Forming method of copper-based desulfurization adsorbent for ultra-deep removal of thiophene

By mixing the copper-based desulfurization adsorbent precursor with a binder and an extrusion aid, and then using an extruder to shape and roast it, the problems of low mechanical strength and reduced desulfurization performance during the molding process of the copper-based desulfurization adsorbent are solved and achieved. A shaped adsorbent with high mechanical strength and high desulfurization efficiency, suitable for ultra-deep desulfurization of coke oven gas.

CN118743976AActive Publication Date: 2024-10-08TAIYUAN UNIVERSITY OF TECHNOLOGY
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410923300.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-10-08
Estimated Expiration
2044-07-10

AI Technical Summary

Technical Problem

In the molding process of existing copper-based desulfurization adsorbents, there are problems such as low mechanical strength and reduced desulfurization performance. Especially when applied in the powder state, equipment resistance increases, mass and heat transfer deteriorates, powder loss is serious, and the molding process is complex and costly. high.

Method used

The copper-based desulfurization adsorbent precursor is uniformly mixed with the binder and extrusion aid, and then kneaded by adding silica sol nitric acid aqueous solution, molded through an extruder, aged at room temperature, dried and then roasted to prepare a high mechanical strength shaped desulfurization adsorbent.

Benefits of technology

On the basis of maintaining the original desulfurization performance, the mechanical strength of the shaped desulfurization adsorbent is significantly improved, its penetration sulfur capacity and specific surface area are increased, and the preparation cost and process complexity are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118743976A_ABST
    Figure CN118743976A_ABST
Patent Text Reader

Abstract

The invention relates to a forming method of a copper-based desulfurization adsorbent for ultra-deep removal of thiophene, which comprises the following steps: uniformly mixing the copper-based desulfurization adsorbent with 30-60% by mass of a binder and 1-10% by mass of an extrusion aid, adding a silica sol nitric acid aqueous solution, kneading to obtain a wet material, carrying out extrusion molding by a banded extruder, standing at normal temperature, aging, drying, and roasting at 350-550 DEG C for 3-8 hours to obtain a formed desulfurization adsorbent, wherein the binder is a mixture obtained by mixing pseudo-boehmite and kaolin according to the mass ratio of 1: (1-3), and the extrusion aid is sesbania powder. The prepared molded desulfurization adsorbent has excellent desulfurization performance while ensuring that the prepared molded desulfurization adsorbent meets the industrial application mechanical strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coke oven gas purification and relates to a molding method of a desulfurization adsorbent, in particular to a molding method of a copper-based desulfurization adsorbent for ultra-deep removal of thiophene. Background Art

[0002] Coke oven gas is one of the main by-products of the coking industry. Every ton of coke produced can generate 400m3 of 3 Using coke oven gas as raw material to prepare natural gas is one of the important ways to efficiently utilize coke oven gas.

[0003] However, the sulfides contained in coke oven gas will poison the nickel-based catalyst for the methanation reaction and shorten its service life. Therefore, most of the sulfides in the coke oven gas need to be removed through rough desulfurization and fine desulfurization. In current industrial production, the process of iron-molybdenum pre-hydrogenation + cobalt-molybdenum primary hydrogenation + zinc oxide adsorption + nickel-molybdenum secondary hydrogenation + zinc oxide adsorption is generally used to remove COS, CS2, mercaptans, sulfides, H2S, etc. in coke oven gas, but there will still be ppm-level thiophene. It is necessary to use an ultra-deep desulfurization adsorption tower after the above-mentioned desulfurization process to ultra-deeply remove the remaining thiophene to the ppb level to meet the use requirements of the methanation catalyst.

[0004] CN112138625A discloses an adsorption desulfurizer for ultra-deep removal of thiophene in coke oven gas and a preparation method thereof, wherein a carrier Al2O3 and additives NiO and ZrO2 are introduced on the basis of Cu / ZnO to improve the mechanical strength of the adsorption desulfurizer and increase the pore structure of the adsorption desulfurizer. The surface area of ​​the adsorption desulfurizer is increased, the activity of the adsorption desulfurizer is enhanced, and the desulfurization efficiency is further improved through the synergistic effect of the metal additives on copper and zinc. However, the utilization rate of the active components copper and zinc in the adsorption desulfurizer is only about 30%, and the amount of the precious metal zirconium is large, resulting in problems such as low sulfur capacity, low activity, and high preparation cost of the adsorption desulfurizer.

