate, an exterior component having an FI value of 10 or more in the low covering area of the laminate (measured from the transfer layer side) can be obtained. Such FI values are the same as those described in "C. Exterior Components" described later, so the description here is omitted.
[0154] C.Exterior components
[0155] Figure 3 It is a schematic cross-sectional view illustrating an exterior member in the present invention. Figure 3 The exterior member 100 shown has the first protective layer 3, the second protective layer 4, the pattern layer 5, the adhesive layer 30 and the metal member 20 in this order. In addition, the first protective layer 3 and the second protective layer 4 have a weathering agent. In addition, the exterior member 100 has a region where the FI value measured from the first protective layer 3 side is 10 or more.
[0156] The exterior member of the present invention has excellent weather resistance and has a design that effectively utilizes the glossiness of the metal member.
[0157] The first protective layer, the second protective layer, the pattern layer, the adhesive layer and the metal member in the present invention are the same as those described in the above-mentioned "A. Transfer sheet" and "B. Method for producing exterior member", and thus description thereof is omitted here.
[0158] 1. FI value
[0159] The exterior member in the present invention has a region where the FI value measured from the first protective layer side is 10 or more.
[0160] Regarding the method for measuring the FI value of the outer packaging member, the outer packaging member is used as Figure 4 The method is the same as that described in "B. Method for manufacturing exterior member 2. Lamination step (1) Metal member" except that the measurement sample S in the transfer sheet is measured from the first protective layer side. For the exterior member of the present invention, the FI value of the exterior member measured at the same location as the location where the coverage is measured to be 50% or less in the transfer layer of the transfer sheet is preferably 10 or more.
[0161] The exterior member in the present invention preferably has a region where the maintenance rate of the FI value of the surface of the metal member (FI value of the exterior member / FI value of the metal member) is 50% or more, and more preferably has a region where the maintenance rate is 60% or more.
[0162] 2. Purpose
[0163] The exterior member in the present invention is usually used for exterior decoration (outdoors). As the purpose of the exterior member, for example, building materials can be mentioned. As a specific example of building materials, exterior members such as eaves ceilings, outer walls, and roofs of buildings such as residences, factories, shops, and hospitals can be mentioned.
[0164] The present invention is not limited to the above-mentioned embodiments. The above-mentioned embodiments are illustrative, and any embodiments having substantially the same configuration as the technical concept described in the claims of the present invention and having the same functions and effects are also included in the technical scope of the present invention.
[0165] Example
[0166] [Example 1]
[0167] (Production of transfer film)
[0168] As a release film, a PET film (Diafoil E130-26, manufactured by Mitsubishi Chemical) was prepared. The 60° glossiness value of the release film on the side opposite to the side where the transfer layer was arranged was 27%, and the arithmetic mean surface roughness Sa was 0.3 μm. On the surface of the PET film, the coating amount after drying was 5 g / m 2 The resin composition for forming the first protective layer was applied in a manner described below and dried. Then, electron beams were irradiated (voltage: 175 keV, 5 Mrad (50 kGy)) to form a first protective layer having a thickness of 5 μm.
[0169] <Resin composition for forming the first protective layer>
[0170] Urethane acrylate: 100 parts by mass
[0171] (Bifunctional caprolactone-modified urethane acrylate / multifunctional urethane acrylate=50 / 50 (mass ratio))
[0172] Triazine UV absorber: 4 parts by mass
[0173] (3 parts by mass of "Tinuvin 479" (manufactured by BASF), 1 part by mass of "Tinuvin 400" (manufactured by BASF))
[0174] Light stabilizer: 3 parts by mass
[0175] (Product name: LS-3410, manufactured by Nippon Emulsifier Co., Ltd.)
[0176] Solvent: appropriate amount
[0177] (Methyl Ethyl Ketone)
[0178] Next, the resin composition for forming the second protective layer described below was applied onto the surface of the obtained first protective layer and dried to form a second protective layer having a thickness of 4 μm.
