Production method for controlling appearance quality of rectangular flat steel

Through optimized rectangular flat steel production methods, including finishing, step heating and pass rolling in the rolling process, combined with cooling bed insulation treatment, the problem of rectangular flat steel section shape control is solved and the R angle is significantly reduced. , improving the appearance quality of the product and the competitiveness of users.

CN118744153APending Publication Date: 2024-10-08WUXI XINGCHENG HUAXIN STEEL
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410688780.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-30
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

It is difficult to effectively control the four R corners of rectangular flat steel with the existing technology, especially for rectangular flat steel with a small aspect ratio. Its cross-sectional shape is difficult to control, and users have high requirements for appearance.

Method used

Through optimized production methods, including billet preparation, heat treatment, rolling and controlled cooling steps, specific steps include the use of square billets, finishing and grinding treatment, step heating, and box-hole flat rolling and vertical rolling during the rolling process , control the rolling temperature, the last pass is flat roll rolling, and a heat preservation cover is set on the cooling bed for cooling.

Benefits of technology

It effectively reduces the four R corners of the rectangular flat steel, ensuring the uniformity and consistency of the cross-sectional shape, reducing the user's subsequent processing volume, and improving the competitiveness of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118744153A_ABST
    Figure CN118744153A_ABST
Patent Text Reader

Abstract

The invention relates to a rectangular flat steel appearance quality control production method, which belongs to a rectangular flat steel hot rolling method, and comprises the following steps: blank preparation: taking a square billet as a raw material, and carrying out finishing and grinding treatment; heating is conducted, specifically, the blank is heated to 1100-1280 DEG C; rolling is conducted, rough rolling, intermediate rolling, pre-finish rolling and finish rolling are conducted in sequence, the square billet is rolled into flat steel, the initial rolling temperature ranges from 1000 DEG C to 1150 DEG C, the finish rolling temperature ranges from 830 DEG C to 1050 DEG C, box type hole flat rolling is adopted for rough rolling, box type hole vertical rolling is adopted for intermediate rolling, free rolling of flat roller flat rolling and box type hole vertical rolling is adopted for pre-finish rolling and finish rolling, and flat roller flat rolling is adopted for the last pass of finish rolling; and controlled cooling is conducted, the rolled flat steel is cut into multiple sections, then one section of flat steel is fed into a cooling bed through a roller way to be cooled, and a heat preservation cover is arranged above the cooling bed. And the appearance quality of the rectangular flat steel is improved, and the four R angles are controlled to be 0-0.5 mm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a production method of flat steel, in particular to a production method for improving the appearance quality of rectangular flat steel. Background Art

[0002] The production process of flat steel shape control mainly includes: billet preparation, heating treatment, rolling, controlled cooling, and finishing. Flat steel is produced in many specifications and small batches. Users have higher requirements for the shape of flat steel. Among all types of flat steel, rectangular flat steel is the most difficult to control, and the cross-sectional shape is more difficult to control, especially rectangular flat steel with a small aspect ratio. That is, the smaller the aspect ratio, the greater the control difficulty. The cross-sectional shape of the hot-rolled rectangular flat steel is required to be approximately rectangular, and the four R angles of the flat steel cross section should be as small as possible. See Figure 1 , Figure 2 , are cross-sectional schematic diagrams of the same specification flat steel before and after the improvement of its appearance quality. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a hot rolling production method for controlling the shape quality of rectangular flat steel in response to the above-mentioned prior art. Through the optimized production method, the technical problem of the difficulty in controlling the shape of rectangular flat steel is solved, and the four R corners of the final rectangular flat steel are reduced.

[0004] The technical solution adopted by the present invention to solve the above problem is: a production method for controlling the shape quality of rectangular flat steel, characterized in that it comprises the following steps:

[0005] S1: Billet preparation, using square billets as raw materials, and undergoing finishing and grinding treatment;

[0006] S2: heating, heating the blank to 1100-1280°C;

[0007] S3: rolling, performing rough rolling, intermediate rolling, pre-finishing rolling and finishing rolling in sequence, rolling the square billet into flat steel, the starting rolling temperature is 1000-1150°C, the final rolling temperature is 830-1050°C, the rough rolling adopts box hole flat rolling, the intermediate rolling adopts box hole vertical rolling, the pre-finishing rolling and finishing rolling adopt flat roll flat rolling and box hole vertical rolling free rolling, and the last pass of finishing rolling is flat roll flat rolling;

[0008] S4: Controlled cooling: Cut the rolled flat steel into multiple sections, and then send the sections of flat steel to the cooling bed through rollers for cooling. An insulation cover is set above the cooling bed.

[0009] Preferably, in step S1, continuous casting of square billets is used, with a specification of more than 200 cubic meters.

[0010] Preferably, in step S2, the blank is heated in a step-beam heating furnace, the blank is evenly distributed in the furnace, side-in and side-out, and step-by-step heating is performed, the heating time is ≥3 hours, and the temperature difference between the head and tail of the blank is controlled within 10°C by a burner.

