Preparation method of composite hydrogel for promoting cartilage tissue repair

By combining aminated chitosan with sodium hyaluronate and polyvinyl alcohol, and adding graphene oxide, a composite hydrogel with excellent mechanical strength and biocompatibility was prepared, solving the problems of mechanical properties and biocompatibility of traditional scaffolds. The contradiction between compatibility significantly improves the effect of cartilage repair.

CN118743785APending Publication Date: 2024-10-08KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411001125.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Traditional tissue engineering scaffolds cannot meet the requirements of mechanical strength and biocompatibility at the same time, limiting the effect of cartilage repair.

Method used

Aminated chitosan and sodium hyaluronate are combined with polyvinyl alcohol, and through cyclic freeze-thaw treatment, graphene oxide is added to prepare a composite hydrogel with excellent mechanical strength, swelling performance and good biodegradability.

Benefits of technology

It improves the mechanical strength and cell adhesion ability of the composite hydrogel, enhances its application potential in cartilage repair, and resolves the contradiction between mechanical properties and biocompatibility of traditional scaffolds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004961595400000081
    Figure BDA0004961595400000081
  • Figure HDA0004961595590000011
    Figure HDA0004961595590000011
  • Figure HDA0004961595590000012
    Figure HDA0004961595590000012
Patent Text Reader

Abstract

The invention discloses a preparation method of composite hydrogel for promoting cartilage tissue repair, which comprises the following steps: respectively dissolving aminated chitosan and sodium hyaluronate in ultrapure water, mixing, filtering out precipitate, freeze-drying, and adding a calcium chloride solution to obtain ACS / SH hydrogel; dissolving polyvinyl alcohol in ultrapure water to obtain a polyvinyl alcohol solution, adding the ACS / SH hydrogel, and uniformly stirring to obtain (ACS / SH) / PVA hydrogel; adding graphene oxide into the (ACS / SH) / PVA hydrogel, and carrying out circulating freeze thawing treatment to obtain (ACS / SH) / PVA / GO composite hydrogel; the composite hydrogel has excellent mechanical strength and swelling property, good biodegradability and hydrophilic resilience, solves the problem that a traditional stent cannot meet mechanical strength and biocompatibility at the same time, can well promote cartilage repair, and has excellent popularization and application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a composite hydrogel for promoting cartilage tissue repair, and belongs to the technical field of hydrogel bioengineering scaffolds. Background Art

[0002] Bone defects caused by trauma, inflammation, tumors, degenerative diseases, etc. are seriously affecting people's health. With the increasing aging of the population, the scope of influence is becoming wider and wider, and it has caused an increasingly heavy medical burden on the public health system. As the main load-bearing tissue of the body, bones have the ability to self-renew. Under normal physiological conditions, they are constantly undergoing reconstruction and remodeling to adapt to the body's load and maintain the mechanical strength of bones. Cartilage is another important component of the human skeletal system. It is a kind of strong and elastic supportive connective tissue that covers the surface of bones in the joint area, provides a smooth and lubricated contact surface for the joint, effectively reduces the friction of synovial joints, and promotes load conduction; it can withstand and conduct high-pressure loads, playing a role in stress buffering. Cartilage is composed of rich cartilage ECM and relatively few chondrocytes. Cartilage ECM plays a role in supporting the growth of chondrocytes, maintaining cartilage structure, bearing and transmitting various mechanical forces, and lubricating joints. Chondrocytes reshape the matrix biochemical components by producing and maintaining cartilage ECM and responding to changes in environmental signals to regulate cartilage homeostasis. Common treatments for cartilage defects include autologous cartilage or chondrocyte transplantation, allogeneic transplantation, and microfracture. These methods also have shortcomings such as insufficient donor sources and greater surgical damage.

[0003] Tissue engineering scaffolds synthesized from polymer materials can have good biocompatibility, biodegradability and matching physical properties by adjusting the structure and physicochemical properties. As ECM scaffold materials, they deliver cells and bioactive factors to the defect area, support the growth of host cells, and promote the formation of new bone and cartilage. Hydrogels are highly water-containing three-dimensional network scaffolds formed by cross-linking hydrophilic polymers or macromolecular monomers. Due to their structure and physicochemical properties similar to those of ECM, they are often designed as bionic ECM scaffold materials for tissue repair and regeneration research. Hydrogels have high biocompatibility and can not only deliver cells, provide cells with a growth environment similar to that of ECM, promote cell migration, adhesion, proliferation and differentiation, but also load and deliver growth factors.

