Copolymerization reactant of tetrahydrofuran and plant-derived 2-methyltetrahydrofuran, and method for producing same
Through acid contact purification and copolymerization process, the coloring problem of 2-methyltetrahydrofuran in polytetramethylene ether glycol is solved, and polytetramethylene ether glycol with low color value and high bio-based carbon content is produced , which meets the performance requirements of biological polyurethane materials.
Patent Information
- Application Number
- CN202380017282.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-28
- Filing Date
- 2023-01-18
- Publication Date
- 2024-10-01
AI Technical Summary
There is a lack of effective purification methods in the prior art to produce non-coloring 2-methyltetrahydrofuran (2MeTHF), which causes coloring in polytetramethylene ether glycol and reduces its value as an industrial raw material, especially in biotechnology. There are performance deficiencies in the development of polyurethane materials.
Through the purification process of contact with acid, separation and dehydration using inorganic acid or strong acidic ion exchange resin, combined with distillation extraction, high-purity 2-methyltetrahydrofuran is obtained, and is added in the copolymerization reaction of tetrahydrofuran and 2-methyltetrahydrofuran. Strong acid catalyst, controls reaction conditions to inhibit coloration.
Achieved the production of polytetramethylene ether glycol with a Hassen unit color value below 60, maintained a bio-based carbon content rate of 97.00% to 100%, and a number average molecular weight between 500 and 5000, ensuring the quality of polyurethane materials. Excellent performance and industrial value.
Smart Images

Figure BDA0004944874180000161
Abstract
Description
Technical Field
[0001] The present invention relates to polytetramethylene ether glycol which is a copolymerization reaction product of tetrahydrofuran and 2-methyltetrahydrofuran derived from plants and a method for producing the same. Background Art
[0002] Polytetramethylene ether glycol is one of the polyols used in polyurethane materials, polyester materials, and polycarbonate materials. Polyurethane materials and polyester materials are used for elastomers, spandex, and the like. Among polytetramethylene ether glycols, polytetramethylene ether glycol obtained by copolymerization of tetrahydrofuran (hereinafter, also referred to as THF) and alkyltetrahydrofuran is known to have excellent flexibility and tensile properties when used as a raw material for spandex (Patent Documents 1 and 2).
[0003] In the fiber used for spandex, the value of polytetramethylene ether glycol with color (color difference) as an industrial raw material is reduced from the viewpoint of design and appearance. Therefore, a purification method of THF, which has been a raw material of polytetramethylene ether glycol, has been proposed. For example, there are methods that focus on dihydrofuran as an impurity and convert it into a high boiling point product by reacting dihydrofuran with an acid catalyst or an acid to facilitate separation by distillation (Patent Documents 2 to 4); a method that converts the impurity to be purified into γ-butyrolactone as a peroxide for purification (Patent Document 5). In these reports, the production method of purified THF is not limited, and there is no distinction between petroleum-based, biological-based, and by-product-based products. THF with substituents is also included in the purification object. However, even though a large number of reports have been made, no purification method limited to 2-methyltetrahydrofuran (hereinafter, also referred to as 2MeTHF) has been found.
[0004] In addition, dihydrofuran is mentioned as an impurity of THFs (particularly THF and 3-methyltetrahydrofuran) used in the production of polytetramethylene ether glycol (Patent Documents 2 to 4), but there is no report focusing on impurities in 2MeTHF.
[0005] On the other hand, in order to realize a recycling-oriented society in recent years and to counter the depletion of fossil fuels, the society needs to develop petroleum-free products using raw materials from biomass. Currently, there are biopolyols using vegetable oils as raw materials, but the biopolyols most suitable for spandex fiber applications are limited, and biopolyether polyols and biopolyurethane resins with excellent properties are needed (Patent Document 6).
[0006] 2MeTHF is usually produced by using a furfural method and a levulinic acid method using raw materials from biomass as starting materials. Therefore, it is expected to be used as a raw material for biopolyether polyols. However, biopolyether polyols synthesized using 2MeTHF as a raw material have the problem of coloration. Therefore, in order to prevent the value as an industrial raw material from being reduced, a method for producing polytetramethylene ether glycol that does not undergo coloration is expected.
[0007] Patent Document 1: Japanese Patent Application Publication No. 2011-162780
[0008] Patent Document 2: Japanese Patent No. 4144656
[0009] Patent Document 3: Japanese Patent No. 6191213
[0010] Patent Document 4: Japanese Patent No. 6601006
[0011] Patent Document 5: Japanese Patent Application Publication No. 2016-17041
[0012] Patent Document 6: International Publication No. 2018 / 220983 Summary of the invention
[0013] The problem to be solved by the present invention is to provide polytetramethylene ether glycol which does not cause coloring and a method for producing the same in order to develop polytetramethylene ether glycol having new properties excellent in chemical properties or mechanical properties as a bio-polyurethane material and to use 2MeTHF derived from plants so as not to reduce its value as an industrial raw material.
[0014] The present inventors have conducted intensive studies on the above-mentioned subject and have found that polytetramethylene ether glycol with reduced coloration can be produced by using 2-methyltetrahydrofuran purified by a purification step including a step of contacting with an acid as 2-methyltetrahydrofuran in a copolymerization reaction of tetrahydrofuran and 2-methyltetrahydrofuran. That is, the gist of the present invention is as follows.
[0015] [1] A polytetramethylene ether glycol which is a copolymerization reaction product of tetrahydrofuran and 2-methyltetrahydrofuran derived from plants, wherein the polytetramethylene ether glycol has a Hazen unit color value (APHA color) of 60 or less.
