Polyurethane prepolymer composition, laminate, and preparation method and use thereof
Through the use of single-component polyurethane prepolymer composition, the problems of high-temperature curing energy consumption and insufficient properties are solved, and synthetic leather with improved properties can be prepared at a temperature of 45°C to 90°C, with improved peel strength and flex resistance. Curvature and logo embeddability.
Patent Information
- Application Number
- CN202380018468.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-25
- Filing Date
- 2023-01-13
- Publication Date
- 2024-10-01
AI Technical Summary
Existing polyurethane prepolymers require high-temperature curing when producing synthetic leather, which consumes a lot of energy. The synthetic leather obtained has insufficient peel strength, flex resistance and embossing properties, and cannot effectively solve the logo embedding properties of foam sheets. question.
Utilizes a one-component polyurethane prepolymer composition that is cured by water or moisture and does not require mixing with a polyol composition, with an isocyanate group content between 5.0% and 13.0% and a polyol functionality in the range of 1.5 to 3.0 , the use of catalysts and fillers, and the curing temperature is controlled between 45°C and 90°C to prepare laminates or synthetic leather with improved properties.
It realizes the preparation of laminates or synthetic leather at lower curing temperatures, improves its embossing properties, curing performance, peel strength and flex resistance, and improves logo embedding properties.
Smart Images

Figure BDA0004959875410000181 
Figure BDA0004959875410000182 
Figure BDA0004959875410000191
Abstract
Description
Technical Field
[0001] The invention relates to a polyurethane prepolymer composition, a laminate, and a preparation method and use thereof. Background Art
[0002] Polyurethane (PU) synthetic leather is usually composed of topcoat, color paint layer and substrate, and the property of color paint layer is critical for the property of obtained synthetic leather. For example, according to the demand in application, some synthetic leathers need to have embedded logo, and whether logo can be obtained depends mainly on the property of color paint layer. One-component or two-component polyurethane compositions comprising solvents have been used to produce color paint layer. Since non-solvent PU synthetic leather is a kind of eco-friendly solution for synthetic leather industry, some solvent-free solutions based on two-component polyurethane or based on water-based sheet materials as color paint layer have been developed. However, in order to produce these two-component polyurethane or based on water-based sheet materials, high temperature curing is needed, which consumes a lot of energy. In addition, the sheet material obtained has insufficient performance, such as peel strength, flex resistance and embossing properties.
[0003] WO2009 / 119752A discloses a solvent-free polyurethane-urea foam sheet produced by foaming a solvent-free urethane resin composition with air or an inert gas, forming the foamed material into a sheet-like material, and hardening the sheet-like material by heating. The solvent-free urethane resin composition comprises (A) a prepolymer produced by a reaction between a diisocyanate compound and a polyol having a molecular weight of 500 to 3000, (B) a crosslinking agent comprising a polyol having an average of 2 to 4 hydroxyl groups, and (C) water, wherein the residual amount of isocyanate groups in a mixture of component (A) and component (B) is 2.0% to 5.0% by mass, the residual amount of isocyanate groups in a mixture of component (A), component (B) and component (C) is 0.01% to 0.5% by mass, and the number average molecular weight of all polyols used as raw materials of component (A) and the polyol of component (B) is 600 or more. However, the patent discloses the use of high curing temperatures of 80°C to 130°C and does not address the logo embedding properties of the foam sheet.
[0004] CN103483529A discloses a method for manufacturing a polyurethane foam sheet by a combination of a moisture curing reaction and a foaming reaction, wherein the reaction of a prepolymer containing 20 to 25 wt% NCO produces a product having excellent viscosity at room temperature even in the absence of an organic solvent and does not require heating to melt. However, the patent application also discloses the use of a high curing temperature of 80 to 130°C and does not address the logo embedding properties of the foam sheet.
[0005] Therefore, there is still a need to provide new polyurethane prepolymer formulations and preparation methods to obtain laminates or synthetic leathers with improved properties, which can overcome one or more of the above-mentioned disadvantages. Summary of the invention
[0006] An object of the present invention is to overcome the problems of the prior art discussed above and to provide a polyurethane prepolymer composition and a method for preparing the same. The polyurethane prepolymer composition is a one-component system, the curing of which involves water or moisture and does not require mixing with a polyol composition. At the same time, the final synthetic leather based on the polyurethane product obtained from the polyurethane prepolymer composition achieves improved properties in terms of embossing properties as well as curing performance, peel strength and flex resistance. In addition, a laminate or synthetic leather can be prepared at a lower curing temperature of 45°C to 90°C.
[0007] Surprisingly, the present inventors have found that the above objects can be achieved by providing a polyurethane prepolymer composition comprising the reaction product of:
[0008] an isocyanate component; and
[0009] Polyol component,
[0010] Wherein the reaction product comprises isocyanate groups in an amount of 5.0 wt % to 13.0 wt % based on the total weight of the isocyanate component and the polyol component, and the polyol component has a functionality in the range of 1.5 to 3.0.
[0011] In a preferred embodiment of the present invention, in the polyurethane prepolymer composition, the amount of isocyanate groups is 8.0% to 12.5% by weight, preferably 9.0% to 12.0% by weight, more preferably 10.0% to 11.0% by weight, each based on the total weight of the isocyanate component and the polyol component.
[0012] In a preferred embodiment of the present invention, the polyurethane prepolymer composition contains no blocked isocyanate groups (NCO); that is, preferably, the polyurethane prepolymer composition contains only isocyanate groups in natural form and no isocyanate groups in blocked form.
[0013] In a preferred embodiment of the present invention, the isocyanate component is selected from aliphatic diisocyanates, aliphatic polyisocyanates, alicyclic diisocyanates, alicyclic polyisocyanates, aromatic diisocyanates, aromatic polyisocyanates and any mixture thereof, preferably the isocyanate component is diphenylmethane diisocyanate.
[0014] In a preferred embodiment of the present invention, the polyol component (B) has a functionality in the range of 1.9 to 2.8, preferably 2.0 to 2.6.
[0015] In a preferred embodiment of the present invention, the polyol component (B) has a weight average molecular weight in the range of 500 g / mol to 10000 g / mol and an OH value in the range of 20 mgKOH / g to 400 mgKOH / g.
[0016] In a preferred embodiment of the present invention, the polyurethane prepolymer composition further comprises at least one catalyst selected from tin compounds, amine compounds, imidazole compounds, morpholine compounds (such as 2,2-dimorpholinodiethyl ether) and any mixture thereof.
[0017] In a preferred embodiment of the present invention, the polyurethane prepolymer composition further comprises at least one filler selected from the group consisting of calcium carbonate, carbon black, silica, hydrated silica, alumina, titanium dioxide, zinc oxide, talc, mica, clay, kaolin, wollastonite, montmorillonite, aluminum hydroxide, barium sulfate, lignin, wood fiber, wood flour, magnesium carbonate monohydrate, dihydrate, trihydrate, tetrahydrate and pentahydrate, magnesium sulfate monohydrate, tetrahydrate, pentahydrate, hexahydrate and heptahydrate, copper (II) sulfate pentahydrate, calcium sulfate hemihydrate, calcium sulfate dihydrate, ferrous sulfate heptahydrate, potassium aluminum sulfate dodecahydrate, sodium sulfate decahydrate, sodium metasilicate pentahydrate, sodium metasilicate nonahydrate and any mixture thereof.