[0005] CN115254006A discloses a desulfurization adsorbent for ultra-deep removal of thiophene from coke oven gas and a preparation method thereof. Pseudo-boehmite is selected as an alumina carrier, and the alumina content is increased by 10-20% and the zirconium oxide content is reduced by adjusting the content and ratio of the carrier and the metal additive zirconium oxide, thereby improving the desulfurization performance of the desulfurization adsorbent, achieving ultra-deep removal of thiophene in coke oven gas, and the penetration sulfur capacity is not less than 39 mg / g.

[0006] Although the desulfurization effect of the desulfurization adsorbent has met the requirements, considering that the adsorbent is in powder state, if it is directly used in industrial production, there will be serious problems such as a sharp increase in equipment resistance, deterioration of mass transfer and heat transfer, and loss of powdered adsorbent driven by the bed airflow, which restricts its practical application in industry. Therefore, it is necessary to consider molding the adsorbent to obtain a catalyst with a certain shape and mechanical strength to reduce the bed pressure drop, improve mass transfer and heat transfer, and at the same time increase the diffusion rate of the reactants.

[0007] However, copper-based adsorbents are brittle materials and have poor powder particle fluidity, making molding difficult. The rotation molding process has defects such as uneven diameter, rough surface, and low mechanical strength; since the required adsorbent molding diameter is small, the compression molding process is not easy to produce, with a low success rate and high cost; the spray drying molding process consumes a lot of electricity and has low thermal efficiency. There is a lot of dust in the production process, the product particle properties are differentiated, and the production process is complex and difficult to control. The extrusion molding process has simple operating conditions and large output, and is currently the most commonly used molding method in industry. However, during the molding process, the addition of binders can easily cause a decrease in the mechanical strength of the adsorbent and the corresponding desulfurization performance. Therefore, it is necessary to obtain a molded adsorbent with high mechanical strength while maintaining the original desulfurization performance of the adsorbent to the greatest extent.

[0008] CN114768885A provides a method for extruding a strip of an acetophenone hydrogenation catalyst, wherein catalyst raw powder, silica sol, deionized water, extrusion aid and pore expander are kneaded into a plastic body in a certain proportion, and then extruded, dried and roasted to prepare a strip catalyst. The addition of the pore expander significantly improves the pore structure of the catalyst, reduces the diffusion in the catalyst pores, and increases the life of the catalyst. However, the catalyst raw powder has been roasted once, and is roasted again after molding. The secondary roasting not only makes the preparation and molding process of the adsorbent complicated, but also has a high cost.

[0009] CN112705168A discloses a method for forming an ultra-microporous MOF adsorbent material, which obtains spherical particles of MOF material that meet industrial needs by adjusting the type and ratio of the binder. It uses polyvinyl alcohol and methyl cellulose to form ZIF-7 powder, and obtains ZIF-7 spherical particles with a higher loading rate. Although the spherical particles have a higher mechanical strength, the adsorption capacity only maintains 89% of the original powder. The addition of the binder during the forming process reduces the performance of the original powder.

[0010] Therefore, if a desulfurization adsorbent with high adsorption capacity can be obtained and has high mechanical strength and maintains or improves its desulfurization performance, it will be of great significance for the application of the desulfurization adsorbent in ultra-deep desulfurization of coke oven gas in industrial production. Summary of the invention

[0011] The purpose of the present invention is to provide a molding method for a copper-based desulfurization adsorbent for ultra-deep thiophene removal, so as to solve the problems of low mechanical strength and decreased desulfurization performance in the molding process of the powdered adsorbent.

[0012] To achieve the above-mentioned purpose of the invention, the present invention provides a molding method of a copper-based desulfurization adsorbent for ultra-deep removal of thiophene, which is based on a copper-based desulfurization adsorbent precursor as a raw material, mixed evenly with a binder in an amount of 30-60% by weight of the copper-based desulfurization adsorbent precursor and an extrusion aid in an amount of 1-10% by weight of the copper-based desulfurization adsorbent precursor, added with a silica sol nitric acid aqueous solution and kneaded to obtain a wet material, extruded and molded by an extruder, aged and dried at room temperature, and calcined at 350-550°C for 3-8 hours to obtain a molded desulfurization adsorbent.