[0016] [2] The polytetramethylene ether glycol according to [1], wherein the Hazen unit color value (APHA color) is 30 or less.
[0017] [3] The polytetramethylene ether glycol according to [1], wherein the biobased carbon content (%) of the plant-derived 2-methyltetrahydrofuran is 100%.
[0018] [4] The polytetramethylene ether glycol according to [1], wherein the tetrahydrofuran is plant-derived and the bio-based carbon content (%) of the tetrahydrofuran is 97.00% to 100%.
[0019] [5] The polytetramethylene ether glycol according to [1], wherein the number average molecular weight of the polytetramethylene ether glycol is 500 to 5,000.
[0020] [6] A method for producing polytetramethylene ether glycol, comprising: a step of obtaining purified plant-derived 2-methyltetrahydrofuran through a purification step including a step of contacting plant-derived 2-methyltetrahydrofuran with an acid; and a step of copolymerizing the purified plant-derived 2-methyltetrahydrofuran with tetrahydrofuran.
[0021] [7] The method for producing polytetramethylene ether glycol according to [6], wherein the purity of the purified plant-derived 2-methyltetrahydrofuran is 99.90% or more.
[0022] [8] The method for producing polytetramethylene ether glycol according to [6], wherein the acid used in the purification step is an inorganic acid or a strongly acidic ion exchange resin.
[0023] [9] The method for producing polytetramethylene ether glycol according to [8], wherein in the purification step, the plant-derived 2-methyltetrahydrofuran is contacted with an acid at a temperature in the range of 20°C to 80°C.
[0024]
[10] The method for producing polytetramethylene ether glycol according to [8], wherein in the purification step, the plant-derived 2-methyltetrahydrofuran is contacted with an acid at a temperature in the range of 30°C to 60°C.
[0025]
[11] The method for producing polytetramethylene ether glycol according to [8], wherein the purification step includes: a step of contacting plant-derived 2-methyltetrahydrofuran with an inorganic acid or a strongly acidic ion exchange resin; a step of separating and dehydrating the 2-methyltetrahydrofuran and the inorganic acid or the strongly acidic ion exchange resin; and a step of extracting the purified 2-methyltetrahydrofuran by distillation.
[0026]
[12] The method for producing polytetramethylene ether glycol according to [6], wherein the purity of the tetrahydrofuran is 99.50% or more.
[0027]
[13] The method for producing polytetramethylene ether glycol according to [6], wherein in the copolymerization step, the ratio (mass ratio) of tetrahydrofuran to plant-derived 2-methyltetrahydrofuran is 99:1 to 50:50.
[0028]
[14] The method for producing polytetramethylene ether glycol according to [6], wherein in the copolymerization step, 5% to 40% by mass of a strong acid catalyst is added relative to the total mass of tetrahydrofuran and 2-methyltetrahydrofuran.
[0029]
[15] The method for producing polytetramethylene ether glycol according to [6], wherein in the copolymerization step, 8% to 40% by mass of a strong acid catalyst is added relative to the total mass of tetrahydrofuran and 2-methyltetrahydrofuran.
[0030] According to the present invention, the coloring of polytetramethylene ether glycol obtained by copolymerization of THF and 2MeTHF can be suppressed, and the industrial value for use in spandex fibers, etc. can be not impaired. In addition, a bio-polyurethane material using the polytetramethylene ether glycol can be provided. DETAILED DESCRIPTION
[0031] Hereinafter, an embodiment of the present invention will be described in detail. However, the following description is an example of the embodiment of the present invention, and the present invention is not limited to these contents, and various modifications can be made within the scope of the gist.
[0032] [Polytetramethylene ether glycol containing bio-based carbon with reduced coloration]
[0033] One embodiment of the present invention is a polytetramethylene ether glycol containing bio-based carbon with reduced coloration. More specifically, the polytetramethylene ether glycol is a copolymerization reaction product of tetrahydrofuran and 2-methyltetrahydrofuran derived from plants, and the polytetramethylene ether glycol has a Hazen unit color value (APHA color) of 60 or less, preferably 30 or less.
[0034] Here, the Hazen unit color value (APHA color) is a scale for evaluating the coloration of a chemical product that is liquid at room temperature or the coloration of a chemical product that is in a molten state after heating, and the color of a solution containing 1 mg of platinum in the form of hexachloroplatinum ions and 2 mg of cobalt (II) chloride hexahydrate in 1 liter is used as scale 1 (JIS K0071-1 Color test methods for chemical products-Part 1: Hazen unit color value (platinum-cobalt scale), refer to JIS K0071-1 Appendix A (Preparation of platinum-cobalt color standard solution)).
[0035] In addition, bio-based carbon refers to carbon derived from biomass raw materials, and in the present invention, it means that at least the raw material 2-methyltetrahydrofuran is derived from plants. As described in the following production method, plant-derived 2-methyltetrahydrofuran is produced using plant-derived raw materials as starting materials and using the furfural method or the levulinic acid method, but can be used without being limited to the production method.
[0036] As an indicator of the degree of plant origin, the bio-based carbon content (%) is known (ASTM D6866 standard). The bio-based carbon content (%) refers to the proportion (%) of the carbon mass of the components derived from biomass in the total carbon mass in the product. It also includes the carbon mass from natural polymers such as starch powder or plant fibers. The preferred bio-based carbon content of 2-methyltetrahydrofuran derived from plants is 97.00% to 100%, and more preferably 100%.