[0018] Another object of the present invention is to provide a process for producing a polyurethane prepolymer composition, wherein the process comprises mixing all components of the composition until homogeneous.
[0019] Another object of the present invention is to provide a laminate comprising the polyurethane prepolymer composition as mentioned above.
[0020] In a preferred embodiment of the present invention, the polyurethane prepolymer composition used as the color paint layer is sandwiched between a topcoat layer and a substrate layer to form a laminate.
[0021] In a preferred embodiment of the invention, the laminate is a synthetic leather, in particular an embossable or embeddable synthetic leather.
[0022] Another object of the present invention is to provide a method for producing a laminate, the method comprising the following steps:
[0023] (1) applying a polyurethane prepolymer composition to a release paper; and
[0024] (2) curing the applied composition in the presence of water,
[0025] Wherein in the curing step (2), the temperature is in the range of 45°C to 90°C, preferably 50°C to 85°C, more preferably 50°C to 80°C.
[0026] In a preferred embodiment of the present invention, the water is present in the form of moisture and / or in the form of water contained in the filler, such as crystal water of the filler and free water absorbed and / or adsorbed by the filler.
[0027] In a preferred embodiment of the present invention, water is introduced in the curing step (2) by controlling the moisture in the curing atmosphere.
[0028] In a preferred embodiment of the present invention, water is introduced in the curing step (2) by adding a filler having water of crystallization, absorbed free water and / or adsorbed free water.
[0029] In a preferred embodiment of the present invention, the wet air has a relative humidity in the range of 30% to 95%, preferably 40% to 70%, more preferably 45% to 65%.
[0030] In a preferred embodiment of the present invention, the filler is selected from the group consisting of monohydrate, dihydrate, trihydrate, tetrahydrate and pentahydrate of magnesium carbonate, monohydrate, tetrahydrate, pentahydrate, hexahydrate and heptahydrate of magnesium sulfate, copper (II) sulfate pentahydrate, calcium sulfate hemihydrate, calcium sulfate dihydrate, ferrous sulfate heptahydrate, potassium aluminum sulfate dodecahydrate, sodium sulfate decahydrate, sodium metasilicate pentahydrate, sodium metasilicate nonahydrate and any mixture thereof.
[0031] Another object of the present invention is to provide the use of the laminate in clothing, accessories, packaging, electronic devices, furniture, furniture upholstery, decorative items, sporting goods or leisure products.
[0032] Surprisingly, it has been found that by using the innovative non-solvent one-component polyurethane prepolymer composition as the color paint layer, the laminate or synthetic leather of the present invention has improved properties in terms of imprintable or logo embedding properties as well as curing performance, peel strength and flex resistance. In addition, the laminate or synthetic leather can be prepared at a relatively low curing temperature of 45°C to 90°C. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 The present invention shows a method for preparing a PU synthetic leather comprising the one-component polyurethane prepolymer composition of the present invention as a color paint layer.
[0034] Figure 2 Shown is a logo embedded in the PU synthetic leather of the present invention. DETAILED DESCRIPTION
[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the invention belongs. As used herein, unless otherwise specified, the following terms have the meanings assigned to them below.
[0036] As used herein, the articles "a" and "an" refer to one or to more than one (ie, to at least one) of the grammatical object of the article or component.
[0037] Unless otherwise indicated, all percentages (%) are by weight and are expressed as % by weight.
[0038] Unless otherwise indicated, the molecular weight of each component or polymer refers to the weight average molecular weight.
[0039] Unless otherwise stated, relative humidity (RH) is the ratio of the partial pressure of water vapor in humid air to the saturation pressure of water at the same temperature.
[0040] Unless otherwise stated, an isocyanate group refers to the organic group -N=C=O, also represented as -NCO.
[0041] Unless otherwise specified, isocyanate refers to an organic compound having one or more isocyanate groups. Diisocyanate refers to an organic compound having two (2) isocyanate groups. Polyisocyanate refers to an organic compound having three (3) or more isocyanate groups.
[0042] Unless otherwise specified, polyol refers to an organic compound having two or more hydroxyl (—OH) groups.
[0043] Unless otherwise specified, the OH value (sometimes also referred to as "hydroxyl value" or "hydroxyl number") is a measure of the concentration of hydroxyl groups in a polyol or polyol component. The OH value is calculated as the number of milligrams of potassium hydroxide required to neutralize the acetic acid absorbed when one gram of a chemical substance containing free hydroxyl groups (in this invention, a polyol or a polyol component) is acetylated.
[0044] Unless otherwise indicated, the functionality (abbreviated "Fn") of a polyol or polyol component refers to the number or average number of OH groups per molecule.
[0045] As used herein, the term "blocked isocyanate group" is used in its ordinary sense to those skilled in the art, who understand that it refers to a blocked isocyanate group (such as a carbamate or urea moiety) in its structure, which is obtained by the reaction of a natural isocyanate group (-NCO) with an isocyanate blocking agent. For many blocked isocyanates, blocking is performed by reaction with a compound containing active hydrogen (such as an alcohol, phenol, amide or amine). Blocked isocyanate groups can be converted to natural isocyanate groups by heating the blocked isocyanate at elevated temperatures.
[0046] As used herein, the term "polyurethane prepolymer" is intended to refer to a macromolecule or oligomer formed by the reaction between one or more polyols and one or more diisocyanates and / or polyisocyanates, wherein the diisocyanates and / or polyisocyanates are in excess. Typically, the polyurethane prepolymer may contain isocyanate groups in blocked or native form. In the present invention, the polyurethane prepolymer composition preferably does not contain blocked isocyanate groups.
[0047] As used herein, the amount of isocyanate groups is calculated based on the weight of the isocyanate groups and the total weight of the isocyanate component and the polyol component.The amount of blocked isocyanate groups is calculated based on the weight of the blocked isocyanate groups and the total weight of the isocyanate component and the polyol component.
[0048] The present invention provides a polyurethane prepolymer composition, which comprises a reaction product of the following substances:
[0049] an isocyanate component; and
[0050] Polyol component,
[0051] wherein the reaction product comprises isocyanate groups in an amount of 5.0 wt % to 13.0 wt % based on the total weight of the isocyanate component and the polyol component; and the polyol component has a functionality in the range of 1.5 to 3.0.
[0052] It should be noted that the reaction product of the isocyanate component and the polyol component contains unreacted or free isocyanate groups. The polyurethane prepolymer composition may undergo a curing process to make the final product. The polyurethane prepolymer composition may be stable for a long period of time under certain storage conditions. The polyurethane prepolymer composition may be prepared in situ prior to the curing process, or alternatively may be stored after preparation and then cured to produce the final product.
[0053] In the present invention, the polyurethane prepolymer composition comprises an isocyanate component (A), a polyol component (B), an optional catalyst (C) and an optional chain extender and / or crosslinker (D), a blowing agent (E), a filler (F) and additives and / or auxiliaries (G) such as pigments, thickeners, wetting agents and antioxidants.