[0013] The copper-based desulfurization adsorbent precursor is a precursor powder prepared according to the method disclosed in CN115254006A, specifically comprising:

[0014] 1) Weigh 5-25 parts of copper nitrate trihydrate, 6-30 parts of zinc nitrate hexahydrate, 5-20 parts of pseudo-boehmite, 0.1-2 parts of nickel nitrate hexahydrate, and 0.1-5 parts of zirconium nitrate pentahydrate in deionized water and dissolve them uniformly to obtain a first solution;

[0015] 2) Weigh 10 to 40 parts of anhydrous sodium carbonate and dissolve them evenly in deionized water to obtain a second solution;

[0016] 3) Mixing the first solution and the second solution at 40-90° C. to perform a coprecipitation reaction;

[0017] 4) Aging the coprecipitation reaction product at 30-90° C. for 1-5 hours, washing and drying, and obtaining a copper-based desulfurization adsorbent precursor.

[0018] Furthermore, the binder is a mixture of pseudo-boehmite and kaolin in a mass ratio of 1: (1-3), and the extrusion aid is sesbania powder.

[0019] By adopting the molding method of the present invention, a molded copper-based desulfurization adsorbent with high mechanical strength can be prepared while maintaining the desulfurization performance of the copper-based desulfurization adsorbent powder prepared in CN115254006A.

[0020] Furthermore, in the molding method described in the present invention, the concentration of the silica sol nitric acid aqueous solution used is preferably 20-50%, and the amount used is preferably 30-60% of the mass of the copper-based desulfurization adsorbent precursor.

[0021] Furthermore, the present invention adds an appropriate amount of concentrated nitric acid as a peptizing agent to the silica sol to obtain the silica sol nitric acid aqueous solution, and the amount of concentrated nitric acid added is preferably 2-15% of the mass of the copper-based desulfurization adsorbent precursor.

[0022] Specifically, the present invention preferably kneads for 10 to 30 minutes after adding the silica sol nitric acid aqueous solution to obtain a uniformly mixed wet material.

[0023] More specifically, the present invention uses a cylindrical molding die with a diameter of 1 to 4 mm to extrude the wet material, and the frequency and rotation speed of the extruder during the extrusion molding is preferably 10 to 30 r / min.

[0024] Furthermore, the present invention requires that the extruded wet strip material with a diameter of 1 to 5 mm be aged in air at room temperature for no less than 4 hours before being dried. The preferred drying condition is drying at 100 to 150° C. for 10 to 15 hours.

[0025] According to tests, the mechanical strength of the molded desulfurization adsorbent prepared by the molding method of the present invention is as high as 64N / cm. It is loaded into a fixed bed reactor and reduced at 200°C for 3 hours under a hydrogen atmosphere. Simulated coke oven gas (58% H2, 26% CH4, 8% CO, 3% CO2, 4% N2, 1% O2) mixed with 300ppmv thiophene is introduced for desulfurization adsorption reaction. The breakthrough sulfur capacity of the molded desulfurization adsorbent is not less than 20mg / g.

[0026] The optimal penetration adsorption amount of the powdered desulfurization adsorbent prepared in CN115254006A is 39.46 mg / g. The present invention is based on the copper-based desulfurization adsorbent precursor of CN115254006A, and adds molding aids such as binders at a ratio of approximately 1:1 to prepare a molded desulfurization adsorbent. The effective components account for about 50% of the total mass of the molded desulfurization adsorbent. Therefore, the penetration adsorption amount of the molded desulfurization adsorbent of the present invention calculated according to the effective components should not be less than 40 mg / g, or even slightly higher than the penetration adsorption amount of the powdered desulfurization adsorbent in CN115254006A. The molded desulfurization adsorbent prepared by the present invention can improve the mechanical strength without reducing the desulfurization performance of the desulfurization adsorbent.

[0027] The present invention uses a copper-based desulfurization adsorbent precursor as a raw material to prepare a molded desulfurization adsorbent. Since the precursor itself has a certain adhesiveness, the amount of the adhesive used can be reduced during the molding process. The molded desulfurization adsorbent not only improves the effective utilization rate of the active components, but also ensures its mechanical strength. The adhesive and extrusion aid used for molding will produce a small amount of CO2 and H2O during the roasting process, thereby leaving more micropores, so that the pore structure and specific surface area of ​​the molded desulfurization adsorbent are increased, the distribution capacity of the active components in the molded desulfurization adsorbent is improved, and more active sites are provided for the reaction adsorption of thiophene, thereby increasing its desulfurization activity.

[0028] The entire preparation process of the molded desulfurization adsorbent of the present invention only requires one calcination treatment, which has little effect on the desulfurization performance and mechanical strength of the molded desulfurization adsorbent, and the preparation process is simple and the cost is reduced.