[0037] By using plant-derived 2-methyltetrahydrofuran purified by the purification method described in the production of polytetramethylene ether glycol described below as a raw material for the reduced-coloration bio-based carbon-containing polytetramethylene ether glycol of one embodiment of the present invention, a predetermined low Hazen unit color value (APHA color) can be achieved.
[0038] As for tetrahydrofuran as another raw material, specifically, there is no particular limitation, and examples thereof include petroleum-based, biological-based (from plants (from biomass)), by-product-based tetrahydrofuran, and the like. In the present invention, tetrahydrofuran from plants is preferred. In the case of manufacturing the tetrahydrofuran (THF) used from raw materials from plants (or from biomass), tetrahydrofuran manufactured by a known method such as the furfural method can be used. The purity of the tetrahydrofuran is preferably 99.00% to 100%, more preferably 99.50% to 100%, and further preferably 99.70% to 100%. In addition, the bio-based carbon content (%) of the tetrahydrofuran used is preferably 97.00% to 100%, more preferably 98.00% to 100%, and most preferably 100%.
[0039] Here, the purity used throughout this specification refers to the purity obtained by gas chromatography. More specifically, it is calculated based on the area % of the chromatogram.
[0040] The number average molecular weight of the bio-based carbon-containing polytetramethylene ether glycol with reduced coloration as one embodiment of the present invention is preferably 500 to 5000. When the number average molecular weight (Mn) of the polytetramethylene ether glycol is 500 or less, the polyurethane resin generated by polymerization using the polytetramethylene ether glycol becomes hard, and the rubber elastic modulus and tensile strength are reduced. When the number average molecular weight is 5000 or more, the stretchability of the polyurethane resin becomes too large, which impairs the properties as a resin. Therefore, the number average molecular weight (Mn) of the bio-based carbon-containing polytetramethylene ether glycol with reduced coloration as one embodiment of the present invention is preferably 500 to 5000, more preferably 1000 or more, more preferably 4500 or less, further preferably 1500 or more, and further preferably 4000 or less.
[0041] In addition, the description in the production method of polytetramethylene ether glycol described below can be cited.
[0042] [Method for producing polytetramethylene ether glycol]
[0043] Another aspect of the present invention is a method for producing the above-mentioned bio-based carbon-containing polytetramethylene ether glycol with reduced coloration.
[0044] The 2MeTHF used in the production method is usually produced by the furfural method or the levulinic acid method using raw materials from plants (in the present invention, products usually indicated as "derived from biomass" are also expressed as "derived from plants") as starting materials, but can be used without being limited to the production method. In order to maximize the purpose of the invention, 2MeTHF using raw materials from plants as starting materials is preferred. Furfural can be synthesized from biomass raw materials from plants such as polysaccharides, i.e., cellulose or hemicellulose, and lignin, which can be recovered from agricultural waste represented by corn cobs or sugarcane bagasse, and is a compound that can be synthesized by an environmentally friendly process.
[0045] In the present invention, "biobutanediol", "biotetrahydrofuran", "biopolyol", "biopolyether polyol" and the like refer to low-molecular or high-molecular compounds derived from plants that have the same physical properties as these petroleum-based compounds. In addition, "biopolyurethane material" refers to a polyurethane material in which components derived from plant compounds account for at least 50% by mass of the raw material.
[0046] The following is a detailed description of a method for producing a bio-based carbon-containing "polytetramethylene ether glycol" with reduced coloration as one embodiment of the present invention. The "polytetramethylene ether glycol" of the present invention is a copolymerization reaction product of the "tetrahydrofuran" and "2-methyltetrahydrofuran derived from plants", and includes the following "purification step" and "copolymerization step".
[0047] <Purification process>
[0048] The method for producing polytetramethylene ether glycol of the present invention comprises the step of purifying unpurified 2MeTHF by a purification step including a step of bringing the "plant-derived 2-methyltetrahydrofuran" (unpurified 2MeTHF) into contact with an acid. More specifically, after bringing the "plant-derived 2-methyltetrahydrofuran" (unpurified 2MeTHF) into contact with an acid, purification including distillation is performed to obtain purified 2MeTHF.
[0049] The purity can be increased to 99.90% or higher by this purification step. However, the purity of "plant-derived 2-methyltetrahydrofuran" (unpurified 2MeTHF) used in the purification step is preferably as high as possible, for example, unpurified 2MeTHF having a purity of 99.50% or higher.
[0050] The purification step of 2MeTHF carried out in the method for producing polytetramethylene ether glycol of the present invention preferably consists of the following steps.
[0051] Purification step (I): a step of contacting 2MeTHF containing 2-methylfuran with an inorganic acid (typically sulfuric acid, nitric acid, or hydrochloric acid) or a strongly acidic ion exchange resin.
[0052] Purification step (II): a step of separating and dehydrating 2MeTHF with an inorganic acid or a strongly acidic ion exchange resin.
[0053] Purification step (III): a step of extracting 2MeTHF by distillation.
[0054] Hereinafter, the details of each step will be described in sequence.
[0055] As the inorganic acid used in the step of contacting 2MeTHF with an inorganic acid or a strongly acidic ion exchange resin in the purification step (I), sulfuric acid, nitric acid, and hydrochloric acid can be used. The concentration of the inorganic acid used is not particularly limited, but in the case of sulfuric acid, it is preferably 10% to 80% by mass, in the case of nitric acid, it is preferably 5% to 45% by mass, in the case of hydrochloric acid, it is preferably 5% to 30% by mass, and more preferably 40% to 70% by mass of sulfuric acid. The amount of the inorganic acid contacted is preferably 5% to 100% by mass relative to 2MeTHF, and more preferably 5% to 30% by mass.