[0179] <Resin composition for forming the second protective layer>
[0180] Polycarbonate urethane acrylic copolymer: 100 parts by mass
[0181] (Urethane component / acrylic component=90 / 10 (mass ratio))
[0182] Triazine UV absorber: 35 parts by mass
[0183] (18 parts by mass of "Tinuvin 479" (manufactured by BASF), 17 parts by mass of "Tinuvin 400" (manufactured by BASF))
[0184] Light stabilizer: 3.5 parts by mass
[0185] ("Tinuvin 123" (manufactured by BASF))
[0186] Hexamethylene diisocyanate curing agent: 6 parts by mass
[0187] Solvent: appropriate amount
[0188] (Methyl Ethyl Ketone)
[0189] Next, a pattern layer (wave pattern) having a thickness of 6 μm was formed on the surface of the obtained second protective layer using a gravure printing machine. The pattern layer mainly included a gray colored portion and a brown colored portion.
[0190] Thus, a transfer sheet having a release film, a first protective layer, a second protective layer, and a pattern layer in order in the thickness direction was obtained. The first protective layer, the second protective layer, and the pattern layer constituted a transfer layer. The thickness of the transfer layer (the total thickness of the first protective layer, the second protective layer, and the pattern layer) was 15 μm.
[0191] [Determination of hiding power, visible light transmittance and ultraviolet light transmittance]
[0192] The gray colored portion of the wavy pattern of the transfer layer of the obtained transfer sheet was measured for hiding power, visible light transmittance, ultraviolet light transmittance, and total light transmittance by the following measurement methods.
[0193] ·Measurement method
[0194] 1) The portion of the obtained transfer sheet where the hiding power is to be measured (the gray colored portion of the wavy pattern) is cut into a predetermined size.
[0195] 2) A tape was attached to the upper end of the transfer surface of the cut transfer sheet to peel the transfer layer from the release film. Then, the tape was removed to obtain a single transfer layer.
[0196] 3) The above transfer layer was stacked on a hiding test paper according to JIS K 5600-4-1, and the tristimulus values YW and YB were measured using a spectrophotometer (CM-3700A manufactured by Konica Minolta), and the hiding ratio YB / YW was calculated as a percentage. The hiding ratio was 22%.
[0197] 4) The visible light transmittance, ultraviolet transmittance and total light transmittance are measured on the gray colored portion of the corrugated pattern for which the hiding power is measured. It should be noted that the visible light transmittance is the average transmittance in the visible light region (wavelength 380 mm or more and 780 nm or less), and the ultraviolet transmittance is the average transmittance in the ultraviolet region (wavelength 280 mm or more and 350 nm or less). The total light transmittance is a value measured in accordance with JIS K 7361-1:1997.
[0198] [Example 2]
[0199] A transfer sheet was prepared by the same method as in Example 1 except that a pattern layer of a metallic pattern including a blue colored portion and an orange colored portion was formed using a gravure printing machine. The visible light transmittance, ultraviolet light transmittance, and total light transmittance were measured at a portion where the hiding power measured by the above-mentioned measuring method was 50% or less (the hiding power of the blue colored portion of the metallic pattern was 30%).
[0200] The results are shown in Table 1.
[0201] [Example 3]
[0202] A transfer sheet was prepared by the same method as in Example 1, except that a pattern layer of a wood grain pattern including a black colored portion and a brown colored portion was formed using a gravure printing machine, to obtain an exterior member. The visible light transmittance, ultraviolet light transmittance, and total light transmittance were measured at a portion where the hiding rate measured by the above-mentioned measuring method was 50% or less (the hiding rate of the brown colored portion of the wood grain pattern was 19%). The results are shown in Table 1.