[0029] The pseudo-boehmite used in the molding process of the present invention can be used as a binder to improve the mechanical strength of the molded desulfurization adsorbent on the one hand, and can also be used as a dispersant to make the desulfurization adsorbent evenly dispersed and have a higher utilization rate, thereby increasing the specific surface area and pore volume of the desulfurization adsorbent and thus increasing the sulfur capacity of the desulfurization adsorbent; while kaolin mainly plays a bonding role and can be filled in the material gaps to a large extent. After calcination, it is not easy to volatilize and decompose, so that the final molded desulfurization adsorbent has better strength. The present invention uses it as a composite binder, and its appropriate addition ratio can not only maintain or improve the sulfur capacity of the desulfurization adsorbent, but also make the molded desulfurization adsorbent have better strength. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is the penetration adsorption amount of thiophene in coke oven gas by the molded desulfurization adsorbent prepared in each embodiment and comparative example.

[0031] Figure 2 It is the mechanical strength of the molded desulfurization adsorbent prepared in each embodiment and comparative example. Implementation

[0032] The specific implementation of the present invention is further described in detail below in conjunction with the accompanying drawings and examples. The following examples are only used to more clearly illustrate the technical solution of the present invention so that those skilled in the art can well understand and utilize the present invention, rather than limiting the scope of protection of the present invention.

[0033] The production processes, experimental methods or detection methods involved in the embodiments and comparative examples of the present invention are all conventional methods in the prior art unless otherwise specified, and their names and / or abbreviations are all conventional names in the field and are very clear and unambiguous in the relevant application fields. Those skilled in the art can understand the conventional process steps based on the names and apply the corresponding equipment to implement them according to conventional conditions or the conditions recommended by the manufacturer.

[0034] The various instruments, equipment, raw materials or reagents used in the embodiments of the present invention are not particularly limited in terms of their sources, and are all conventional products that can be purchased through regular commercial channels, or can be prepared according to conventional methods well known to those skilled in the art. Example

[0035] Example 1

[0036] 7.25 g of copper nitrate trihydrate, 8.93 g of zinc nitrate hexahydrate, 3.74 g of pseudoboehmite, 0.40 g of nickel nitrate hexahydrate, and 0.32 g of zirconium nitrate pentahydrate were weighed, added to 200 mL of deionized water, and dissolved uniformly to obtain a first solution.

[0037] 11.13 g of anhydrous sodium carbonate was added to 350 mL of deionized water and dissolved uniformly to obtain a second solution.

[0038] The above two solutions were simultaneously added dropwise into a stirred reaction vessel to cause a coprecipitation reaction at 70° C. The dropping rate of the first solution was 10 ml / min, the dropping rate of the second solution was 15 ml / min, and the pH value of the coprecipitation reaction was adjusted to 7.5.

[0039] The coprecipitation reaction product was aged at 80° C. for 3 h, filtered, the filter cake was washed with deionized water for 3 to 5 times, and dried in an oven at 110° C. for 12 h to obtain a copper-based desulfurization adsorbent precursor.

[0040] 200 g of copper-based desulfurization adsorbent precursor, 10 g of sesbania powder, 33.3 g of pseudo-boehmite and 66.7 g of kaolin were weighed and added into a kneading device, and stirred for 15 minutes to mix them evenly.

[0041] Weigh 85.5 g of 30% silica sol, 6 g of concentrated nitric acid and 120 g of deionized water, add them slowly into a kneading device in sequence, and knead for 15 minutes to obtain a uniform wet material.

[0042] The wet material was quickly transferred to an extruder with a 2mm round hole die, and the strip-shaped material was extruded at a speed of 18r / min. After aging at room temperature in air for 6h, it was placed in an oven at 110℃ for 12h, placed in a muffle furnace, heated to 350℃ at a heating rate of 2℃ / min in air atmosphere, and calcined for 4.5h to prepare a shaped desulfurization adsorbent, which was recorded as PA1.

[0043] Weigh 6g of PA1, load it into a fixed bed reactor with an inner diameter of 18mm, and heat it to 200℃ for 3h under hydrogen atmosphere. Keep the reaction temperature at 200℃, introduce a certain amount of simulated coke oven gas (composition 58% H2, 26% CH4, 8% CO, 3% CO2, 4% N2, 1% O2) into the fixed bed reactor, and mix 300ppmv thiophene into the simulated coke oven gas to carry out desulfurization adsorption reaction. Use gas chromatography to detect the change of thiophene content at the outlet of the fixed bed reactor. The calculation results are as follows: Figure 1 The penetration sulfur capacity of PA1 in the sample is 20.33 mg / g.