[0056] As the strongly acidic ion exchange resin in the purification step (I), specifically, aromatic sulfonic acid type cation exchange resin, benzyl sulfonic acid type cation exchange resin, etc. can be cited. As the parent resin of these exchange resins, styrene, methacrylic acid, phenolic resins, etc. can be cited. As specific products, DIAION SK series, DIAION PK series (all made by Mitsubishi Chemical Corporation) can be cited. The amount of the strongly acidic ion exchange resin contacted is preferably 5% to 100% by mass relative to 2MeTHF.
[0057] In the purification step (I), the temperature during contact with the acid can be arbitrarily selected within the range of 78°C (boiling point of 2MeTHF), which is the boiling point of 2MeTHF, for example, within the range of 20°C to 80°C. In order to improve the efficiency of the contact, it is preferably 30°C to 60°C. As a contact method, it can be any of intermittent and continuous. In the case of intermittent mixing and stirring for 0.1 hour to 10 hours, preferably 0.5 hour to 3 hours. In the case of continuous mixing, the operation is performed in a manner such that the contact time with the inorganic acid or the strongly acidic ion exchange resin reaches 0.1 hour to 10 hours, preferably 0.5 hour to 3 hours. The used inorganic acid or strongly acidic ion exchange resin can also be used when the purification step is repeated.
[0058] For the process of separating 2MeTHF from an inorganic acid or a strongly acidic ion exchange resin in the purification process (II), if it is an intermittent process, it is carried out by a liquid separation operation after stopping the mixing and stirring and letting it stand. If it is a strongly acidic ion exchange resin, it can also be separated by filtration. If it is a continuous process, it is immediately let stand and separate liquids after contacting with an inorganic acid or a strongly acidic ion exchange resin in a contact tower or a contact kettle, or it is carried out using a filtering device. The temperature during liquid separation is not particularly limited. By carrying out the process at the same temperature as the contact temperature with the inorganic acid or the strongly acidic ion exchange resin, the process can be simplified. The time required for standing and liquid separation varies depending on the type and concentration of the inorganic acid used. In order to avoid process losses, it is ideal to set the standing time to be longer than the time for identifying the interface between the 2MeTHF layer and the inorganic acid layer. After separating the inorganic acid, the following operation can also be performed: relative to 2MeTHF, 10% to 100% by mass of water is added, mixed and stirred, and allowed to stand and separate liquids, thereby further removing the inorganic acid layer remaining in the 2MeTHF layer.
[0059] The dehydration process of purification step (II) can be carried out by using an alkali metal hydroxide or an alkaline earth metal hydroxide. Add an alkali metal hydroxide or an alkaline earth metal hydroxide to the 2MeTHF layer after separating the inorganic acid layer, and separate the liquid to remove the free water layer. As a specific example of the alkali metal hydroxide, the hydroxides of sodium, potassium, lithium, cesium, etc. can be listed, preferably sodium hydroxide. As a specific example of the alkaline earth metal hydroxide, the hydroxides of beryllium, magnesium, calcium, barium, etc. can be listed. It should be noted that if the mixing of water is less due to the use of a strongly acidic ion exchange resin, dehydration is not required, and dehydration can also be omitted. The dehydration equipment can be any of intermittent and continuous.
[0060] In the purification step (III), 2MeTHF is extracted by distillation. The distillation method may be either intermittent or continuous. The distillation is performed using a distillation tower having a theoretical plate number of 1 or more and 50 or less. In order to improve the purification efficiency of the distilled mixture, the theoretical plate number of the distillation tower is preferably set to 5 or more, preferably 10 or more. In order not to consume too much energy required for distillation, it is preferably 50 or less.
[0061] The lower limit of the reflux ratio of the distillation column is 0.01 or more, preferably 0.1 or more, and the upper limit is 10 or less, preferably 5 or less. If the lower limit is too small, the distillate mixture may not be separated sufficiently, and if the upper limit is too large, the energy required for distillation becomes huge, and the economic efficiency decreases.
[0062] Regarding the pressure during the distillation of 2MeTHF, it can be carried out under reduced pressure from atmospheric pressure. The degree of reduced pressure when carried out under reduced pressure can be set arbitrarily between 1 kPa and 101 kPa. If the degree of reduced pressure is reduced, the energy required for evaporation is reduced, but the energy used to reduce the temperature of the cooling medium used in the condenser for condensing the vapor increases, so it is preferred to set the degree of reduced pressure with good energy efficiency in view of the equipment used. Regarding the distillation temperature, it is determined based on the evaporation temperature of 2MeTHF, and the evaporation temperature of 2MeTHF is determined by the setting of the pressure.
[0063] When distillation is performed intermittently and at normal pressure, an azeotropic composition of THF and water and a low-boiling fraction having a boiling point lower than 2MeTHF will be distilled at the initial stage of distillation. Therefore, 0% to 10% by mass of the liquid treated in the purification step (II) of the distillation is removed in the form of initial distillation. Next, the purified 2MeTHF is distilled. The ratio of the extracted purified 2MeTHF is 80% to 95% by mass of the liquid treated in the purification step (II) of the distillation. Finally, 0% to 10% by mass of the liquid treated in the purification step (II) of the distillation containing a large amount of high-boiling components remains in the distiller. Each of the above steps (I) to (III) can also be operated in a continuous manner.