[0203] [Example 4]
[0204] A transfer sheet was prepared by the same method as in Example 1, except that a pattern layer containing a square pattern of a gray colored portion was formed using a gravure printing machine, to obtain an exterior member. The visible light transmittance, ultraviolet light transmittance, and total light transmittance were measured at a portion where the hiding rate measured by the above-mentioned measuring method was 50% or less (the hiding rate of the gray colored portion of the square pattern was 26%). The results are shown in Table 1.
[0205] [Example 5]
[0206] A transfer sheet was prepared by the same method as in Example 1, except that a pattern layer including a colored portion and a transmissive portion was formed using a gravure printing machine, to obtain an exterior member. The visible light transmittance, ultraviolet light transmittance, and total light transmittance were measured at a portion where the coverage measured by the above-mentioned measurement method was 50% or less (the coverage of the transmissive portion of the vertical line pattern was 14%). The results are shown in Table 1.
[0207] [Comparative Example 1]
[0208] A transfer sheet was prepared in the same manner as in Example 1, except that a stone pattern layer was formed using a gravure printer, to obtain an exterior member. The visible light transmittance, ultraviolet light transmittance, and total light transmittance were measured at the black portion of the stone pattern (coverage 55%). The results are shown in Table 1.
[0209] [Comparative Example 2]
[0210] A transfer sheet was prepared in the same manner as in Example 1, except that a rust-like pattern layer was formed using a gravure printing machine, and a solid layer was further formed to form a transfer layer having a thickness of 15 μm, to obtain an exterior member. The visible light transmittance, ultraviolet light transmittance, and total light transmittance were measured at the brown portion of the rust-like pattern (coverage 74%). The results are shown in Table 1.
[0211] (Production of exterior components)
[0212] A hot-melt two-component adhesive (solvent-based) was applied to the surface of the transfer sheet obtained above on the pattern layer side and dried to form an adhesive layer (thickness 10 μm).
[0213] Next, the obtained adhesive layer and the metal member (aluminum member, FI value 22) were arranged in a manner facing each other, and a laminator (RT-300 manufactured by Navitas Machinery) was used to heat and pressurize the transfer sheet side under the conditions of a laminating roller temperature of 180°C and a conveying speed of 2m / min, and aged at 50°C for 3 days, thereby making the transfer sheet, the adhesive layer and the metal member closely attached. Then, the release film was peeled off to obtain an exterior member.
[0214] (evaluate)
[0215] Determination of FI value
[0216] The FI value of the obtained exterior member was measured at the same position as the measurement position of the hiding rate of the transfer layer in the transfer sheet. The lightness index L was measured at the deflection angles of 15°, 45°, and 110° from the specularly reflected light by irradiating light C from the first direction inclined 45° relative to the vertical direction perpendicular to the surface using a multi-angle spectrophotometer MA68II manufactured by X-Rite. * The measurement conditions were set to light source D65 and 10° visual field. Next, each lightness index was substituted into the above formula to calculate the flop index (FI). The results are shown in Table 1.
[0217] Visual brightness
[0218] Twenty random adults visually observed the appearance of the exterior member and evaluated it based on the following criteria. The results are shown in Table 1.
[0219] ◎: More than 18 people answered that they feel good under indoor fluorescent lights
[0220] 0:15 to 17 people answered that they feel good under indoor fluorescent lights
[0221] △: 11 to 14 people answered that they feel good under indoor fluorescent lights
[0222] ×: Less than 10 people answered that they have a good sense of brightness under indoor fluorescent lights
[0223] [Table 1]
[0224]
[0225] As shown in Table 1, it was confirmed that in the low-hiding region, the transfer layer having an ultraviolet transmittance of 1% or less and a visible light transmittance of 40% or more can be designed to effectively utilize the glossiness of the metal member as the base.
[0226] The present invention provides, for example, the following inventions. [1]
[0228] A transfer sheet is used for manufacturing an exterior member having a metal member.
[0229] The transfer sheet comprises a release film and a transfer layer disposed on one surface of the release film.