[0044] The compressive strength of the molded desulfurization adsorbent was measured using a particle strength tester. The molded desulfurization adsorbent was cut into 5 mm long particles, 20 particles were randomly selected to measure their mechanical strength, and the maximum and minimum values ​​were removed to obtain the average value to obtain the mechanical strength result. Figure 2 PA1 in it has a mechanical strength of 64.1N / cm.

[0045] Example 2

[0046] 8.25 g of copper nitrate trihydrate, 9.93 g of zinc nitrate hexahydrate, 3.74 g of pseudoboehmite, 0.40 g of nickel nitrate hexahydrate, and 0.35 g of zirconium nitrate pentahydrate were weighed, added into 200 mL of deionized water, and dissolved uniformly to obtain a first solution.

[0047] 11.13 g of anhydrous sodium carbonate was added to 300 mL of deionized water and dissolved uniformly to obtain a second solution.

[0048] The above two solutions were simultaneously added dropwise into a stirred reaction vessel to cause a coprecipitation reaction at 60° C. The dropping rate of the first solution was 10 ml / min, the dropping rate of the second solution was 15 ml / min, and the pH value of the coprecipitation reaction was adjusted to 7.5.

[0049] The coprecipitation reaction product was aged at 80° C. for 2 h, filtered, the filter cake was washed with deionized water for 3 to 5 times, and dried in an oven at 100° C. for 12 h to obtain a copper-based desulfurization adsorbent precursor.

[0050] 200 g of copper-based desulfurization adsorbent precursor, 10 g of sesbania powder, 25 g of pseudo-boehmite and 75 g of kaolin were weighed and added into a kneading device, and stirred for 15 minutes to mix them evenly.

[0051] Weigh 85.5 g of 30% silica sol, 6 g of concentrated nitric acid and 120 g of deionized water, add them slowly into a kneading device in sequence, and knead for 15 minutes to obtain a uniform wet material.

[0052] The wet material was quickly transferred to an extruder with a 2mm round hole die, and the strip-shaped material was extruded at a speed of 18r / min. After aging at room temperature in air for 6h, it was placed in an oven at 120℃ for 12h, placed in a muffle furnace, and heated to 400℃ at a heating rate of 3℃ / min in air atmosphere and calcined for 6h to prepare a shaped desulfurization adsorbent, which was recorded as PA2.

[0053] The desulfurization performance and mechanical strength of PA2 were tested according to the method in Example 1. The results are as follows Figure 1 and Figure 2 As shown in PA2, its penetration sulfur capacity is 19.64 mg / g and its mechanical strength is 52.24 N / cm.

[0054] Example 3

[0055] 12.08 g of copper nitrate trihydrate, 14.88 g of zinc nitrate hexahydrate, 6.74 g of pseudoboehmite, 0.67 g of nickel nitrate hexahydrate, and 0.53 g of zirconium nitrate pentahydrate were weighed, added into 200 mL of deionized water, and dissolved uniformly to obtain a first solution.

[0056] 18.55 g of anhydrous sodium carbonate was added to 300 mL of deionized water and dissolved uniformly to obtain a second solution.

[0057] The above two solutions were simultaneously added dropwise into a stirred reaction vessel to cause a coprecipitation reaction at 70° C. The dropping rate of the first solution was 10 ml / min, the dropping rate of the second solution was 15 ml / min, and the pH value of the coprecipitation reaction was adjusted to 7.3.

[0058] The coprecipitation reaction product was aged at 80° C. for 3 h, filtered, the filter cake was washed with deionized water for 3 to 5 times, and dried in an oven at 110° C. for 12 h to obtain a copper-based desulfurization adsorbent precursor.

[0059] 200 g of copper-based desulfurization adsorbent precursor, 10 g of sesbania powder, 50 g of pseudo-boehmite and 50 g of kaolin were weighed and added into a kneading device, and stirred for 15 minutes to mix them evenly.

[0060] Weigh 85.5 g of 30% silica sol, 6 g of concentrated nitric acid and 120 g of deionized water, add them slowly into a kneading device in sequence, and knead for 15 minutes to obtain a uniform wet material.

[0061] The wet material was quickly transferred to an extruder with a 2mm round hole die, and the strip-shaped material was extruded at a speed of 18r / min. After aging for 6h at room temperature in air, it was placed in an oven and dried at 150°C for 10h. It was placed in a muffle furnace and heated to 450°C at a heating rate of 4°C / min in an air atmosphere and calcined for 5h to prepare a shaped desulfurization adsorbent, which was recorded as PA3.