[0064] The 2MeTHF remaining in the inorganic acid water discharged in the purification step (II) or the primary fraction separated in the purification step (III) can be recovered in another distillation operation. The purification method of the present invention can also be applied to the recovered 2MeTHF.
[0065] The highly purified 2MeTHF obtained by the purification steps (I) to (III) is suitable for use as a raw material for producing the polytetramethylene ether glycol of the present invention, in particular, as a raw material for producing "polytetramethylene ether glycol having a Hasson unit color value (APHA color) of 60 or less" (polymerization reaction). In addition, as a raw material for producing polytetramethylene ether glycol (polymerization reaction), THF and / or 3-methyltetrahydrofuran may be mixed in the 2MeTHF for use (copolymerization reaction step). Therefore, the "method for producing polytetramethylene ether glycol" of the present invention includes a "method for producing polytetramethylene ether glycol" using the above-mentioned purified 2-methyltetrahydrofuran (purified 2MeTHF) and adopting the following "copolymerization reaction step".
[0066] <Copolymerization reaction step>
[0067] In the production method of the present invention, specifically, in the copolymerization reaction step of tetrahydrofuran (THF) and 2-methyltetrahydrofuran (2MeTHF) derived from plants, the ratio (mass ratio) of THF to 2MeTHF can be arbitrarily selected in consideration of the required performance or cost (specifically, the cost of the copolymerization reaction step, the reaction time, the yield, the output, the physical property values of the obtained copolymerization reaction product or polytetramethylene ether glycol, the physical property values of the polyurethane resin obtained using the polytetramethylene ether glycol, etc.). However, if the ratio of 2MeTHF is extremely low, the expected performance cannot be exerted, and on the contrary, if the ratio is too high, it is disadvantageous in terms of cost due to the decrease in reactivity. Therefore, the ratio (mass ratio) of THF to 2MeTHF is preferably 99:1 to 50:50, more preferably 97:3 to 55:45, and particularly preferably 93:7 to 60:40.
[0068] In the manufacture method of the present invention, the copolymerization reaction of THF and 2MeTHF is preferably carried out by adding 5% to 40% by mass of a strong acid catalyst relative to the total mass of THF and 2MeTHF. From the viewpoint of good reaction conversion rate and good yield, the lower limit of the addition amount of the strong acid catalyst is preferably 5% by mass, more preferably 8% by mass, and particularly preferably 15% by mass. From the viewpoint of avoiding the molecular weight reduction when the reactive species become more and cause the reaction equilibrium, the upper limit of the addition amount of the strong acid catalyst is preferably 40% by mass, more preferably 36% by mass.
[0069] In the production method of the present invention, the copolymerization reaction of THF and 2MeTHF is carried out by mixing THF and 2MeTHF in the preferred mass ratio described above and adding a strong acid catalyst while maintaining the temperature at 0°C to 50°C.
[0070] In the production method of the present invention, as the catalyst used in the copolymerization reaction of THF and 2MeTHF, specifically, acetic anhydride, perchloric acid, fluorosulfonic acid, fuming sulfuric acid can be cited. Strong acid catalysts can be used alone or in combination with multiple strong acids. When using multiple strong acids, the temperature range of 0°C to 50°C can be divided into several stages and used separately.
[0071] The polytetramethylene ether glycol can be obtained by hydrolyzing the reaction liquid of the polymerization reaction. The hydrolysis is preferably carried out by adding 10% to 100% by mass of water relative to the mass of the reaction liquid and at a temperature of 30° C. to 120° C. The water layer is separated from the reaction liquid after the hydrolysis is completed, and unreacted raw materials and the like are separated to obtain the polytetramethylene ether glycol.
[0072] The polytetramethylene ether glycol obtained by the copolymerization reaction step of THF and 2MeTHF in the production method of the present invention preferably has a number average molecular weight (Mn) of 500 to 5,000 as described in the section of the bio-based carbon-containing polytetramethylene ether glycol with reduced coloration.
[0073] The polytetramethylene ether glycol of the present invention, that is, the polytetramethylene ether glycol obtained by the production method of the present invention, can be used to produce a polyurethane material containing a polyisocyanate or a chain extender as a main raw material.
[0074] In the chemical reaction of the manufacturing process of the polyurethane material, as the polyisocyanate compound, a polyisocyanate compound having two or more isocyanate groups in the molecule can be used. For example, polyisocyanates such as toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), xylylene diisocyanate (XDI), isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HDI), naphthalene diisocyanate (NDI), and hydrogenated diphenylmethane diisocyanate can be cited, and they can be used alone or in combination of two or more.
[0075] In the chemical reaction of the manufacturing process of the polyurethane material, as a chain extender, a chain extender having two or more hydroxyl groups or amino groups is preferably used, for example, ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, glycerol, trimethylolpropane, ethylenediamine, propylenediamine, phenylenediamine, diaminodiphenylmethane, etc., which can be used alone or in combination of two or more.