[0004] Sodium hyaluronate (SH, also known as hyaluronic acid) is a linear macromolecular acidic mucopolysaccharide that exists in the connective tissue of most mammals and humans. It has good biocompatibility, degradability, moisturizing and lubricity, but hyaluronic acid has poor mechanical strength, rapid degradation in the body and poor adhesion to cells, which greatly limits its use in biomaterials. Therefore, it is often chemically modified or compounded with other natural polymer materials to make hydrogels. Chitosan (CS) is the product of chitin deacetylation, mainly derived from the shells and bones of crustacean insects, and is currently the only natural alkaline polysaccharide. Chitosan has good biocompatibility, degradability and multiple biological activities, including antibacterial and antioxidant properties. At the same time, chitosan molecules contain a large number of amino and hydroxyl groups, which make it useful for surface modification and chemical modification. Polyvinyl alcohol (PVA) is a hydrophilic polymer material with good biocompatibility, non-toxicity, and good chemical stability. It can form hydrogels through chemical or physical cross-linking. Traditional PVA hydrogels have poor mechanical strength. Excessive external force applied to them will cause permanent damage to their cross-linked structure, and their performance is usually difficult to meet actual needs. However, they can be made multifunctional through the modification of various composite products. Graphene oxide (GO) is a derivative of graphene that contains a large number of oxygen-containing organic functional groups. Because GO has a 2D nanostructure, rich oxygen-containing functional groups, high specific surface area and good mechanical properties, it has application value in energy, electronics, biomedicine and other fields. GO is often used as a nanofiller in hydrogels to enhance the performance of hydrogels and expand the application of hydrogels. The oxygen-containing functional groups in GO are negatively charged and can exhibit strong sol and gel properties through interactions such as π-π conjugation, covalent bonds, hydrogen bonds and electrostatic forces. Summary of the invention

[0005] The present invention provides a method for preparing a composite hydrogel for promoting cartilage tissue repair. The obtained composite hydrogel has excellent mechanical strength, swelling performance, good biodegradability, hydrophilicity and resilience, solves the problem that traditional scaffolds cannot simultaneously meet the requirements of mechanical strength and biocompatibility, can better promote cartilage repair, and has excellent prospects for promotion and application.

[0006] In order to achieve the above object, the technical solution of the present invention is as follows:

[0007] A method for preparing a composite hydrogel for promoting cartilage tissue repair, the specific steps are as follows:

[0008] (1) aminated chitosan (ACS) and sodium hyaluronate (SH) are dissolved in ultrapure water respectively, mixed, filtered to remove the precipitate, freeze-dried, and then added with calcium chloride solution (CaCl2) to obtain ACS / SH hydrogel;

[0009] (2) dissolving polyvinyl alcohol (PVA) in ultrapure water to obtain a polyvinyl alcohol (PVA) solution, adding the ACS / SH hydrogel obtained in step (1), and stirring evenly to obtain a (ACS / SH) / PVA hydrogel;

[0010] (3) (ACS / SH) / PVA hydrogel was subjected to cyclic freeze-thaw treatment to obtain composite hydrogel.

[0011] The aminated chitosan in step (1) is prepared by aminating chitosan with 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride (EDC), and the specific steps are as follows:

[0012] Dissolve 8-12 g chitosan in 300-500 mL phosphate solution, stir magnetically at 20-30 °C, add 28-36 mL ethylenediamine (ED) solution after complete dissolution, stir for 1-2 h, adjust the pH value to weak acidity (4-6) with concentrated hydrochloric acid, add 3.6-5.6 g 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride (EDC) at 25-35 °C, stir for 1-3 h, and place in a constant temperature box at 30-45 °C. The reaction is carried out for 4 to 8 hours, and the mixture is taken out and dialyzed in a dialysis bag for 2 to 6 days. The precipitate in the bag is placed in a freeze dryer and dried for 24 hours, and then taken out and ground to obtain aminated chitosan powder. The chitosan has a deacetylation degree of ≥95% and a viscosity of 100 to 200 mPa·s. The phosphate solution is a 0.2 mol / L sodium dihydrogen phosphate solution. The concentrated hydrochloric acid is commercially available concentrated hydrochloric acid with a concentration of 38%. The concentration of ethylenediamine is analytical grade, and the specification of the dialysis bag is 8000 to 14000 MW.