[0054] Isocyanate component (A)
[0055] In the present invention, the isocyanate component (A) comprises at least one isocyanate. The isocyanate used to produce the polyurethane prepolymer composition of the present invention includes all isocyanates known for producing polyurethanes. The isocyanate may be any diisocyanate or polyisocyanate. These diisocyanates and polyisocyanates include aliphatic, cycloaliphatic, araliphatic and / or aromatic isocyanates such as trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, heptamethylene diisocyanate and / or octamethylene diisocyanate, 2-methylpentamethylene 1,5-diisocyanate, 2-ethylbutene 1,4-diisocyanate, pentamethylene 1,5-diisocyanate, butene 1,4-diisocyanate, 1-isocyano-3,3,5-trimethyl-5-isocyanomethylcyclohexane (isophorone diisocyanate, IPDI), 1,4-bis(isocyanomethyl)cyclohexane and / or 1,3-bis(isocyanomethyl)cyclohexane. Cyclohexane (HXDI), cyclohexane 1,4-diisocyanate, 1-methylcyclohexane 2,4-diisocyanate and / or 2,6-diisocyanate and / or dicyclohexylmethane 4,4'-diisocyanate, 2,4'-diisocyanate and 2,2'-diisocyanate, diphenylmethane 2,2'-diisocyanate, 2,4'-diisocyanate and / or 4,4'-diisocyanate (MDI), polymeric MDI, naphthalene-1,5-diisocyanate (NDI), toluene 2,4-diisocyanate and / or 2,6-diisocyanate (TDI), 3,3'-dimethyldiphenyl diisocyanate, 1,2-diphenylethane diisocyanate and / or phenylene diisocyanate. Particular preference is given to using diphenylmethane 2,2′-diisocyanate, 2,4′-diisocyanate and / or 4,4′-diisocyanate and polymeric MDI, in particular diphenylmethane 4,4′-diisocyanate or diphenylmethane 2,4′-diisocyanate or mixtures thereof, such as a mixture in a weight ratio of 1:1.
[0056] In the present invention, in the polyurethane prepolymer composition, the amount of the isocyanate group (NCO) is 5.0 wt % to 13.0 wt % based on the total weight of the polyurethane composition.
[0057] It has surprisingly been found in the present invention that the amount of isocyanate groups (NCO) in the polyurethane prepolymer composition has an important influence on the properties of the laminate or leather of the present invention obtained from the polyurethane prepolymer composition. An amount of isocyanate groups (NCO) of 8.0% to 12.5% by weight, preferably 9.0% to 12.0% by weight, more preferably 10.0% to 11.0% by weight, each based on the total weight of the isocyanate component and the polyol component, in combination with the following specific polyol component (B), leads to excellent properties of the polyurethane product of the present invention, especially embossing or logo embedding properties, especially logo embedding properties, as well as peel strength, curability and / or flex resistance. The inventors have found that blocked isocyanate groups (NCO) have an adverse effect on the properties of the polyurethane prepolymer composition, so in the present invention, the polyurethane prepolymer composition preferably does not contain blocked isocyanate groups.
[0058] Polyol component (B)
[0059] According to the present invention, the polyol component (B) comprises at least one polyol. The polyol used is selected from polyols having a functionality in the range of 1.5 to 3.0, preferably a functionality in the range of 1.9 to 2.8, more preferably 2.0 to 2.6.
[0060] The polyols used preferably have a weight average molecular weight in the range of 500 to 10000 g / mol, preferably 800 to 6000 g / mol, more preferably 900 to 4000 g / mol and an OH value in the range of 20 to 400 mgKOH / g, preferably 20 to 300 mgKOH / g, more preferably 20 to 200 mgKOH / g.
[0061] The polyol component (B) can be a single polyol or a mixture of at least two single polyols. Preferably, the polyol component (B) is a mixture of at least two single polyols. Preferably, a polyether polyol mixture is used as the polyol.
[0062] Suitable polyether polyols preferably have a weight average molecular weight in the range of 850 g / mol to 1500 g / mol, preferably 900 g / mol to 1200 g / mol, have a functionality in the range of 1.9 to 2.1, and have an OH value in the range of 50 mgKOH / g to 400 mgKOH / g, preferably 100 mgKOH / g to 200 mgKOH / g. These polyether polyols may be polyether polyols obtained by ring-opening polymerization of oxygen-containing heterocyclic compounds containing 3 to 6 carbon atoms, such as tetrahydrofuran. Preferably, the polyol is produced by polymerization of tetrahydrofuran as a repeating unit, preferably terminated with primary hydroxyl groups.
[0063] The polyether polyols used also preferably have a weight average molecular weight in the range of 3000 to 4000 g / mol, preferably 3200 to 3600 g / mol, have a functionality in the range of 1.5 to 2.0, and have an OH value in the range of 20 to 200 mgKOH / g, preferably 20 to 60 mgKOH / g. These polyether polyols may be polyether polyols produced by polymerizing epoxides such as ethylene oxide and / or propylene oxide as repeating units and using propylene glycol as a starter, preferably terminated with ethylene oxide having primary hydroxyl groups.
[0064] The polyether polyols used also preferably have a weight average molecular weight in the range of 1000 g / mol to 3000 g / mol, preferably 1500 g / mol to 2500 g / mol, and have a functionality in the range of 1.8 to 2.0, and have an OH value in the range of 20 mgKOH / g to 200 mgKOH / g, preferably 30 mgKOH / g to 100 mgKOH / g. These polyether polyols may be polyether polyols obtained by homopolymerization of diols such as propylene glycol, ethylene glycol, butanediol.
[0065] The polyether polyols used also preferably have a weight average molecular weight in the range of 3500 g / mol to 5000 g / mol, preferably 4000 g / mol to 4500 g / mol, and have a functionality in the range of 2.5 to 2.9, preferably 2.6 to 2.8, and have an OH value in the range of 20 mgKOH / g to 200 mgKOH / g, preferably 25 mgKOH / g to 100 mgKOH / g. The polyether polyols are preferably based on epoxides such as ethylene oxide (EO) and propylene oxide (PO). These polyether polyols can be polyether polyols produced by polymerizing epoxides as repeating units (such as produced by ethylene oxide and / or propylene oxide) and using glycerol as an initiator (preferably terminated by ethylene oxide with primary hydroxyl groups).
[0066] In a preferred embodiment according to the present invention, the polyol comprises a mixture of the above-mentioned polyether polyol derived from tetrahydrofuran and the above-mentioned polyether polyol derived from epoxide in a weight ratio of 1:1 to 3, preferably 1:1 to 1.5.
[0067] In a preferred embodiment according to the present invention, the polyol comprises a mixture of the above epoxide-derived polyether polyol and the above homopolymeric polyether polyol derived from diol in a weight ratio of 1:1 to 3, preferably 1:1 to 1.5.
[0068] The polyol used in the present invention is produced by a known method or is commercially available.