[0076] In the chemical reaction of the manufacturing process of the polyurethane material, the raw materials from biomass are combined, specifically, the 2MeTHF from plants, THF (biotetrahydrofuran) from plants or butanediol (biobutanediol) from plants of the present invention are combined and used as starting materials, thereby being able to manufacture polyurethane (biopolyurethane) resin materials from plants. For biopolyurethane materials, the content of components from biomass is 50% to 80% by mass relative to 100% by weight of the polyurethane material. Generally, the higher the content of components from plants (from biomass) in the resin, the more environmentally friendly it is, but in order to achieve more than 80% by mass of biopolyurethane materials, in addition to 2MeTHF, it is also necessary to make the raw materials of polyisocyanate compounds, chain extenders, etc. also come from plants, and there are many problems in terms of technology and economy.
[0077] Furthermore, the item of reduced coloration bio-based carbon-containing polytetramethylene ether glycol may be cited.
[0078] Example
[0079] Hereinafter, the present invention will be described in detail by way of examples, but the present invention is not limited to the following examples and can be implemented in various ways within the scope of the gist of the present invention. In the purification examples and synthesis examples, unless otherwise specified, reagents manufactured by Kishida Chemical Co., Ltd., Organic Co., Ltd., Tokyo Chemical Industry Co., Ltd., Fujifilm Wako Pure Chemical Industries, Ltd., and other well-known chemical manufacturing or sales companies are used.
[0080] The analysis equipment and sample analysis methods used in the examples are as follows.
[0081] [Analysis of 2MeTHF]
[0082] Gas chromatography (GC):
[0083] Device name: Gas chromatograph manufactured by Shimadzu Corporation, model: GC-2014
[0084] Analytical column: DB-1 manufactured by T&D Co., Ltd. (inner diameter 0.25 mm × 30 m, film thickness 0.25 μm)
[0085] Column temperature: 40℃ (6.5 minutes) → (20℃ / min.) → 200℃ (15 minutes)
[0086] Flow rate: He, 0.7mL / min.
[0087] Injection volume: 0.1μL
[0088] Inj temperature: 200℃
[0089] Detector: FID
[0090] Det temperature: 200℃
[0091] Range: 10 1
[0092] [Coloring judgment]
[0093] The degree of coloration was determined by colorimetric comparison of the Hazen unit color value (APHA color) using the test method described in Japanese Industrial Standard JIS K0071-1:2007.
[0094] [Determination of number average molecular weight (Mn) of polytetramethylene ether glycol]
[0095] The hydroxyl value of polytetramethylene ether glycol was measured by the test method described in Japanese Industrial Standard JIS K1557-1:2007, and Mn was calculated.
[0096] [Purification Example 1, Unpurified Example 1 and Unpurified Example 2] Purification of 2MeTHF 1
[0097] 1000 g of unpurified 2MeTHF (unpurified example 1) (manufactured by Tokyo Chemical Industry Co., Ltd.) and 100 g of 60% sulfuric acid (manufactured by Kishida Chemical Co., Ltd.) were added to a 3 L reaction container and stirred at 60°C for 1 hour. After standing for 30 minutes, liquid separation was performed to obtain 700 g of an oil layer. 300 g of water was added to the oil layer, and liquid separation was performed to obtain 650 g of a washed oil layer.
[0098] 400 g of the 60% sulfuric acid aqueous layer obtained after separation and 350 g of the washed aqueous layer were added to a 2 L container, and the mixture was heated to 90° C. and simple distillation was performed to recover 250 g of 2MeTHF.
[0099] The above-mentioned cleaned oil layer 650g and the above-mentioned recovered 2MeTHF 250g were mixed, and 50g of sodium hydroxide (manufactured by Kishida Chemical Co., Ltd.) was added and stirred for 30 minutes. By decantation, 800g of crude 2MeTHF (unpurified example 2) was obtained. The purity (%) (hereinafter referred to as GC purity) of the unpurified 2MeTHF (unpurified example 1) and the obtained crude 2MeTHF (unpurified example 2) measured by gas chromatography is shown in Table 1.
[0100] 800 g of the crude 2MeTHF obtained above was added to a 1L container and heated to 80°C. Distillation was performed using a distillation tower with a theoretical plate number of 10. 40 g of the initial fraction was distilled out at a reflux ratio of 1 and removed. 700 g of purified 2MeTHF (yield 70% relative to unpurified 2MeTHF) was obtained at a reflux ratio of 0.1. The purity (%) (GC purity) of the obtained purified 2MeTHF (Purification Example 1) is shown in Table 1.
[0101] It was confirmed that the bio-based carbon content (%) of 2MeTHF used in Purification Example 1 was 100%.
[0102] (Measurement method: ASTM D6866-22 Method B, Geoscience Laboratory Co., Ltd.)
[0103] [Purification Example 2] Purification of 2MeTHF
[0104] 720 g of purified 2MeTHF (yield 72% relative to unpurified 2MeTHF) was obtained in the same manner as in Purification Example 1 except that the initial fraction 40 g of Purification Example 1 was changed to 20 g. The GC purity of the obtained purified 2MeTHF (Purification Example 2) is shown in Table 1.
[0105] [Purification Example 3] Purification of 2MeTHF
[0106] 720 g of purified 2MeTHF (yield 65% relative to unpurified 2MeTHF) was obtained in the same manner as in Purification Example 1 except that the sulfuric acid concentration in Purification Example 1 was 25%. The GC purity of the obtained purified 2MeTHF (Purification Example 3) is shown in Table 1.