[0230] The transfer layer includes a first protective layer, a second protective layer, and a pattern layer in order from the release film side in the thickness direction.
[0231] The first protective layer and the second protective layer have a weathering agent,
[0232] The transfer layer has a low hiding region having a hiding rate of 50% or less as measured in accordance with JIS K 5600-4-1,
[0233] In the low-hidden area, the ultraviolet light transmittance is 1% or less, and the visible light transmittance is 40% or more. [2]
[0235] The transfer sheet according to [1], wherein the transfer layer has a thickness of 10 μm to 30 μm. [3]
[0237] The transfer sheet according to [1] or [2], wherein the first protective layer comprises a cured product of an ionizing radiation-curable resin composition. [4]
[0239] The transfer sheet according to any one of [1] to [3], wherein the second protective layer comprises a cured product of a thermosetting resin composition. [5]
[0241] The transfer sheet according to any one of [1] to [4], wherein the first protective layer comprises a cured product of an electron beam curable resin composition comprising urethane (meth)acrylate. [6]
[0243] The transfer sheet according to any one of [1] to [5], wherein the second protective layer comprises a cured product of a thermosetting resin composition comprising a polycarbonate-based urethane acrylic copolymer. [7]
[0245] The transfer sheet according to any one of [1] to [6], wherein the first protective layer contains at least one of an ultraviolet absorber and a light stabilizer as the weathering agent. [8]
[0247] The transfer sheet according to any one of [1] to [7], wherein the first protective layer contains a triazine-based ultraviolet absorber as the weathering agent. [9]
[0249] The transfer sheet according to any one of [1] to [8], wherein the second protective layer contains at least one of an ultraviolet absorber and a light stabilizer as the weathering agent.
[10]
[0251] The transfer sheet according to any one of [1] to [9], wherein the second protective layer contains a triazine-based ultraviolet absorber as the weathering agent.
[11]
[0253] The transfer sheet according to any one of [1] to
[10] , wherein the 60° glossiness value of the surface of the release film opposite to the transfer layer is 25% or more.
[12]
[0255] The transfer sheet according to any one of [1] to
[11] , wherein the arithmetic mean surface roughness Sa of the surface of the release film opposite to the transfer layer is 0.5 μm or less.
[13]
[0257] The transfer sheet according to any one of [1] to
[12] , wherein the FI value of the metal member is 20 or more and 25 or less,
[0258] When the transfer sheet is laminated on the metal component with the aid of an adhesive layer so that the surface on the pattern layer side faces the metal component and the release film is peeled off to form a laminate, the FI value of the low covering area in the laminate (measured from the transfer layer side) is greater than 10.
[14]
[0260] The transfer sheet according to any one of [1] to
[13] , wherein the metal member is an aluminum member.
[15]
[0262] A method for manufacturing an exterior member, which is a method for manufacturing an exterior member having a metal member, the manufacturing method comprising:
[0263] a preparation step of preparing the transfer sheet described in any one of [1] to
[14] ; and
[0264] The laminating step is to laminate the transfer sheet onto the metal member via an adhesive layer so that the surface of the transfer sheet on the pattern layer side faces the metal member.
[16]
[0266] The method for producing an exterior member according to
[15] , further comprising a peeling step of peeling the release film from the transfer sheet after the lamination step.
[17]
[0268] An exterior component, which is an exterior component having a metal component,
[0269] The exterior component has a first protective layer, a second protective layer, a pattern layer, an adhesive layer and the above-mentioned metal component in order in the thickness direction.
[0270] The first protective layer and the second protective layer have a weathering agent,
[0271] The FI value of the metal component is 20 or more and 25 or less,
[0272] The exterior member has a region where the FI value measured from the first protective layer side is 10 or more.