[0013] The mass ratio of the aminated chitosan to sodium hyaluronate in step (1) is 1-2:1; the molecular weight of sodium hyaluronate is 1000K; the mass volume ratio of the total mass of the aminated chitosan and sodium hyaluronate to the mass volume ratio of the calcium chloride solution is 1:5-7.

[0014] The mass concentration of the polyvinyl alcohol (PVA) solution in step (2) is 10% to 20%, and the mass ratio of ACS / SH hydrogel to polyvinyl alcohol (PVA) is 0.5 to 3:1.

[0015] Step (3) is replaced by: adding graphene oxide to the hydrogel obtained in step (2), and subjecting the resultant to cyclic freeze-thaw treatment to obtain a composite hydrogel; the amount of graphene oxide added is 0.1% to 0.9% of the mass of the (ACS / SH) / PVA hydrogel.

[0016] The specific method of the freeze-thaw cycle treatment in step (3) is as follows: freezing at -40°C for 2 to 8 hours, thawing at 25°C for 2 to 4 hours, and freezing and thawing again for 2 to 6 cycles.

[0017] The present invention also uses the composite hydrogel for promoting cartilage repair prepared by the method to make a cylindrical scaffold through a mold, and tests its mechanical properties, swelling properties, hydrophilicity, etc.

[0018] The aminated chitosan of the present invention not only retains the original properties of chitosan, but also increases the number of amino groups on the chitosan molecular chain, thereby strengthening the electrostatic interaction between the chitosan and the carboxyl groups on the sodium hyaluronate molecular chain, and also strengthening the metal ion chelation between the chitosan and the calcium ions in calcium chloride, thereby enhancing the mechanical strength of the hydrogel.

[0019] The invention adds polyvinyl alcohol, which not only utilizes the hydrophilicity of polyvinyl alcohol to enhance the cell adhesion of the composite hydrogel, but also crystallizes the macromolecular chains of polyvinyl alcohol to obtain a shaped hydrogel through freeze-thaw cycles, thereby further enhancing the mechanical properties of the composite hydrogel.

[0020] The composite hydrogel prepared by the invention has complete appearance, high mechanical strength, high porosity, good resilience, good hydrophilicity and swelling properties, and is suitable for use as a tissue engineering scaffold in cartilage repair. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a photo of the ACS / SH / PVA / GO composite hydrogel prepared in Example 9;

[0022] Figure 2 SEM images of ACS / SH / PVA hydrogel and ACS / SH / PVA / GO hydrogel;

[0023] Figure 3 The mechanical properties of ACS / SH / PVA hydrogel and ACS / SH / PVA / GO composite hydrogel;

[0024] Figure 4 Swelling curves of ACS / SH / PVA hydrogel and ACS / SH / PVA / GO composite hydrogel;

[0025] Figure 5 To test the hydrophilicity of ACS / SH / PVA hydrogel and ACS / SH / PVA / GO composite hydrogel;

[0026] Figure 6 This is the resilience test of ACS / SH / PVA / GO composite hydrogel. DETAILED DESCRIPTION

[0027] The present invention is further described in detail below in conjunction with the examples, but the embodiments and protection of the present invention are not limited thereto. It should be noted that if there are any details not particularly described in the examples, they can be realized or understood by those skilled in the art with reference to the prior art. The molecular weight of the sodium hyaluronate used in the examples is 1000K.

[0028] Example 1

[0029] The preparation of aminated chitosan, the specific steps are as follows:

[0030] 8g of chitosan was dissolved in 300mL of 0.2mol / L sodium dihydrogen phosphate solution, and magnetically stirred at 20°C. After complete dissolution, 28mL of ethylenediamine (ED) was added, and stirred for 1h. The pH value was adjusted to 4 with concentrated hydrochloric acid. At 25°C, 3.6g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride (EDC) was added, and stirred for 1h. The mixture was reacted in a 30°C thermostat for 4h. After being taken out, the mixture was dialyzed in a dialysis bag for 2 days. The precipitate in the bag was placed in a freeze dryer and dried for 24h. The mixture was taken out and ground to obtain aminated chitosan powder. The deacetylation degree of chitosan was ≥95%, and the viscosity was 100-200mPa·s. The concentrated hydrochloric acid was commercially available with a concentration of 38%. The ethylenediamine was analytical grade, and the specification of the dialysis bag was 8000-14000MW.