[0069] In the present invention, the polyol component (B), if in the form of a mixture, has an average functionality (FAv) of 1.5 to 2.1. Preferably, the polyol component (B) has an average functionality of 1.8 to 2.0, more preferably 1.9 to 2.0.
[0070] In the present invention, FAv refers to the average functionality of a plurality of polyols contained in the polyol component (a), and is represented by the following formula:
[0071] FAv=MR1*F1+MR2*F2+MR3*F3+…,
[0072] wherein MR1 is the molar ratio of the first polyol in the polyol component (B), and F1 is the functionality of the first polyol in the polyol component (B); MR2 is the molar ratio of the second polyol in the polyol component (B), and F2 is the functionality of the second polyol in the polyol component (B); MR3 is the molar ratio of the second polyol in the polyol component (B), and F2 is the functionality of the third polyol in the polyol component (B); …
[0073] In the present invention, the molecular weight of each component is determined using gel permeation chromatography (GPC) according to GB / T 21863-2008.
[0074] In the present invention, the OH value of each polyol component is determined according to DIN 53240.
[0075] In the present invention, functionality (Fn) refers to the number of terminal hydroxyl groups per polyol molecule. Functionality is determined by the following formula:
[0076] Fn=Mn*(OHv) / 56100
[0077] wherein Mn represents the number average molecular weight of the polyol, and OHv represents the OH value of the polyol component.
[0078] Catalyst (C)
[0079] As catalyst (C), all compounds which accelerate the isocyanate-polyol reaction can be used. Such compounds are known and described, for example, in "Kunststoffhandbuch, Volume 7, Polyurethane", Carl Hanser Verlag, 3rd edition, 1993, Chapter 3.4.1. These catalysts include amine-based catalysts and organometallic compound-based catalysts or mixtures thereof.
[0080] As the catalyst based on an organometallic compound, for example, an organotin compound can be used, such as tin(II) salts of organic carboxylic acids, for example, tin(II) acetate, tin(II) octoate, tin(II) ethylhexanoate, and tin(II) laurate; and dialkyltin(IV) salts of organic carboxylic acids, for example, dibutyltin diacetate, dibutyltin dilaurate, dibutyltin maleate, and dioctyltin diacetate; and Zn salts or Bi salts, for example, zinc octoate, bismuth(III) neodecanoate, bismuth 2-ethylhexanoate, and bismuth octoate; or an alkali metal salt of a carboxylic acid, for example, potassium acetate or potassium formate.
[0081] As amine-based catalysts, for example, strongly basic amines such as N,N,N-triethylaminoethoxyethanol, bis(N,N-dimethylaminoethyl) ether, dimethylcyclohexylamine, trimethylhydroxyethylethylenediamine, dimethylbenzylamine, triethylamine, triethylenediamine, pentamethyldipropylenetriamine, dimethylethanolamine, tetramethylhexamethylenediamine, tris(dimethylaminopropyl)hexahydrotriazine, dimethylaminopropylamine, diazabicycloundecene, diazabicyclononene, diazabicyclooctane, preferably triethylenediamine or bis(N,N-dimethylaminoethyl) ether, can be used.
[0082] As catalysts based on imidazole or morpholine, for example, imidazole, N-methylimidazole, N-ethylimidazole, N-ethylmorpholine, 2,2-dimorpholinodiethyl ether may be used.
[0083] The catalyst (C) used in the present invention is commercially available.
[0084] Generally, the amount of the catalyst (C) is preferably 0.05 to 5 wt%, more preferably 0.5 to 3 wt%, based on the total weight of the isocyanate component and the polyol component.
[0085] The catalyst can also be used to cure polyurethane prepolymer compositions to produce various articles, such as sheets, molded articles, foams, and the like.
[0086] Chain extenders and crosslinkers (D)
[0087] Chain extenders and / or crosslinkers (D) which can be used are substances having a molar mass of preferably less than 500 g / mol, particularly preferably 60 g / mol to 400 g / mol, wherein the chain extenders have 2 hydrogen atoms reactive toward isocyanates and the crosslinkers have 3 hydrogen atoms reactive toward isocyanates. These chain extenders can be used alone or preferably in the form of a mixture. Preference is given to using diols and / or triols having a molecular weight of less than 500, particularly 60 to 400 and in particular 60 to 350. Examples of those that can be used are aliphatic, cycloaliphatic and / or araliphatic diols having 2 to 14, preferably 2 to 10, carbon atoms, such as ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,10-decanediol, 1,2-dihydroxycyclohexane, 1,3-dihydroxycyclohexane and 1,4-dihydroxycyclohexane, diethylene glycol, dipropylene glycol, tripropylene glycol, diethanolamine or triols, such as 1,2,4-trihydroxycyclohexane or 1,3,5-trihydroxycyclohexane, glycerol and trimethylolpropane. Preference is given to using ethylene glycol, 1,3-propylene glycol or 1,4-butanediol, in particular 1,4-butanediol.
[0088] The amount of the chain extender and / or crosslinker is preferably 0.5 to 5 wt%, more preferably 1.5 to 4.5 wt%, based on the total weight of the isocyanate component and the polyol component.
[0089] Foaming agent (E)
[0090] The system may also contain a blowing agent (E). Suitable blowing agents (E) are known per se to the person skilled in the art and are, for example, selected from the group consisting of carbon dioxide, alkanes (such as propane, isobutane and pentane), alcohols (such as methanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methylpropanol and tert-butanol), ethers (such as dimethyl ether), ketones (such as acetone or methyl ethyl ketone), halogenated hydrocarbons (such as hydrofluoropropylene), water, nitrogen and mixtures of these substances. Preferably, water is used as the only blowing agent.
[0091] The amount of the blowing agent (E) is preferably 0.1 to 5% by weight, more preferably 0.1 to 1.0% by weight, based on the total weight of the isocyanate component and the polyol component.
[0092] Filler(F)
[0093] Fillers can be mixed with the polyurethane prepolymer composition during the curing process. Fillers can adjust or improve the mechanical, optical, electrical, acoustic or thermal properties or other qualities, such as visual appearance and surface quality, of the final product made from the polyurethane prepolymer composition.
[0094] According to the present invention, the filler can be selected from calcium carbonate, carbon black, silicon dioxide, hydrated silicon dioxide, aluminum oxide, titanium dioxide, zinc oxide, talc, mica, clay, kaolin, wollastonite, montmorillonite, aluminum hydroxide, barium sulfate, lignin, wood fiber, wood powder, magnesium carbonate monohydrate, dihydrate, trihydrate, tetrahydrate and pentahydrate, magnesium sulfate monohydrate, tetrahydrate, pentahydrate, hexahydrate and heptahydrate, copper (II) sulfate pentahydrate CuSO4 5H2O (CAS 7758-99-8), calcium sulfate hemihydrate CaSO4 0.5H2O (CAS10034-76-1), calcium sulfate dihydrate CaSO4 2H2O (CAS10101-41-4), ferrous sulfate heptahydrate FeSO4 7H2O (CAS 7782-63-0), potassium aluminum sulfate dodecahydrate KAl(SO4)2 12H2O (CAS 7784-24-9), sodium sulfate decahydrate Na2SO4·10H2O (CAS 7727-73-3), sodium metasilicate pentahydrate Na2SiO3·5H2O (CAS10213-79-3) and sodium metasilicate nonahydrate Na2SiO3·9H2O (CAS13517-24-3) and any mixture thereof. Among them, calcium carbonate, aluminum hydroxide and the above-mentioned compounds containing water of crystallization are preferred. Based on the total weight of the isocyanate component and the polyol component, the amount of the filler is 0 wt % to 200 wt %, preferably 1 wt % to 50 wt %, more preferably 5 wt % to 40 wt %.