[0062] The desulfurization performance and mechanical strength of PA3 were tested according to the method in Example 1. The results are as follows Figure 1 and Figure 2 As shown in PA3, its penetration sulfur capacity is 19.06 mg / g and its mechanical strength is 58.56 N / cm.

[0063] Example 4

[0064] 12.08 g of copper nitrate trihydrate, 14.88 g of zinc nitrate hexahydrate, 6.38 g of pseudo-boehmite, 0.40 g of nickel nitrate hexahydrate, and 0.47 g of zirconium nitrate pentahydrate were weighed, added into 200 mL of deionized water, and dissolved uniformly to obtain a first solution.

[0065] 18.55 g of anhydrous sodium carbonate was added to 300 mL of deionized water and dissolved uniformly to obtain a second solution.

[0066] The above two solutions were simultaneously added dropwise into a stirred reaction vessel to cause a coprecipitation reaction at 70° C. The dropping rate of the first solution was 10 ml / min, the dropping rate of the second solution was 15 ml / min, and the pH value of the coprecipitation reaction was adjusted to 7.5.

[0067] The coprecipitation reaction product was aged at 80° C. for 3 h, filtered, the filter cake was washed with deionized water for 3 to 5 times, and dried in an oven at 110° C. for 12 h to obtain a copper-based desulfurization adsorbent precursor.

[0068] 200 g of copper-based desulfurization adsorbent precursor, 10 g of sesbania powder, 40 g of pseudo-boehmite and 80 g of kaolin were weighed and added into a kneading device, and stirred for 15 minutes to mix them evenly.

[0069] Weigh 85.5 g of 30% silica sol, 6 g of concentrated nitric acid and 120 g of deionized water, add them slowly into a kneading device in sequence, and knead for 15 minutes to obtain a uniform wet material.

[0070] The wet material was quickly transferred to an extruder with a 2mm round hole die, and the strip-shaped material was extruded at a speed of 18r / min. After aging at room temperature in air for 6h, it was placed in an oven at 130°C for 10h, placed in a muffle furnace, and heated to 500°C at a heating rate of 5°C / min in an air atmosphere and calcined for 4h to prepare a shaped desulfurization adsorbent, which was recorded as PA4.

[0071] The desulfurization performance and mechanical strength of PA4 were tested according to the method in Example 1. The results are as follows Figure 1 and Figure 2 As shown in the PA4, its penetration sulfur capacity is 17.89 mg / g and its mechanical strength is 60.45 N / cm.

[0072] Example 5

[0073] 200 g of the copper-based desulfurization adsorbent precursor prepared in Example 1, 10 g of sesbania powder, 26.7 g of pseudo-boehmite and 53.3 g of kaolin were weighed and added into a kneading device, and stirred for 15 minutes to mix them evenly.

[0074] Weigh 85.5 g of 30% silica sol, 6 g of concentrated nitric acid and 120 g of deionized water, add them slowly into a kneading device in sequence, and knead for 15 minutes to obtain a uniform wet material.

[0075] The wet material was quickly transferred to an extruder with a 2mm round hole die, and the strip-shaped molding material was extruded at a speed of 18r / min. After aging for 6h at room temperature in air, it was placed in an oven at 110℃ for 10h, placed in a muffle furnace, and heated to 550℃ at a heating rate of 3℃ / min in air atmosphere and calcined for 3h to prepare a molded desulfurization adsorbent, which was recorded as PA5.

[0076] The desulfurization performance and mechanical strength of PA5 were tested according to the method in Example 1. The results are as follows Figure 1 and Figure 2 As shown in PA5, its penetration sulfur capacity is 18.14 mg / g and its mechanical strength is 55.51 N / cm.

[0077] Comparative Example 1

[0078] 7.25 g of copper nitrate trihydrate, 8.93 g of zinc nitrate hexahydrate, 3.74 g of pseudoboehmite, 0.40 g of nickel nitrate hexahydrate, and 0.32 g of zirconium nitrate pentahydrate were weighed, added to 200 mL of deionized water, and dissolved uniformly to obtain a first solution.

[0079] 11.13 g of anhydrous sodium carbonate was added to 350 mL of deionized water and dissolved uniformly to obtain a second solution.