[0107]
Table 1
[0108] 2MeTHF GC purity (%) Unpurified Example 1 Unpurified 2MeTHF 99.87 Unpurified Example 2 Crude 2MeTHF 99.88 Purification Example 1 Purification of 2MeTHF 99.95 Purification Example 2 Purification of 2MeTHF 99.90 Purification Example 3 Purification of 2MeTHF 99.90
[0109] [Example 1] Synthesis of THF-2MeTHF copolymerization product 1
[0110] To a 1L reaction vessel, add 255g of THF (manufactured by Kishida Chemical Co., Ltd.) and 45g of purified 2MeTHF obtained in Purification Example 1, and cool at 0°C. Add 2g of 70% perchloric acid (manufactured by Kishida Chemical Co., Ltd.) to the reaction vessel. Then, add 58g of 25% fuming sulfuric acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) dropwise at -5°C to 5°C for 5 hours. After stirring the reaction solution at -5°C to 5°C for 2 hours, add 160g of water, heat to 70°C, and reflux for 3 hours. After reflux, let stand at 65°C to 70°C for 1 hour, and remove the water layer. Add 100g of water and 100g of THF to the oil layer, heat to 70°C, and reflux for 3 hours. After reflux, let stand at 65°C to 70°C for 1 hour, and remove the water layer. Add 200 mL of ion exchange resin IRA-96S (produced by Organic Co., Ltd.) to the oil layer and stir at room temperature (around 20°C to 25°C) for 1 hour. After filtering and removing the ion exchange resin, concentrate under reduced pressure at 120°C to obtain THF-2MeTHF copolymerization reaction product (125 g, yield 42%). The above synthesis results (mass, mass ratio and yield of each raw material, etc.) and the analysis results of the obtained THF-2MeTHF copolymerization reaction product (number average molecular weight (Mn) and Hazen unit color value (APHA color)) are shown in Table 2.
[0111] [Example 2] Synthesis of THF-2MeTHF Copolymer 2
[0112] To a 1L reaction vessel, add 360g of THF (manufactured by Kishida Chemical Co., Ltd.) and 240g of purified 2MeTHF obtained in Purification Example 2, and cool at 0°C. Add 8g of 70% perchloric acid (manufactured by Kishida Chemical Co., Ltd.) to the reaction vessel. Then, add 205g of 25% fuming sulfuric acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) dropwise at -5°C to 5°C for 5 hours. After stirring the reaction solution at -5°C to 5°C for 5 hours, add 100g of water, heat to 70°C, and reflux for 3 hours. After reflux, let stand at 65°C to 70°C for 1 hour, and remove the water layer. Add 100g of water and 100g of THF to the oil layer, heat to 70°C, and reflux for 3 hours. After reflux, let stand at 65°C to 70°C for 1 hour, and remove the water layer. 200 mL of ion exchange resin IRA-96S (manufactured by Organic Co., Ltd.) was added to the oil layer and stirred at room temperature (near 20°C to 25°C) for 1 hour. After filtering and removing the ion exchange resin, the mixture was concentrated under reduced pressure at 120°C to obtain a THF-2MeTHF copolymerization product (200 g, yield 30%). As in Example 1, the above synthesis results and the analysis results of the obtained THF-2MeTHF copolymerization product are shown in Table 2.
[0113] [Examples 4, 5, 7, 9 to 13] Synthesis of THF-2MeTHF Copolymers 4, 5, 7, 9 to 13
[0114] A THF-2MeTHF copolymer was obtained by the same synthesis as in Example 1 except that the amounts of THF, 2MeTHF, 70% perchloric acid and fuming sulfuric acid were changed to the values shown in Table 2. The results are shown in Table 2 together with those in Example 1.
[0115] [Examples 3, 6 and 8] Synthesis of THF-2MeTHF Copolymers 3, 6 and 8
[0116] Except that the purified 2MeTHF obtained in Purification Example 3 was used in Example 1 instead of the non-purified Example 1, and the amounts of THF, 2MeTHF, 70% perchloric acid and fuming sulfuric acid were changed to the values shown in Table 2, the synthesis was carried out in the same manner as in Example 1 to obtain a THF-2MeTHF copolymer. The results are also shown in Table 2 as in Example 1.
[0117] [Comparative Example 1] Synthesis of THF-2MeTHF Copolymer 14
[0118] Add 360 g of THF and 240 g of unpurified 2MeTHF of unpurified example 1 to a reaction container with a volume of 1 L, and cool at 0°C. Add 8 g of 70% perchloric acid to the reaction container. Then, add 205 g of 25% fuming sulfuric acid dropwise at -5°C to 5°C for 5 hours. After stirring the reaction solution at -5°C to 5°C for 5 hours, add 100 g of water, heat to 70°C, and reflux for 3 hours. After reflux, let stand at 65°C to 70°C for 1 hour, and remove the water layer. Add 100 g of water and 100 g of THF to the oil layer, heat to 70°C, and reflux for 3 hours. After reflux, let stand at 65°C to 70°C for 1 hour, and remove the water layer. Add 200 mL of ion exchange resin IRA-96S to the oil layer, and stir at room temperature (near 20°C to 25°C) for 1 hour. After the ion exchange resin was removed by filtration, the mixture was concentrated under reduced pressure at 120°C to obtain a THF-2MeTHF copolymer (200 g, yield 30%). As in Example 1, the above synthesis results and the analysis results of the obtained THF-2MeTHF copolymer are shown in Table 2.