[0011] Preferably, in step S3, a heat-insulating roller is arranged between rough rolling and intermediate rolling, and the intermediate rolling is headless rolling. The rough rolling and intermediate rolling are not rolled continuously, which can improve the rough rolling speed and increase the second flow rate. The box hole radius R of the rough rolling is 25 to 38 mm, which reduces the influence of the rolling heat on the cooling water of the rolling mill, and effectively ensures the head and tail temperatures in the subsequent rolling process.

[0012] Preferably, in step S3, pre-finishing rolling and finishing rolling are performed in a total of three rolling passes, which are flat roll flat rolling, box-type hole vertical rolling and flat roll flat rolling in sequence, wherein the flat roll flat rolling is free rolling, and the reduction amount of the box-type hole vertical rolling is 7 to 15 mm, ensuring the side temperature of the flat steel during the rolling process.

[0013] Preferably, in step S3, the billet is locally heated during the rolling process so that the temperature difference between the head, the middle and the tail of the billet is within 20°C, and the billet temperature is controlled at 830-1000°C during the rolling process.

[0014] Preferably, in step S3, since there are many specifications of flat steels and in consideration of continuous production, for flat steels of different thicknesses, the vertical rolling hole type before pre-finishing rolling is shared; flat steels of different specifications with a thickness difference of 2 mm share a medium rolling hole type; and flat steels of different specifications with a thickness difference of 1 mm share a rough rolling hole type.

[0015] Preferably, in step S4, the shearing length of the flat steel is 40 to 60 meters, the opening angles of the insulation covers at both ends of the cooling bed are 0 to 30°, and the opening angle of the insulation cover in the middle is 30° to 60°. The opening angle of the insulation cover can be adjusted depending on the arrangement of the flat steel on the cooling bed, the density of the arrangement, etc.

[0016] Preferably, step S5 is also included, in which the flat steel is cut into designed lengths by shears after cooling on the cooling bed, and the bundles are transported off the line by rollers. The bundles weigh less than 3 tons and are hoisted to the finished product stacking site by slings.

[0017] Compared with the prior art, the advantages of the present invention are:

[0018] 1. Heating control

[0019] (1) During the rolling process, heating and insulation are used to ensure that the temperature difference between the head, middle and tail of the rolling process is controlled within 20°C, and the rolling temperature is uniform and fluctuates little, so as to effectively ensure that the temperature is stable and the deviation is small during the rolling process, and the cross-sectional shape of the entire flat steel remains uniform.

[0020] 2. Rolling control

[0021] (1) Optimization of rough rolling pass: The radius of the rough rolling box hole is adjusted from R15-20 mm to R25-38 mm to increase the deformation of the corners and avoid the corners being affected by cooling water and causing low temperature, which leads to uneven temperature of the entire cross section of the red steel. The temperature uniformity of the entire cross section is adjusted by optimizing the rolling pass.

[0022] (2) The flat rolling of pre-finishing rolling and finishing rolling adopts free rolling, and the vertical rolling is hole-type rolling. By optimizing the vertical rolling hole type, the reduction is generally adjusted to 7-15mm to ensure the side temperature of the flat steel during the rolling process; the vertical rolling hole type before finishing rolling K3 is shared, the K2 hole with a thickness range of ±2mm is shared, and the k1 hole with a thickness range of ±1mm is shared.

[0023] (3) The rolling process adopts medium and low temperature rolling, and the rolling temperature is controlled at 830-1000℃ by means of rolling speed, cooling water in the idle section, etc.

[0024] 3. Cooling

[0025] (1) The flat steel is cooled on a cooling bed through an input roller. The cooling bed control program can realize different forms of flat steel distribution, such as empty steps and close arrangements. The cooling bed is equipped with a heat preservation cover, and the angle can be adjusted according to performance requirements.

[0026] The advantage of the present invention is that a set of shape control processes from billet to finished product is developed according to the steel type and specification, which is unique. Improving the cross-sectional shape can reduce the user's post-processing workload, and the user can achieve small deformation to process the desired product, thereby enhancing the core competitiveness of their own products. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a cross-sectional diagram of the rectangular flat steel before the shape quality is improved, with an R angle of 2.5-4mm;

[0028] Figure 2 This is a schematic diagram of the cross section of the rectangular flat steel after the appearance quality is improved, and the R angle is 0.0-0.5mm;

[0029] Figure 3 To improve the rolling pass of the front rectangular flat steel;

[0030] Figure 4 The invention improves the rolling passes of the rectangular flat steel. DETAILED DESCRIPTION

[0031] The present invention is further described in detail below in conjunction with the accompanying drawings. The embodiments are exemplary and intended to be used to explain the present invention, but should not be understood as limiting the present invention.

[0032] The flat steel shape control hot rolling production process includes the following steps:

[0033] S1: Billet preparation, using continuous casting billets as raw materials, billet cross-section 200 square, piled in square piles in the warehouse, billets are finely shaped and ground, and placed in the qualified product area after passing the finishing and grinding process.