[0080] The above two solutions were simultaneously added dropwise into a stirred reaction vessel to cause a coprecipitation reaction at 70° C. The dropping rate of the first solution was 10 ml / min, the dropping rate of the second solution was 15 ml / min, and the pH value of the coprecipitation reaction was adjusted to 7.5.

[0081] The coprecipitation reaction product was aged at 80° C. for 3 h, filtered, the filter cake was washed with deionized water for 3 to 5 times, and dried in an oven at 110° C. for 12 h to obtain a copper-based desulfurization adsorbent precursor.

[0082] The copper-based desulfurization adsorbent precursor was placed in a muffle furnace, heated to 350° C. at a heating rate of 2° C. / min, and calcined in an air atmosphere for 4.5 h to prepare a desulfurization adsorbent powder.

[0083] 200 g of desulfurization adsorbent powder, 10 g of sesbania powder, 33.3 g of pseudo-boehmite and 66.7 g of kaolin were weighed and added into a kneading device, and stirred for 15 minutes to mix them evenly.

[0084] Weigh 85.5 g of 30% silica sol, 6 g of concentrated nitric acid and 120 g of deionized water, add them slowly into a kneading device in sequence, and knead for 15 minutes to obtain a uniform wet material.

[0085] The wet material was quickly transferred to an extruder with a 2mm round hole die, and the strip-shaped material was extruded at a speed of 18r / min. After aging for 6h at room temperature in air, it was placed in an oven at 110℃ for 12h, placed in a muffle furnace, heated to 350℃ at a heating rate of 2℃ / min in air atmosphere, and calcined for 4.5h to prepare a shaped desulfurization adsorbent, which was recorded as PB1.

[0086] The desulfurization performance and mechanical strength of PB1 were tested according to the method in Example 1. The results are as follows Figure 1 and Figure 2 As shown in PB1, its penetration sulfur capacity is 18.69 mg / g, slightly lower than that of Example 1, but its mechanical strength is only 41.91 N / cm, which is significantly lower than that of Example 1, which has a mechanical strength of only 64.1 N / cm.

[0087] Comparative Example 2

[0088] 200 g of the copper-based desulfurization adsorbent precursor prepared in Example 1, 10 g of sesbania powder, 66.7 g of pseudo-boehmite and 33.3 g of kaolin were weighed and added into a kneading device, and stirred for 15 minutes to mix them evenly.

[0089] Weigh 85.5 g of 30% silica sol, 6 g of concentrated nitric acid and 120 g of deionized water, add them slowly into a kneading device in sequence, and knead for 15 minutes to obtain a uniform wet material.

[0090] The wet material was quickly transferred to an extruder with a 2mm round hole die, and the strip-shaped material was extruded at a speed of 18r / min. After aging at room temperature in air for 6h, it was placed in an oven at 120℃ for 12h, placed in a muffle furnace, and heated to 400℃ at a heating rate of 3℃ / min in air atmosphere and calcined for 6h to prepare a shaped desulfurization adsorbent, which was recorded as PB2.

[0091] The desulfurization performance and mechanical strength of PB2 were tested according to the method in Example 1. The results are as follows: Figure 1 and Figure 2 As shown in PB2, its penetration sulfur capacity is reduced to 15.35 mg / g, and the mechanical strength is reduced to 36.67 N / cm.

[0092] Comparative Example 3

[0093] 200 g of the copper-based desulfurization adsorbent precursor prepared in Example 1, 10 g of sesbania powder, 75 g of pseudo-boehmite and 25 g of kaolin were weighed and added into a kneading device, and stirred for 15 minutes to mix them evenly.

[0094] Weigh 85.5 g of 30% silica sol, 6 g of concentrated nitric acid and 120 g of deionized water, add them slowly into a kneading device in sequence, and knead for 15 minutes to obtain a uniform wet material.

[0095] The wet material was quickly transferred to an extruder with a 2mm round hole die, and the strip-shaped material was extruded at a speed of 18r / min. After aging at room temperature in air for 6h, it was placed in an oven at 120℃ for 12h, placed in a muffle furnace, and heated to 400℃ at a heating rate of 3℃ / min in air atmosphere and calcined for 6h to prepare a shaped desulfurization adsorbent, which was recorded as PB3.

[0096] The desulfurization performance and mechanical strength of PB3 were tested according to the method in Example 1. The results are as follows: Figure 1 and Figure 2 As shown in PB3 in the figure, its penetration sulfur capacity is reduced to 16.91 mg / g, and its mechanical strength is significantly reduced to 23.59 N / cm.