[0095] The filler may contain water in the form of content, such as free water absorbed and / or adsorbed by the filler, or water in the form of crystal water. As an example, the filler may be wet calcium carbonate, or contain crystal water in the crystal lattice of the filler. The following compounds are particularly preferred: calcium carbonate, sodium metasilicate pentahydrate and sodium metasilicate nonahydrate. Based on the total weight of the filler, the filler may contain 0.05% to 65% by weight of water, preferably 0.10% to 60% by weight of water, more preferably 0.10% to 55% by weight of water.
[0096] The filler may also be any mixture of the above-mentioned different fillers.
[0097] Additives and / or auxiliary agents (G)
[0098] The additives and / or auxiliary agents (G) that can be used include surfactants, preservatives, pigments, colorants, antioxidants, silicone oil leveling agents, stabilizers, thickeners, wetting agents and reinforcing agents. When preparing non-solvent polyurethane systems, one or a mixture of the above additives and / or auxiliary agents is usually used to improve the properties of the obtained polyurethane product, such as texture replication, peel strength, flex resistance and curing properties.
[0099] Generally, the amount of the additives and / or auxiliary agents is preferably 0 to 12 wt %, more preferably 0.1 to 10 wt %, based on the total weight of the isocyanate component and the polyol component.
[0100] According to the present invention, thickeners, wetting agents and antioxidants are preferably used. Those materials that can be used (if present) include all thickeners, wetting agents and antioxidants commonly used in non-solvent polyurethane systems. The amount of each of them is preferably 0.1% to 5% by weight, more preferably 0.5% to 1% by weight, each based on the total weight of the non-solvent polyurethane system.
[0101] Further information on the manner of use and mode of action of the aforementioned auxiliaries and additives as well as further examples are given by way of example in the "Kunststoffhandbuch, Band 7, Polyurethane"
[0102] ["Plastics handbook, Volume 7, Polyurethanes"], Carl Hanser Verlag, 3rd edition, 1993, Chapter 3.4.
[0103] The polyurethane prepolymer composition of the present invention can be cured in the presence of water at a temperature of 45°C to 90°C, preferably 50°C to 85°C, more preferably 50°C to 80°C, even more preferably 50°C to 70°C, especially 50°C to 65°C to form the desired polyurethane product.
[0104] Water can be present in moisture, such as during moisture curing. In the moisture curing process, the amount of water is such that the reactants form a desired polyurethane product (such as a polyurethane sheet) at a relative humidity in the range of 30% to 95%, preferably 40% to 70%, and more preferably 45% to 65%.
[0105] Water can be present in the filler added to the polyurethane prepolymer composition before or during solidification. Water can be free water absorbed and / or adsorbed by filler or crystal water in the lattice of filler, which can be released from filler at the temperature during solidification. Filler can be selected from calcium carbonate, carbon black, silicon dioxide, hydrated silicon dioxide, aluminum oxide, titanium dioxide, zinc oxide, talcum, mica, clay, kaolin, wollastonite, montmorillonite, aluminum hydroxide, barium sulfate, lignin, wood fiber, wood powder, monohydrate, dihydrate, trihydrate, tetrahydrate and pentahydrate of magnesium carbonate, monohydrate, tetrahydrate, pentahydrate, hexahydrate and heptahydrate of magnesium sulfate, copper sulfate (II) pentahydrate, calcium sulfate hemihydrate, calcium sulfate dihydrate, ferrous sulfate heptahydrate, potassium aluminum sulfate dodecahydrate, sodium sulfate decahydrate, sodium metasilicate pentahydrate, sodium metasilicate nonahydrate or any mixture thereof. Filler can contain water in the form of content, or water in the form of crystal water. The filler may contain 0.05 to 65% by weight of water, preferably 0.10 to 60% by weight of water, more preferably 0.10 to 55% by weight of water, based on the total weight of the filler. As known to those skilled in the art, fillers containing water or capable of releasing water (e.g., water of crystallization) may introduce water into the polyurethane prepolymer composition. At elevated temperatures, e.g., at temperatures of 45° C. to 90° C., the introduced water may react with the polyurethane prepolymer composition and promote the curing process.
[0106] In the present invention, the relative humidity can be adjusted by any method known to those skilled in the art, for example, a humidity control oven can be used to form a desired relative humidity with water.
[0107] The present invention also provides a method for producing a polyurethane prepolymer composition, which comprises mixing an isocyanate component and a polyol component until they are uniform, that is, forming a homogeneous mixture. The mixing method can be any conventional method used in the art, such as mechanical stirring.
[0108] The present invention also provides a laminate obtained from the polyurethane prepolymer composition of the present invention.
[0109] In the present invention, the polyurethane prepolymer composition used as the color paint layer is sandwiched between the topcoat surface layer and the base layer. That is, the laminate includes the color paint layer formed by the polyurethane prepolymer composition and the topcoat surface layer or / and the base layer.
[0110] In the present invention, the laminate is a synthetic leather, in particular an embossable or embeddable synthetic leather.
[0111] The present invention also provides a method for producing a laminate, the method comprising the following steps:
[0112] (1) applying a polyurethane prepolymer composition to a release paper; and
[0113] (2) curing the applied composition in the presence of water,
[0114] Wherein in the curing step (2), the temperature is in the range of 45°C to 90°C, preferably 50°C to 85°C, more preferably 50°C to 80°C.
[0115] In the present invention, water is introduced in the curing step (2) by controlling the moisture under the curing atmosphere.
[0116] In the present invention, water is introduced in the solidification step (2) by adding a filler having crystal water, absorbed free water and / or adsorbed free water.
[0117] In the present invention, the moisture is controlled to have a relative humidity in the range of 30% to 95%, preferably 40% to 70%, more preferably 45% to 65%. As mentioned above, the moisture is provided by water, which is in the form of moisture and / or is contained in the filler and forms moisture by heating.
[0118] In the present invention, the filler used in the above method is selected from the monohydrate, dihydrate, trihydrate, tetrahydrate and pentahydrate of magnesium carbonate, the monohydrate, tetrahydrate, pentahydrate, hexahydrate and heptahydrate of magnesium sulfate, copper (II) sulfate pentahydrate, calcium sulfate hemihydrate, calcium sulfate dihydrate, ferrous sulfate heptahydrate, potassium aluminum sulfate dodecahydrate, sodium sulfate decahydrate, sodium metasilicate pentahydrate, sodium metasilicate nonahydrate and any mixture thereof.