[0273] Description of Reference Numerals
[0274] 1…Release film
[0275] 2…Transfer layer
[0276] 3…1st protection layer
[0277] 4…Second protection layer
[0278] 5…Pattern layer
[0279] 10…Transfer film
[0280] 20…Metal components
[0281] 30…Adhesive layer
[0282] 100…Exterior components
Claims
1. A transfer sheet for use in manufacturing an exterior member having a metal member, The transfer sheet comprises a release film and a transfer layer disposed on one surface of the release film. The transfer layer includes a first protective layer, a second protective layer, and a pattern layer in order from the release film side in the thickness direction. The first protective layer and the second protective layer have a weathering agent, The transfer layer has a low hiding region having a hiding rate of 50% or less as measured in accordance with JIS K 5600-4-1, In the low-hiding area, the ultraviolet light transmittance is 1% or less, and the visible light transmittance is 40% or more.
2. The transfer sheet according to claim 1, wherein The transfer layer has a thickness of 10 μm or more and 30 μm or less.
3. The transfer sheet according to claim 1, wherein The first protective layer includes a cured product of an ionizing radiation-curable resin composition.
4. The transfer sheet according to claim 1, wherein The second protective layer includes a cured product of a thermosetting resin composition.
5. The transfer sheet according to claim 1, wherein The first protective layer includes a cured product of an electron beam curable resin composition, and the electron beam curable resin composition includes urethane (meth)acrylate.
6. The transfer sheet according to claim 1, wherein The second protective layer includes a cured product of a thermosetting resin composition, and the thermosetting resin composition includes a polycarbonate-based urethane acrylic copolymer.
7. The transfer sheet according to claim 1, wherein The first protective layer contains at least one of an ultraviolet absorber and a light stabilizer as the weathering agent.
8. The transfer sheet according to claim 1, wherein The first protective layer contains a triazine-based ultraviolet absorber as the weathering agent.
9. The transfer sheet according to claim 1, wherein The second protective layer contains at least one of an ultraviolet absorber and a light stabilizer as the weathering agent.
10. The transfer sheet according to claim 1, wherein The second protective layer contains a triazine-based ultraviolet absorber as the weathering agent.
11. The transfer sheet according to claim 1, wherein The 60° glossiness value of the surface of the release film on the opposite side to the transfer layer is 25% or more.
12. The transfer sheet according to claim 1, wherein The arithmetic mean surface roughness Sa of the surface of the release film on the opposite side to the transfer layer is 0.5 μm or less.
13. The transfer sheet according to claim 1, wherein The FI value of the metal component is greater than or equal to 20 and less than or equal to 25, When the transfer sheet is laminated on the metal member via an adhesive layer so that the surface on the pattern layer side faces the metal member and the release film is peeled off to form a laminate, the FI value of the low hiding area in the laminate measured from the transfer layer side is 10 or more.
14. The transfer sheet according to claim 1, wherein The metal component is an aluminum component.
15. A method for manufacturing an exterior member, which is a method for manufacturing an exterior member having a metal member, the manufacturing method comprising: a preparation step of preparing the transfer sheet according to any one of claims 1 to 14; and The laminating step is to laminate the transfer sheet on the metal member via an adhesive layer so that the surface of the transfer sheet on the pattern layer side faces the metal member.
16. The method for manufacturing an exterior member according to claim 15, wherein: After the lamination step, there is a peeling step of peeling the release film from the transfer sheet.
17. An exterior member comprising a metal member, The exterior component has a first protective layer, a second protective layer, a pattern layer, an adhesive layer, and the metal component in order in the thickness direction. The first protective layer and the second protective layer have a weathering agent, The FI value of the metal component is greater than or equal to 20 and less than or equal to 25, The exterior member has a region where the FI value measured from the first protective layer side is 10 or more.
Citation Information
Patent Citations
Decorative sheet, method for producing the same and decorative material
JP2016168785A
Decorative sheet and decorative material using same
CN112789175A
Three-dimensional molding film and resin molding
JP2019064027A
Decorative sheet and decorative material using same
US20210283879A1
Decorative member
WO2016125906A1