[0119] [Comparative Example 2] Synthesis of THF-2MeTHF Copolymer 15
[0120] Add 360g of THF and 240g of crude 2MeTHF of unpurified Example 2 to a reaction container with a volume of 1L, and cool to 0°C. Add 8g of 70% perchloric acid to the reaction container. Then, add 205g of 25% fuming sulfuric acid dropwise at -5°C to 5°C for 5 hours. After stirring the reaction solution at -5°C to 5°C for 5 hours, add 100g of water, heat to 70°C, and reflux for 3 hours. After reflux, let stand at 65°C to 70°C for 1 hour, and remove the water layer. Add 100g of water and 100g of THF to the oil layer, heat to 70°C, and reflux for 3 hours. After reflux, let stand at 65°C to 70°C for 1 hour, and remove the water layer. Add 200mL of ion exchange resin IRA-96S to the oil layer, and stir at room temperature (near 20°C to 25°C) for 1 hour. After the ion exchange resin was removed by filtration, the mixture was concentrated under reduced pressure at 120°C to obtain a THF-2MeTHF copolymer (200 g, yield 30%). As in Example 1, the above synthesis results and the analysis results of the obtained THF-2MeTHF copolymer are shown in Table 2.
[0121] [Comparative Example 3] Synthesis of THF-2MeTHF Copolymer 16
[0122] The unpurified 2MeTHF (unpurified example 1) was distilled using a distillation column with a theoretical plate number of 10 plates, omitting the acid washing with 60% sulfuric acid and the dehydration step with sodium hydroxide in purification example 1. The 2MeTHF was used and the amounts of THF, 2MeTHF, 70% perchloric acid and fuming sulfuric acid were changed to the values shown in Table 2. The synthesis was performed in the same manner as in Example 1 to obtain a THF-2MeTHF copolymer. The results are also shown in Table 2 as in Example 1.
[0123]
Table 2
[0124]
[0125] As can be seen from Table 2, the copolymerization product of THF and the purified 2MeTHF of the present invention, namely polytetramethylene ether glycol, has a smaller Hazen unit color value (APHA color) and is less colored than the polytetramethylene ether glycol synthesized using unpurified 2MeTHF in the comparative example.
[0126] The method for producing polytetramethylene ether glycol of the present invention can produce non-colored polytetramethylene ether glycol. The polytetramethylene ether glycol obtained by the method for producing polytetramethylene ether glycol of the present invention is plant-derived, has little coloration, and is high-quality polytetramethylene ether glycol, and is excellent as a bio-polyurethane material for a recycling-oriented society.
Claims
1. A polytetramethylene ether glycol, wherein The polytetramethylene ether glycol is a copolymerization reaction product of tetrahydrofuran and 2-methyltetrahydrofuran derived from plants, and the Hazen unit color value (APHA color) of the polytetramethylene ether glycol is 60 or less.
2. The polytetramethylene ether glycol according to claim 1, wherein The Hazen unit color value (APHA color) is 30 or less.
3. The polytetramethylene ether glycol according to claim 1, wherein The bio-based carbon content (%) of the plant-derived 2-methyltetrahydrofuran was 100%.
4. The polytetramethylene ether glycol according to claim 1, wherein The tetrahydrofuran is derived from plants, and the bio-based carbon content (%) of the tetrahydrofuran is 97.00% to 100%.
5. The polytetramethylene ether glycol according to claim 1, wherein The number average molecular weight of the polytetramethylene ether glycol is 500-5000.
6. A method for producing polytetramethylene ether glycol, wherein: include: a step of obtaining purified plant-derived 2-methyltetrahydrofuran through a purification step including a step of contacting plant-derived 2-methyltetrahydrofuran with an acid; and A step of copolymerizing the purified plant-derived 2-methyltetrahydrofuran with tetrahydrofuran.
7. The method for producing polytetramethylene ether glycol according to claim 6, wherein The purity of the purified plant-derived 2-methyltetrahydrofuran is 99.90% or more.
8. The method for producing polytetramethylene ether glycol according to claim 6, wherein The acid used in the purification process is an inorganic acid or a strong acid ion exchange resin.
9. The method for producing polytetramethylene ether glycol according to claim 8, wherein In the purification step, plant-derived 2-methyltetrahydrofuran is brought into contact with an acid at a temperature ranging from 20°C to 80°C.
10. The method for producing polytetramethylene ether glycol according to claim 8, wherein In the purification step, plant-derived 2-methyltetrahydrofuran is brought into contact with an acid at a temperature ranging from 30°C to 60°C.
11. The method for producing polytetramethylene ether glycol according to claim 8, wherein The purification process comprises: A process of contacting plant-derived 2-methyltetrahydrofuran with an inorganic acid or a strongly acidic ion exchange resin; The process of separating and dehydrating 2-methyltetrahydrofuran with an inorganic acid or a strong acid ion exchange resin; and A step of extracting the purified 2-methyltetrahydrofuran by distillation.
12. The method for producing polytetramethylene ether glycol according to claim 6, wherein: The purity of the tetrahydrofuran is above 99.50%.
13. The method for producing polytetramethylene ether glycol according to claim 6, wherein: In the copolymerization step, the ratio (mass ratio) of tetrahydrofuran to plant-derived 2-methyltetrahydrofuran is 99:1 to 50:
50.
14. The method for producing polytetramethylene ether glycol according to claim 6, wherein: In the copolymerization step, 5% to 40% by mass of a strong acid catalyst is added based on the total mass of tetrahydrofuran and 2-methyltetrahydrofuran.
15. The method for producing polytetramethylene ether glycol according to claim 6, wherein: In the copolymerization step, 8% to 40% by mass of a strong acid catalyst is added based on the total mass of tetrahydrofuran and 2-methyltetrahydrofuran.