[0119] In the present invention, in step (1), the polyurethane prepolymer composition may be formed into a layer or sheet-like material using an application method such as dip coating, knife coating, roller coating, and spin coating.
[0120] The invention also provides for the use of the laminate as upper material in clothing and accessories, as covering material for boxes and electronic devices, as synthetic leather covering in the furniture / furniture upholstery sector, in decorative items, sports goods or leisure products.
[0121] The laminate of the present invention can be used anywhere as a substitute for real leather. For example, in clothing and accessories, as the upper material of handbags, shoes, boots, gloves, hats or outerwear items (such as jackets, pants and belts). It can also be used as a covering material for boxes and electronic devices (such as suitcases, briefcases, watch straps, smart phone boxes, earphone boxes and camera boxes). In addition, in the field of furniture / furniture decoration, the laminate of the present invention can be used as a synthetic leather covering for sofas, car seats, car interiors, chairs, cushions and coffee tables, and for certain types of decorations (such as wall hangings). In addition, the laminate of the present invention can also be used for sports goods or leisure products, such as game balls, saddles, toys, etc.
[0122] Top coating
[0123] In the present invention, the topcoat layer can be any layer that can be combined with a color paint layer in the art. Suitable aqueous polyurethane dispersions for forming the surface layer of the topcoat layer are disclosed in, for example, PCT / CN2020 / 084834, the contents of which are expressly incorporated herein by reference.
[0124] Color paint layer
[0125] In the present invention, the color paint layer is obtained from the polyurethane prepolymer composition according to the present invention.
[0126] The present invention also provides a laminate produced by the polyurethane prepolymer composition. The laminate of the present invention can be used as a color paint layer for producing synthetic leather. The synthetic leather includes a base layer, wherein the base layer is below the color paint layer. The top coat and the color paint layer are as defined above. The base layer is obtained as follows:
[0127] Basal layer
[0128] In the present application, synthetic leather includes a substrate layer below the color paint layer. In principle, the substrate layer can be any layer that can form an adhesive bond with the color paint layer. The thickness of the substrate layer is usually in the range of 0.01mm to 20mm, preferably in the range of 0.1mm to 15mm. The substrate layer is, for example, a nonwoven fabric, a textile, real leather, wood, TPU, other plastics or split leather. A preferred embodiment utilizes a nonwoven fabric or split leather as the substrate layer.
[0129] PU sheets / laminates / leather can be processed in many ways, for example:
[0130] The PU sheet / laminate / leather is continuously embossed by a hot embossing roller at a temperature of 150°C to 250°C and then the texture / pattern is replicated.
[0131] The PU sheet / laminate / leather is heated to a desired temperature, such as 150°C to 250°C, and then the leather is embossed continuously by an embossing roller without a heater.
[0132] The PU sheet / laminate / leather is heated to a desired temperature, such as 150°C to 250°C, and then the leather is continuously sucked by a vacuum embossing roll with micro voids and a textured surface.
[0133] The PU sheet / laminate / leather is embossed by a hot plate (150°C to 250°C) instead of a continuous way like embossing rollers.
[0134] The PU sheet / laminate / leather is pressed by a hot pressing die or plate (150°C to 250°C) with a designed brand logo or character in a very short time such as 1 to 10 seconds.
[0135] In this application, the curing performance test of PU sheet / laminate / leather is carried out at a shorter curing time of 10 minutes and a longer curing time of 15 minutes or 30 minutes. If the curing performance is excellent in a shorter time, the product is suitable for a continuous production process in actual production. If the curing performance is excellent until a longer time, the product is more suitable for a discontinuous production process in actual production.
[0136] Example
[0137] The present invention will now be described with reference to Examples and Comparative Examples, but these Examples and Comparative Examples are not intended to limit the present invention.
[0138] Use the following ingredients:
[0139] Polyol No. 1 is a polypropylene glycol having a functionality of 1.93 and an OH value of 55 mgKOH / g.
[0140] Polyol No. 2 was produced by polymerizing ethylene oxide as a repeating unit and using propylene glycol as an initiator, and was capped with ethylene oxide having a primary hydroxyl group, had a functionality of 1.76, and an OH value of 29.5 mgKOH / g.
[0141] Polyol No. 3 was produced by polymerizing tetrahydrofuran as a repeating unit and was terminated with primary hydroxyl groups, had a functionality of 2, and had an OH value of 112.3 mgKOH / g.
[0142] Polyol No. 4 was produced by polymerizing ethylene oxide as a repeating unit and using glycerol as an initiator, and was terminated with ethylene oxide having a primary hydroxyl group, had a functionality of 2.72 and an OH value of 35 mgKOH / g.
[0143] Polyol No. 5 was produced by polymerizing ethylene oxide and polypropylene oxide as repeating units and using TDA (toluenediamine) as an initiator, and was capped with polypropylene oxide, had a functionality of 3.8, and an OH value of 405 mgKOH / g.
[0144] Isocyanate (ISO) No. 1: Lupranat MS-C from BASF.
[0145] Isocyanate (ISO) No. 2: Lupranat MI from BASF.
[0146] Catalyst: 2,2-dimorpholinodiethyl ether, abbreviated as "DMDEE" (CAS:
[0147] 6425-39-4).
[0148] Filler 1: CaCO3, containing 0.35 wt% water.
[0149] Filler 2: Sodium metasilicate nonahydrate (CAS 13517-24-3), abbreviated as
[0150] "SMNH".
[0151] These raw materials were used to prepare PU prepolymer formulations and comparative formulations, which were denoted as "Formulations 1 to 10" and "Comparative Formulations 1 to 7". Then, several synthetic leather samples were prepared from the polyurethane prepolymer composition by the method described below, which were denoted as "Example 1 to Example 10" and "Comparative Example 1 to Comparative Example 7". Synthetic leather samples (e.g., Formulation 7) made from the same polyurethane prepolymer composition under different curing conditions (temperature, relative humidity, or filler content) were denoted, for example, as Example 7-1, Example 7-2, etc.
[0152] In order to compare the PU synthetic leather samples with commercially available synthetic leather products, solvent-based PU leather and water-based PU leather were used. The solvent-based PU leather was made of a DMF-based polyurethane resin (from Warren Synthetic Leather (Suzhou) Co., Ltd. (Warren Synthetic Leather (Suzhou) CO., LTD)). The water-based PU leather was made of a water-based polyurethane resin (from Warren Synthetic Leather (Suzhou) Co., Ltd.).
[0153] Property Test
[0154] Peel strength test
[0155] The peel strength test is carried out on the PU artificial leather just peeled off from the cured release paper, and the test should be completed within 20 minutes, including sample preparation and testing. This test follows the standard SATRA TM 411.
[0156] Curing properties test
[0157] The curing properties were judged by pressing the top coating of the PU synthetic leather with a fingernail and then visually evaluating according to the following ratings:
[0158] Level 1: Nail mark rebounds for >10 seconds, or the topcoat is damaged;
[0159] Level 2: Nail mark rebound (7 seconds to 9 seconds);
[0160] Level 3: Nail mark rebound (4 seconds to 6 seconds);
[0161] Level 4: Nail mark rebound (1 second to 3 seconds);
[0162] Level 5: No obvious nail marks.