[0031] Example 2

[0032] The preparation of aminated chitosan, the specific steps are as follows:

[0033] Dissolve 10g chitosan in 400mL of 0.2mol / L sodium dihydrogen phosphate solution, stir magnetically at 25°C, add 32mL of ethylenediamine (ED) after complete dissolution, stir for 1.5h, adjust pH value to 5 with concentrated hydrochloric acid, add 4.6g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride (EDC) at 30°C, stir for 2h, react in a 35°C thermostat for 6h, take out and dialyze in a dialysis bag for 4 days, put the precipitate in the bag into a freeze dryer and dry for 24h, take out and grind to obtain aminated chitosan powder; the deacetylation degree of chitosan is ≥95%, and the viscosity is 100-200mPa·s; the concentrated hydrochloric acid is commercially available concentrated hydrochloric acid with a concentration of 38%; the ethylenediamine is analytical grade, and the specification of the dialysis bag is 8000-14000MW.

[0034] Example 3

[0035] The preparation of aminated chitosan, the specific steps are as follows:

[0036] 12g chitosan was dissolved in 500mL of 0.2mol / L sodium dihydrogen phosphate solution, and magnetically stirred at 30°C. After complete dissolution, 36mL of ethylenediamine (ED) solution was added, and stirred for 2h. The pH value was adjusted to 6 with concentrated hydrochloric acid. At 35°C, 5.6g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride (EDC) was added, and stirred for 3h. The mixture was reacted in a 45°C constant temperature box for 8h. After being taken out, the mixture was dialyzed in a dialysis bag for 6 days. The precipitate in the bag was placed in a freeze dryer and dried for 24h. The mixture was taken out and ground to obtain aminated chitosan powder. The deacetylation degree of chitosan was ≥95%, and the viscosity was 100-200mPa·s. The concentrated hydrochloric acid was commercially available with a concentration of 38%. The ethylenediamine was analytical grade, and the specification of the dialysis bag was 8000-14000MW.

[0037] Example 4

[0038] The preparation method of ACS / SH / PVA composite hydrogel includes the following specific steps:

[0039] S1. Take 1.5 g of aminated chitosan (ACS) prepared in Example 2 and 1.5 g of sodium hyaluronate (SH) and dissolve them in 300 mL of ultrapure water (1:1).

[0040] S2, dripping the sodium hyaluronate solution into the aminated chitosan solution at a rate of 3 r / min through a peristaltic pump to generate a flocculent precipitate;

[0041] S3, filter the flocculent precipitate generated in S2, freeze-dry it for 12 hours, and grind it into powder after taking it out;

[0042] S4, take 0.5g of powder and add 3mL of 2.0mol / L calcium chloride solution (CaCl2), stir evenly to obtain ACS / SH hydrogel;

[0043] S5. Take 4 g of polyvinyl alcohol, dissolve it in 40 mL of ultrapure water at 85° C., and stir it magnetically for 1 h to obtain a polyvinyl alcohol solution (10%);

[0044] S6, taking 2 g of the ACS / SH hydrogel prepared in S4, adding it to a polyvinyl alcohol solution (ACS / SH:PVA=1:2), stirring thoroughly to obtain an ACS / SH / PVA sol;

[0045] S7. Freeze the ACS / SH / PVA sol at -40°C for 3 h and thaw at 25°C for 3 h; perform freeze-thaw cycle treatment for 2 cycles to obtain ACS / SH / PVA composite hydrogel.

[0046] Example 5

[0047] The preparation method of ACS / SH / PVA composite hydrogel includes the following specific steps:

[0048] S1. Take 1.5 g of aminated chitosan (ACS) prepared in Example 2 and 1.5 g of sodium hyaluronate (SH) and dissolve them in 300 mL of ultrapure water (1:1).

[0049] S2, dripping the sodium hyaluronate solution into the aminated chitosan solution at a rate of 3 r / min through a peristaltic pump to generate a flocculent precipitate;

[0050] S3, filter the flocculent precipitate generated in S2, freeze-dry it for 12 hours, and grind it into powder after taking it out;

[0051] S4, take 0.6g of powder and add 3mL of 2.0mol / L calcium chloride solution (CaCl2), stir evenly to obtain ACS / SH hydrogel;

[0052] S5. Take 4 g of polyvinyl alcohol, dissolve it in 40 mL of ultrapure water at 85° C., and stir it magnetically for 1 h to obtain a polyvinyl alcohol solution (10%);

[0053] S6, taking 4 g of the ACS / SH hydrogel prepared in S4, adding it to a polyvinyl alcohol solution (ACS / SH:PVA=1:1), stirring thoroughly to obtain an ACS / SH / PVA sol;

[0054] S7. Freeze the ACS / SH / PVA sol at -40°C for 2 h and thaw at 25°C for 2 h; perform freeze-thaw cycle treatment for 2 cycles to obtain ACS / SH / PVA composite hydrogel.