[0097] The desulfurization performance and mechanical strength test results of the molded desulfurization adsorbents prepared in the above-mentioned Examples 1 to 5 and Comparative Examples 1 to 3 show that the present invention uses a copper-based desulfurization adsorbent precursor for molding. Due to the strong fluidity and stacking state of the precursor's own raw materials or the interaction between the powder particles, the mechanical strength of the molded desulfurization adsorbent is the largest, and the desulfurization adsorbent molded by the precursor will produce more micropores after calcination, and has a larger specific surface area, which can reduce the influence of internal diffusion during the desulfurization evaluation process and further improve the desulfurization activity of the molded desulfurization adsorbent. The mechanical strength of Comparative Examples 1 to 3 is greatly reduced, and the corresponding desulfurization performance is also reduced.

[0098] The above embodiments of the present invention do not describe all the details in detail, nor limit the present invention to the above embodiments. Various changes, modifications, substitutions and variations made by ordinary technicians in this field without departing from the principles and purpose of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for forming a copper-based desulfurization adsorbent for ultra-deep thiophene removal, which is to use a copper-based desulfurization adsorbent precursor as a raw material, mix it evenly with a binder of 30-60% of the mass of the copper-based desulfurization adsorbent precursor and an extrusion aid of 1-10% of the mass of the copper-based desulfurization adsorbent precursor, add a silica sol nitric acid aqueous solution to knead to obtain a wet material, extrude it with an extruder, place it at room temperature for aging and drying, and roast it at 350-550° C. for 3-8 hours to prepare a molded desulfurization adsorbent; in, The copper-based desulfurization adsorbent precursor is a precursor powder prepared according to the following method: 1) Weigh 5-25 parts of copper nitrate trihydrate, 6-30 parts of zinc nitrate hexahydrate, 5-20 parts of pseudo-boehmite, 0.1-2 parts of nickel nitrate hexahydrate, and 0.1-5 parts of zirconium nitrate pentahydrate in deionized water and dissolve them uniformly to obtain a first solution; 2) Weigh 10 to 40 parts of anhydrous sodium carbonate and dissolve them evenly in deionized water to obtain a second solution; 3) Mixing the first solution and the second solution at 40-90° C. to perform a coprecipitation reaction; 4) Aging the coprecipitation reaction product at 30-90° C. for 1-5 h, washing and drying to obtain a copper-based desulfurization adsorbent precursor; The binder is a mixture of pseudo-boehmite and kaolin in a mass ratio of 1: (1-3), and the extrusion aid is sesbania powder.

2. The method for forming the copper-based desulfurization adsorbent for ultra-deep thiophene removal according to claim 1, Its characteristics are The concentration of the silica sol nitric acid aqueous solution is 20-50%, and the amount used is 30-60% of the mass of the copper-based desulfurization adsorbent precursor.

3. The molding method of the copper-based desulfurization adsorbent for ultra-deep thiophene removal according to claim 1, Its characteristics are The amount of nitric acid in the silica sol nitric acid aqueous solution is 2-15% of the mass of the copper-based desulfurization adsorbent precursor.

4. The molding method of the copper-based desulfurization adsorbent for ultra-deep thiophene removal according to claim 1, Its characteristics are The kneading time is 10 to 30 minutes.

5. The molding method of the copper-based desulfurization adsorbent for ultra-deep thiophene removal according to claim 1, Its characteristics are The hole diameter of the extrusion die is 1 to 4 mm.

6. The method for forming the copper-based desulfurization adsorbent for ultra-deep thiophene removal according to claim 1, Its characteristics are The frequency speed of the extruder is 10-30r / min.

7. The molding method of the copper-based desulfurization adsorbent for ultra-deep thiophene removal according to claim 1, Its characteristics are The extruded wet material is aged in air at room temperature for not less than 4 hours and then dried.

8. The method for forming the copper-based desulfurization adsorbent for ultra-deep thiophene removal according to claim 7, Its characteristics are Dry at 100-150°C for 10-15h.

Citation Information

Patent Citations

  • Adsorption agent for reducing sulphur content of catalytic cracking production

    CN101314726A

  • Desulfurization adsorbent and preparation method and application thereof

    CN102114404A

  • Desulfuration adsorbent for catalytic gasoline as well as preparation method and application of adsorbent

    CN103551107A

  • Absorptive desulfurization agent applied to benzene and homologs

    CN107008232A

  • Sulfur dioxide adsorbent and preparation method thereof

    CN111545162A