[0163] Flexibility test
[0164] The flexural resistance test was carried out according to standard ISO 5402 as follows:
[0165] The test pieces of PU synthetic leather were prepared according to ISO 2418, including cutting at least three vertical test pieces and at least three horizontal test pieces, conditioning the test pieces according to ISO 2419 and testing in a conditioned atmosphere. The test pieces were visually evaluated for cracks / adhesion loss / color change after 25 times magnification. The expression "pass" indicates that there are no visible cracks / adhesion loss / visible color change. The expression "failure" means that there is damage on the test piece.
[0166] Tests to identify embedded properties:
[0167] The logo embedding property test was performed as follows.
[0168] The PU laminate / leather is pressed by a hot pressing die or plate (150°C to 250°C) with a designed brand logo or character in a very short time such as 1 to 10 seconds.
[0169] The logo embedding machine was a Model 380 (Nanjing Yueyi Clothing Co. Ltd) equipped with a custom embossing plate. The logo embedding process was as follows:
[0170] (1) Set the temperature to 160°C and wait until the embossable sheet maintains a constant temperature;
[0171] (2) Set the pressing time to 1 second;
[0172] (3) Place the leather sample on the console, first press the pressure button, then press the operation button with both hands. Once the process is completed, the embossing plate automatically moves upwards, and the sample can then be collected.
[0173] The depth of the embedded logo was measured using a 3D profilometer measurement system from Keyence (model: VR-3200). The logo typically includes one or more shapes or characters. Figure 2A logo consisting of two squares, four letters "B", "A", "S" and "F" in larger fonts, and a slogan in smaller fonts is shown. As shown in Table 1, the first square, denoted as "Square 1", is a larger square with its central portion taken out; the second square, denoted as "Square 2", is a smaller square. In the synthetic leather in which the logo is embedded, the logo is formed by pressing the synthetic leather to obtain a recessed area or several discontinuous recessed areas. In a designated area of 3.5 cm × 1.2 cm of the leather sample, the maximum height relative to the reference plane is measured, and its value is denoted as ΔHmax. Similarly, the minimum height relative to the same reference plane is measured, and its value is denoted as ΔHmin. The difference ΔHmax-ΔHmin is expressed as the depth of the embedded logo. In this test, ΔHmax and ΔHmin are measured on six designated areas of the leather sample (two squares, letters "B", "A", "S" and "F" in larger fonts), and the average of the six ΔHmax-ΔHmin values is reported as the depth of the embedded logo.
[0174] Table 1
[0175]
[0176] Preparation of PU prepolymer
[0177] The following components in Table 2 were used to prepare the PU prepolymer. In each case, all components of the PU prepolymer were mixed to form a mixture for forming a color paint layer of PU synthetic leather.
[0178] Table 2
[0179]
[0180]
[0181] Preparation of PU synthetic leather
[0182] Solution 1
[0183] A PU synthetic leather comprising a top coating layer, a color paint layer and a base layer was prepared.
[0184] Processing reference Figure 1 .like Figure 1 As shown, the processing of polyurethane synthetic leather is as follows:
[0185] First, a commercially available formulation (Haptex CC 6945 / 91C-CB, from BASF) for forming a topcoat was applied to a Favini B100 release paper by knife coating at a thickness of 100 μm within 4 hours, followed by drying at 80° C. for 2 minutes and at 120° C. for 2 minutes in oven No. 1. Next, each mixture for forming a color lacquer layer in Table 1 was applied to the top of the dried topcoat by knife coating at a thickness of 250 μm, and heated at a temperature of 50° C. and a relative humidity of 50% in oven No. 2 for 1.5 to 10 minutes. Then, a substrate layer made of a polymer composition of 70% by weight polyester and 30% by weight polyamide with a thickness of 1 mm was applied to the dried color lacquer layer, and cured by heating at a temperature of 50° C. and a relative humidity (RH) of 50% in oven No. 3 for 10 to 30 minutes, followed by pressing. PU synthetic leather was obtained after peeling off the release paper. The experimental results of PU leather performance are shown in Table 3.
[0186] Table 3
[0187]
[0188]
[0189] As can be seen from the above results, the inventive examples of the polyurethane prepolymer composition achieve better peel strength and curing properties than the comparative examples.
[0190] Solution 2
[0191] Test the properties of PU leather under different curing conditions.
[0192] Regarding the tests as shown in Table 4 below, the polyurethane prepolymer composition according to Formulation 2 was used to form a color coating layer, except that the curing conditions were changed in each test.
[0193] Table 4
[0194]
[0195]
[0196] *(5min) refers to the curing time in a climate chamber.
[0197] **Logo embedment refers to the average depth of the logo in mm.
[0198] Regarding the tests as shown in Table 5 below, the polyurethane prepolymer composition according to Formulation 7 was used to form a color coating layer, except that the curing conditions were changed in each test.
[0199] Table 5
[0200]
[0201]
[0202] From the above results, it can be seen that the artificial leather of the present invention produced from the non-solvent one-component polyurethane prepolymer composition of the present invention has a logo embedding property equal to or better than that of solvent-based PU leather or water-based PU leather.
[0203] Solution 3
[0204] The following components and amounts in Table 6 were used to prepare PU prepolymers. In each case, all components of the PU prepolymer were mixed to form a mixture for forming a color paint layer of PU synthetic leather. The filler CaCO3 contained 0.35% by weight of water.
[0205] Table 6
[0206] Weight / portion Preparation 2 Comparative Preparation 3 ISO No. 2 36.6 70 Polyol No. 1 31.7 15 Polyol No. 2 31.7 15 <![CDATA[CaCO3]]> 30 30 DMDEE 2 2 Diacetyl monoxime 0 18 NCO / % 10.1 11.6 Closed NCO / % 0 10.8
[0207] Comparative Formulations 5 to 7 were prepared by blending Formulation 2 and Comparative Formulation 3 at different ratios to obtain PU prepolymer compositions having different amounts of blocked isocyanate groups, as shown in Table 7. The preparation of PU synthetic leather was the same as that in Example 1.
[0208] Table 7
[0209] Comparative Preparation 4 Comparative Preparation 5 Comparative Preparation 6 Amount of Preparation 2 75% by weight 80% by weight 83.3% by weight Comparative Preparation 3 Amount 25 wt% 20% by weight 16.7 wt% NCO / % 10.4 9.16 8.59 Closed NCO / % 2.7 2.16 1.80
[0210] The leather samples made from the polyurethane prepolymer compositions of Comparative Formulations 4 to 6 were cured at a temperature of 80° C. and a relative humidity of 70% for 10 to 30 minutes. The results are shown in Table 8.
[0211] Table 8
[0212]
[0213] In order to compare the effects of blocked isocyanate groups and unblocked isocyanate groups on its properties, we conducted the following experiment to deblock the isocyanate groups, wherein leather samples made from the PU prepolymer compositions of Comparative Formulations 4 to 6 were cured at 80° C. and 70% relative humidity for 10 to 30 minutes, and then transferred to an oven at 130° C. to 140° C. for 5 to 30 minutes to convert most of the blocked isocyanate groups into natural isocyanate groups. The results are shown in Table 9.