[0055] Example 6

[0056] The preparation method of ACS / SH / PVA composite hydrogel includes the following specific steps:

[0057] S1. Take 1.8 g of aminated chitosan (ACS) prepared in Example 2 and 1.2 g of sodium hyaluronate (SH) and dissolve them in 300 mL of ultrapure water (1.5:1).

[0058] S2, dripping the sodium hyaluronate solution into the aminated chitosan solution at a rate of 3 r / min through a peristaltic pump to generate a flocculent precipitate;

[0059] S3, filter the flocculent precipitate generated in S2, freeze-dry it for 12 hours, and grind it into powder after taking it out;

[0060] S4, take 0.6g of powder and add 4.2mL of 3.0mol / L calcium chloride solution (CaCl2), stir evenly to obtain ACS / SH hydrogel;

[0061] S5. Take 2 g of polyvinyl alcohol, dissolve it in 15 mL of ultrapure water at 90° C., and stir it magnetically for 2 h to obtain a polyvinyl alcohol solution (15%);

[0062] S6, taking 4 g of the ACS / SH hydrogel prepared in S4, adding it to a polyvinyl alcohol solution (ACS / SH:PVA=2:1), stirring thoroughly to obtain an ACS / SH / PVA sol;

[0063] S7. Freeze the ACS / SH / PVA sol at -40°C for 5 h and thaw at 25°C for 3 h; perform freeze-thaw cycle treatment for 4 cycles to obtain ACS / SH / PVA composite hydrogel.

[0064] Example 7

[0065] The preparation method of ACS / SH / PVA composite hydrogel includes the following specific steps:

[0066] S1. Take 2 g of aminated chitosan (ACS) prepared in Example 2 and 1 g of sodium hyaluronate (SH) and dissolve them in 300 mL of ultrapure water (2:1).

[0067] S2, dripping the sodium hyaluronate solution into the aminated chitosan solution at a rate of 3 r / min through a peristaltic pump to generate a flocculent precipitate;

[0068] S3, filter the flocculent precipitate generated in S2, freeze-dry it for 12 hours, and grind it into powder after taking it out;

[0069] S4: 0.6 g of powder was added into 4 mL of 4.0 mol / L calcium chloride solution (CaCl2), and stirred evenly to obtain ACS / SH hydrogel;

[0070] S5. Take 1 g of polyvinyl alcohol, dissolve it in 5 mL of ultrapure water at 95°C, and stir it magnetically for 3 h to obtain a polyvinyl alcohol solution (20%);

[0071] S6, taking 3 g of the ACS / SH hydrogel prepared in S4, adding it to a polyvinyl alcohol solution (ACS / SH:PVA=3:1), stirring thoroughly to obtain an ACS / SH / PVA sol;

[0072] S7. Freeze the ACS / SH / PVA sol at -40°C for 8 h and thaw at 25°C for 4 h; perform freeze-thaw cycle treatment for 6 cycles to obtain ACS / SH / PVA composite hydrogel.

[0073] Example 8

[0074] The preparation method of ACS / SH / PVA / GO composite hydrogel, the specific steps are as follows:

[0075] S1, take 9.2 g of ACS / SH / PVA (2:1) sol prepared in S6 of Example 5;

[0076] S2. Take 0.0092 g of graphene oxide (GO) and add it to the ACS / SH / PVA sol, stir it thoroughly to obtain ACS / SH / PVA / GO sol (0.1%).

[0077] S3. Freeze the ACS / SH / PVA / GO sol obtained in S2 at -40°C for 5 h and thaw at 25°C for 3 h; perform freeze-thaw cycle treatment for 4 cycles to obtain ACS / SH / PVA / GO composite hydrogel.

[0078] Example 9

[0079] The preparation method of ACS / SH / PVA / GO composite hydrogel, the specific steps are as follows:

[0080] S1, take 9.2 g of ACS / SH / PVA (2:1) sol prepared in S6 of Example 5;

[0081] S2. Take 0.0276 g of graphene oxide (GO) and add it to the ACS / SH / PVA sol, stir it thoroughly to obtain ACS / SH / PVA / GO sol (0.3%);

[0082] S3. Freeze the ACS / SH / PVA / GO sol obtained in S2 at -40°C for 5 h and thaw at 25°C for 3 h; perform freeze-thaw cycle treatment for 4 cycles to obtain ACS / SH / PVA / GO composite hydrogel.

[0083] Example 10

[0084] The preparation method of ACS / SH / PVA / GO composite hydrogel, the specific steps are as follows:

[0085] S1, take 9.2 g of ACS / SH / PVA (2:1) sol prepared in S6 of Example 5;

[0086] S2. Take 0.0460 g of graphene oxide (GO) and add it to the ACS / SH / PVA sol, stir it thoroughly to obtain ACS / SH / PVA / GO sol (0.5%).

[0087] S3. Freeze the ACS / SH / PVA / GO sol obtained in S2 at -40°C for 5 h and thaw at 25°C for 3 h; perform freeze-thaw cycle treatment for 4 cycles to obtain ACS / SH / PVA / GO composite hydrogel.

[0088] Embodiment 11

[0089] The preparation method of ACS / SH / PVA / GO composite hydrogel, the specific steps are as follows:

[0090] S1, take 9.2 g of ACS / SH / PVA (2:1) sol prepared in S6 of Example 5;

[0091] S2. Take 0.0644 g of graphene oxide (GO) and add it to the ACS / SH / PVA sol, stir it thoroughly to obtain ACS / SH / PVA / GO sol (0.7%).

[0092] S3. Freeze the ACS / SH / PVA / GO sol obtained in S2 at -40°C for 5 h and thaw at 25°C for 3 h; perform freeze-thaw cycle treatment for 4 cycles to obtain ACS / SH / PVA / GO composite hydrogel.

[0093] Example 12

[0094] The preparation method of ACS / SH / PVA / GO composite hydrogel, the specific steps are as follows:

[0095] S1, take 9.2 g of ACS / SH / PVA (2:1) sol prepared in S6 of Example 5;

[0096] S2, adding 0.0828 g of graphene oxide (GO) to ACS / SH / PVA sol, stirring well to obtain ACS / SH / PVA / GO sol (0.9%);

[0097] S3. Freeze the ACS / SH / PVA / GO sol obtained in S2 at -40°C for 5 h and thaw at 25°C for 3 h; perform freeze-thaw cycle treatment for 4 cycles to obtain ACS / SH / PVA / GO composite hydrogel.

[0098] Comparative Example 1

[0099] The preparation method of ACS / SH hydrogel includes the following specific steps:

[0100] S1. Take 1.5 g of the aminated chitosan powder prepared in Example 2 and 1.5 g of the sodium hyaluronate powder and dissolve them in 300 mL of ultrapure water (ACS:SH=1:1).

[0101] S2, dripping the sodium hyaluronate solution into the aminated chitosan solution at a rate of 3 r / min through a peristaltic pump to generate a flocculent precipitate;

[0102] S3, filtering the flocculent precipitate generated in S2, and freeze-drying it for 12 hours;

[0103] S4, grinding the freeze-dried precipitate of S3 into powder;

[0104] S5. Take 0.6 g of the gel powder obtained in S4, add 4 mL of 3.0 M calcium chloride solution, and stir well to obtain ACS / SH hydrogel.

[0105] like Figure 1 Shown is a photo of the ACS / SH / PVA / GO composite hydrogel prepared in Example 9 for promoting cartilage repair.

[0106] like Figure 2 Shown are SEM images of the ACS / SH / PVA composite hydrogel prepared in Example 5 and the ACS / SH / PVA / GO hydrogel in Example 9.

[0107] Test Example 1

[0108] The mechanical properties of ACS / SH hydrogel, ACS / SH / PVA composite hydrogel and ACS / SH / PVA / GO composite hydrogel were tested. The specific steps are as follows:

[0109] The ACS / SH hydrogel, ACS / SH / PVA composite hydrogel and ACS / SH / PVA / GO composite hydrogel without freeze-thaw cycles were placed in polylactic acid cylindrical molds, frozen at -40 °C for 5 h, thawed at 25 °C for 3 h, and freeze-thawed for 4 cycles. The hydrogels were taken out and made into cylinders with specifications of d = 9.25 mm and h = 10.00 mm. A universal testing machine was used to perform compression tests at a speed of 2 mm / s, and curves were drawn for different deformation amounts, such as Figure 3 As shown in the figure, the ACS / SH / PVA hydrogel reaches a maximum pressure of 0.44 MPa when the ratio is 1:1 and the deformation is 70%; the ACS / SH / PVA / GO hydrogel reaches a maximum pressure of 1.04 MPa when the GO content is 0.5% and the deformation is 70%. The ACS / SH hydrogel cannot maintain a fixed shape, and even if it is placed in a mold and freeze-thawed, it cannot maintain the shape of a cylinder. Therefore, it is assumed that its pressure is much less than 0.44 MPa. Figure 3 It can be seen that the addition of polyvinyl alcohol not only greatly improves the ability of the hydrogel to maintain its shape, but also enhances its mechanical properties; the addition of graphene oxide further improves the mechanical strength of the composite hydrogel, which is 136% higher than before addition.

[0110] Test Example 2

[0111] The dynamic swelling performance test of ACS / SH / PVA composite hydrogel and ACS / SH / PVA / GO composite hydrogel was carried out. The specific steps are as follows:

[0112] The ACS / SH / PVA composite hydrogel and ACS / SH / PVA / GO composite hydrogel without freeze-thaw cycles were taken and placed in polylactic acid cylindrical molds respectively, frozen at -40°C for 5h, thawed at 25°C for 3h, and freeze-thaw cycles were performed for 4 cycles. The samples were taken out and made into cylinders with specifications of d=9.25mm and h=10.00mm. Three parallel samples were set for each group. The prepared cylindrical hydrogels were freeze-dried to obtain freeze-dried hydrogels, which were weighed and recorded as W0. The cylinders made of the two composite hydrogels were respectively placed in centrifuge tubes filled with 30mL of ultrapure water and placed in a constant temperature oscillating box for swelling. The cylinders were taken out at 0h, 0.2h, 0.5h, 1h, 3h, 6h, 14h, 24h, and 48h, and the surface moisture was wiped dry with filter paper, and the weight was recorded as W. S , the swelling rate of the hydrogel is calculated as follows:

[0113]

[0114] Where W S — is the mass of the hydrogel after swelling, in g

[0115] W0—is the mass of freeze-dried hydrogel, in g.

[0116] like Figure 4 As shown in the figure, the addition of polyvinyl alcohol makes the swelling rate of the composite hydrogel reach a maximum of 381% at 3 hours, but there is a downward trend in the swelling rate after 3 hours. This is because the molecular chains of the hydrogel gradually open and begin to degrade. The addition of graphene oxide makes the three-dimensional network structure of the hydrogel denser, the internal pores more dense, and the pore diameter smaller, which prolongs the degradation time. It only begins to degrade slowly at 24 hours. At the same time, its maximum swelling rate decreases, but still remains above 220%.

[0117] Test Example 3

[0118] The hydrophilicity test of ACS / SH / PVA composite hydrogel and ACS / SH / PVA / GO composite hydrogel was carried out. The specific steps are as follows:

[0119] Take the ACS / SH / PVA composite hydrogel (Example 6) and the ACS / SH / PVA / GO composite hydrogel (Example 9) that have not been freeze-thawed, and put them into polylactic acid cylindrical molds respectively, freeze them at -40°C for 5h, thaw them at 25°C for 3h, and perform freeze-thaw cycle treatment for 4 cycles. Take them out and make cylinders with specifications of d=9.25mm and h=10.00mm. Three parallel samples are set in each group. The cylindrical samples are placed on the device to be tested, and 10μL of ultrapure water is added to the surface of the composite hydrogel at a liquid addition rate of 0.5mL / min. The contact angle of the water droplet is measured multiple times at room temperature and the average value is taken.

[0120] like Figure 5 As shown in the figure, the contact angle of ACS / SH / PVA composite hydrogel is 68.5°, which is hydrophilic. The addition of graphene oxide enhances the hydrophilicity of ACS / SH / PVA / GO composite hydrogel, with a contact angle of 40.0°. Hydrophilicity is conducive to cell adhesion and growth.

[0121] Test Example 4

[0122] The rebound performance test of ACS / SH / PVA / GO composite hydrogel is carried out as follows:

[0123] The ACS / SH / PVA / GO composite hydrogel (Example 10) without freeze-thaw cycles was taken and placed in polylactic acid cylindrical molds, respectively, frozen at -40 ° C for 5 h, thawed at 25 ° C for 3 h, and freeze-thaw cycles were performed for 4 cycles. The sample was taken out and made into a cylinder with specifications of d = 9.25 mm and h = 10.00 mm. The cylindrical sample was placed on a glass plane and stress was applied to it from above, such as Figure 6 As shown, when the composite hydrogel is compressed to a height of 1 / 2h and the stress is removed, the composite hydrogel can quickly recover to its initial height, indicating that the composite hydrogel has good resilience and is consistent with the elastic properties of cartilage tissue.