[0214] Table 9
[0215]
[0216] From the above results in Tables 8 and 9, it can be seen that the leather samples made from the PU prepolymer composition containing blocked isocyanate groups (NCO) have low peel strength and curing properties, which are indicated by low curing grade, low peel strength and reduced logo embedding depth. The PU prepolymer composition of Comparative Example 4 containing 2.7% of blocked isocyanate groups (NCO) has significantly worse curing properties than Comparative Example 6 containing 1.8% of blocked isocyanate groups (NCO).
[0217] Furthermore, it can be seen that, for leather samples made from the same formulation, the leather samples in Table 8 containing blocked isocyanate groups exhibit significantly lower peel strength and curing properties than the corresponding leather samples in Table 9 containing only a small amount of blocked isocyanate groups.
[0218] Solution 4
[0219] Formulation 10 was selected for preparing PU synthetic leather with a filler containing crystal water, sodium metasilicate nonahydrate (CAS 13517-24-3), which kept the synthetic leather at 50 RH to 60% RH at an oven temperature as shown in Table 10. Then no humidity control oven was required to provide water. The experimental results of the PU leather properties are shown in Table 10.
[0220] Table 10
[0221]
[0222] From the above results, it can be seen that, with the help of the crystal water present in the filler, the leather sample made from the PU prepolymer composition has good properties in terms of curing properties, peel strength and flexure by controlling the temperature alone. It can also be seen that compared with the leather samples cured in moisture (see Examples 7-1 to 7-12), the leather samples prepared by relying on the crystal water of the filler need to be cured at a higher temperature to obtain good properties.
[0223] The structures, materials, compositions and methods described herein are intended to be representative embodiments of the present invention, and it should be understood that the scope of the present invention is not limited by the scope of these embodiments. Those skilled in the art will recognize that the present invention can be operated using variations of the disclosed structures, materials, compositions and methods, and such variations are considered to be within the scope of the present invention. Therefore, the present invention is intended to cover such modifications and variations that fall within the scope of the appended claims.
Claims
1. A polyurethane prepolymer composition comprising the reaction product of: an isocyanate component; and Polyol component, wherein the reaction product comprises isocyanate groups in an amount of 5.0 wt % to 13.0 wt % based on the total weight of the isocyanate component and the polyol component; and The polyol component has a functionality ranging from 1.5 to 3.
0.
2. The polyurethane prepolymer composition according to claim 1, wherein the amount of the isocyanate groups is 8.0 wt % to 12.5 wt %, preferably 9.0 wt % to 12.0 wt %, more preferably 10.0 wt % to 11.0 wt %, each based on the total weight of the isocyanate component and the polyol component.
3. The polyurethane prepolymer composition according to claim 1, wherein the polyurethane prepolymer composition does not contain blocked isocyanate groups.
4. The polyurethane prepolymer composition according to claim 1, wherein the isocyanate component is selected from aliphatic diisocyanates, aliphatic polyisocyanates, alicyclic diisocyanates, alicyclic polyisocyanates, aromatic diisocyanates, aromatic polyisocyanates and any mixture thereof, preferably the isocyanate component is diphenylmethane diisocyanate.
5. The polyurethane prepolymer composition of claim 1, wherein the polyol component has a functionality ranging from 1.9 to 2.8, preferably 2.0 to 2.
6. 6 . The polyurethane prepolymer composition according to claim 5 , wherein the polyol component has a weight average molecular weight in the range of 500 g / mol to 10,000 g / mol and an OH value in the range of 20 mgKOH / g to 400 mgKOH / g.
7. The polyurethane prepolymer composition according to claim 1, wherein the polyurethane prepolymer composition further comprises at least one catalyst selected from the group consisting of tin compounds, amine compounds, imidazole compounds, morpholine compounds such as 2,2-dimorpholinodiethyl ether, and any mixture thereof.
8. The polyurethane prepolymer composition according to claim 1, wherein the polyurethane prepolymer composition further comprises at least one filler selected from the group consisting of calcium carbonate, carbon black, silica, hydrated silica, alumina, titanium dioxide, zinc oxide, talc, mica, clay, kaolin, wollastonite, montmorillonite, aluminum hydroxide, barium sulfate, lignin, wood fiber, wood flour, monohydrate, dihydrate, trihydrate, tetrahydrate and pentahydrate of magnesium carbonate, monohydrate, tetrahydrate, pentahydrate, hexahydrate and heptahydrate of magnesium sulfate, copper (II) sulfate pentahydrate, calcium sulfate hemihydrate, calcium sulfate dihydrate, ferrous sulfate heptahydrate, potassium aluminum sulfate dodecahydrate, sodium sulfate decahydrate, sodium metasilicate pentahydrate, sodium metasilicate nonahydrate and any mixture thereof.
9. A process for producing a polyurethane prepolymer composition according to any one of claims 1 to 8, the process comprising mixing all components of the composition. 10 . A laminate comprising the polyurethane prepolymer composition according to claim 1 as a color paint layer.
11. The laminate according to claim 10, wherein the polyurethane prepolymer composition is sandwiched between the topcoat surface layer and the substrate layer.
12. The laminate according to claim 10, which is a synthetic leather, in particular an embossable or embeddable synthetic leather.
13. A method for producing a laminate according to any one of claims 10 to 12, the method comprising the steps of: (1) applying the polyurethane prepolymer composition according to any one of claims 1 to 8 onto a release paper; as well as (2) curing the applied composition in the presence of water, Wherein in the annealing step (2), the temperature is in the range of 45°C to 90°C, preferably 50°C to 85°C, more preferably 50°C to 80°C.
14. The method according to claim 13, wherein the water is introduced in the curing step (2) by controlling the moisture in the curing atmosphere.
15. The method according to claim 14, wherein the moisture is controlled to have a relative humidity in the range of 30% to 95%, preferably 40% to 70%, more preferably 45% to 65%.
16. The method according to claim 13, wherein the water is introduced in the solidification step (2) by adding a filler having crystal water, absorbed free water and / or adsorbed free water.
17. The method according to claim 16, wherein the filler is selected from the group consisting of monohydrate, dihydrate, trihydrate, tetrahydrate and pentahydrate of magnesium carbonate, monohydrate, tetrahydrate, pentahydrate, hexahydrate and heptahydrate of magnesium sulfate, copper (II) sulfate pentahydrate, calcium sulfate hemihydrate, calcium sulfate dihydrate, ferrous sulfate heptahydrate, potassium aluminum sulfate dodecahydrate, sodium sulfate decahydrate, sodium metasilicate pentahydrate, sodium metasilicate nonahydrate and any mixture thereof.
18. Use of the laminate according to any one of claims 10 to 12 in clothing, accessories, packaging, electronic devices, furniture, furniture upholstery, decorative items, sporting articles or leisure products.
Citation Information
Patent Citations
Manufacturing method of polyurethane foam sheet and leather sample sheet made by using it
CN103483529A
Solvent-free polyurethane-urea foam sheet, method for production thereof, and synthetic leather
WO2009119752A1