[0124] Through the above-mentioned embodiments and test example results, it can be seen that the composite hydrogel prepared by the present invention has good mechanical properties and a porous structure; in the preparation process, no toxic cross-linking agent is used, and the raw materials used are all non-toxic and harmless polymer materials, so that the composite hydrogel prepared by the method has good biocompatibility; both the hydrophilicity and swelling properties show that the composite hydrogel is very conducive to the attachment and growth of cells, and the composite hydrogel has good injectability and is expected to be applied in the field of biological 3D printing technology.

[0125] The above descriptions are only preferred embodiments and test examples of the present invention, and are not intended to limit the scope of the present invention. Any equivalent transformations made using the contents of the present invention's specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the protection scope of the present invention.

Claims

1. A method for preparing a composite hydrogel for promoting cartilage tissue repair, It is characterized in that The specific steps are as follows: (1) dissolving aminated chitosan and sodium hyaluronate in ultrapure water respectively, filtering out the precipitate after mixing, freeze-drying, and adding calcium chloride solution to obtain ACS / SH hydrogel; (2) dissolving polyvinyl alcohol in ultrapure water to obtain a polyvinyl alcohol solution, adding the ACS / SH hydrogel obtained in step (1), and stirring evenly to obtain a (ACS / SH) / PVA hydrogel; (3) (ACS / SH) / PVA hydrogel was subjected to cyclic freeze-thaw treatment to obtain composite hydrogel.

2. The method for preparing the composite hydrogel for promoting cartilage tissue repair according to claim 1, It is characterized in that The specific steps of the method for preparing the aminated chitosan in step (1) are as follows: Dissolve 8-12g chitosan in 300-500mL phosphate solution, stir magnetically at 20-30℃, add 28-36mL ethylenediamine after complete dissolution, stir for 1-2h, adjust pH value to 4-6 with concentrated hydrochloric acid, add 3.6-5.6g 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride at 25-35℃, stir for 1-3h, react at 30-45℃ for 4-8h, take out and dialyze in a dialysis bag for 2-6 days, freeze-dry the precipitate in the bag, take out and grind to obtain aminated chitosan powder.

3. The method for preparing the composite hydrogel for promoting cartilage tissue repair according to claim 2, It is characterized in that The chitosan has a deacetylation degree of ≥95% and a viscosity of 100-200 mPa·s; the phosphate solution is a 0.2 mol / L sodium dihydrogen phosphate solution; the concentrated hydrochloric acid is commercially available concentrated hydrochloric acid with a concentration of 38%; and the specification of the dialysis bag is 8000-14000 MW.

4. The method for preparing the composite hydrogel for promoting cartilage tissue repair according to claim 1, It is characterized in that The mass ratio of aminated chitosan to sodium hyaluronate in step (1) is 1-2:1; the molecular weight of sodium hyaluronate is 1000K; the mass volume ratio of the total mass of aminated chitosan and sodium hyaluronate to the mass volume ratio of calcium chloride solution is 1:5-7.

5. The method for preparing the composite hydrogel for promoting cartilage tissue repair according to claim 1, It is characterized in that The mass concentration of the polyvinyl alcohol solution in step (2) is 10% to 20%, and the mass ratio of ACS / SH hydrogel to polyvinyl alcohol is 0.5 to 3:

1.

6. The method for preparing the composite hydrogel for promoting cartilage tissue repair according to claim 1, It is characterized in that Step (3) is replaced by: adding graphene oxide to the hydrogel obtained in step (2), and subjecting the resultant to cyclic freeze-thaw treatment to obtain a composite hydrogel; the amount of graphene oxide added is 0.1% to 0.9% of the mass of the (ACS / SH) / PVA hydrogel.

7. A method for preparing a composite hydrogel for promoting cartilage tissue repair according to claim 1 or 6, It is characterized in that The specific method of freeze-thaw cycle treatment in step (3) is as follows: freezing at -40°C for 2 to 8 hours, thawing at 25°C for 2 to 4 hours, and freezing and thawing again for 2 to 6 cycles.