[0034] S2: Heating treatment, send the square steel to the step heating furnace for heating, the raw materials are evenly distributed in the furnace, the heating furnace enters and exits from the side, and the heating is step-by-step. The heating temperature of rectangular flat steel 15*30mm 60Si2Mn and other spring flat steels is 1100~1180℃, the heating time is 4 hours, and the rolling temperature is 1000~1130℃. The temperature difference between the tail and the head is controlled within 10℃ through the burners at the north and south ends.

[0035] S3: rolling, through rough rolling, heating, intermediate rolling, pre-finishing rolling, finishing rolling, the square billet is rolled into flat steel, rough rolling and intermediate rolling are hole-type rolling, according to the production specifications, K1 flat rolling uses a 15-16*30 square box hole with an aspect ratio, K2 vertical rolling uses a 17-20*30 square box hole with an aspect ratio, K3 flat roll flat rolling free rolling, K4 vertical rolling uses a 22-28*35 square box hole, K5 flat roll flat rolling free rolling, rolling temperature 830-1000℃. Figure 4 shown.

[0036] S4: Controlled cooling, (1) The rolled flat steel is cut into multiple sections with a length range of 40 to 60 meters by a process flying shear, and then the sections of flat steel are conveyed to the cooling bed through a roller conveyor for cooling. There is a heat preservation cover above the cooling bed, which can be opened and closed freely. The specifications are 15mm*30mm 60Si2Mn and other spring flat steel production. The heat preservation at both ends of the cooling bed is opened at 0°~30°, and the heat preservation cover in the middle is opened at an angle of 30°~60°.

[0037] S4: controlled cooling, (2) Specifications 15*30mm 60Si2Mn and other spring flat steel production flat steel upper and lower sheets overlap, close-packed steel input.

[0038] S5: Finishing: After cooling on the cooling bed, the baled goods are cut into the length required by the user by a shearing machine, and transported to the finished product stacking site by roller conveyor. The weight of the baled goods is generally less than 3 tons, and the baled goods are hoisted to the finished product stacking site with slings. The stacking site is selected according to the season. In autumn and winter, a closed area is generally selected.

[0039] Improve the contrast of the cross-sectional shape before and after (R angle):

[0040] Specification / mm Improved front R angle size / mm Improved R angle size / mm 30 Series 2.5~3.5 0~0.5 40 Series 2.5~3.5 0~0.5 50 Series 2.5~3.5 0~0.5 60 Series 2.5~3.5 0~0.5 70 Series 2.5~3.5 0~0.5

[0041] In addition to the above embodiments, the present invention also includes other implementation modes. Any technical solutions formed by equivalent transformation or equivalent replacement should fall within the protection scope of the claims of the present invention.

Claims

1. A production method for controlling the shape quality of rectangular flat steel, characterized in that: The following steps are included S1: Billet preparation, using square billets as raw materials, and undergoing finishing and grinding treatment; S2: heating, heating the blank to 1100-1280°C; S3: rolling, rough rolling, intermediate rolling, pre-finishing rolling and finishing rolling are carried out in sequence to roll the square billet into flat steel, the starting rolling temperature is 1000-1150°C, the final rolling temperature is 830-1050°C, the rough rolling adopts box-type hole flat rolling, the intermediate rolling adopts box-type hole vertical rolling, the pre-finishing rolling and finishing rolling adopt flat roll flat rolling and box-type hole vertical rolling alternately, and the last pass of finishing rolling is flat roll flat rolling; S4: Controlled cooling: Cut the rolled flat steel into multiple sections, and then send the sections of flat steel to the cooling bed through rollers for cooling. An insulation cover is set above the cooling bed.

2. The method according to claim 1, characterized in that: Step S1, using continuous casting of square billets with a specification of more than 200 square meters.

3. The method according to claim 1, characterized in that: Step S2, the blank is put into a step-beam heating furnace for heating. The blank is evenly distributed in the furnace, and is heated from the side. The heating time is ≥ 3 hours, and the temperature difference between the head and tail of the blank is controlled within 10°C by the burner.

4. The method according to claim 1, characterized in that: Step S3, a heat-insulating roller table is arranged between the rough rolling and the intermediate rolling, the intermediate rolling is headless rolling, the rough rolling and the intermediate rolling are not rolled continuously, and the box hole radius R of the rough rolling is 25-38 mm.

5. The method according to claim 1, characterized in that: Step S3, pre-finishing rolling and finishing rolling are three rolling steps in total, which are flat roll flat rolling, box-type hole vertical rolling and flat roll flat rolling in sequence, wherein the flat roll flat rolling is free rolling, and the reduction amount of the box-type hole vertical rolling is 7 to 15 mm.

6. The method according to claim 1, characterized in that: Step S3, locally heating the billet during rolling so that the temperature difference between the head, the middle and the tail of the billet is within 20°C, and controlling the billet temperature at 830-1000°C during rolling.

7. The method according to claim 1, characterized in that: Step S3, for flat steels of different thicknesses, the vertical rolling pass before pre-finishing rolling is shared; flat steels of different specifications with a thickness difference of 2 mm share the intermediate rolling pass; and flat steels of different specifications with a thickness difference of 1 mm share the rough rolling pass.

8. The method according to claim 1, characterized in that: Step S4, the shearing length of the flat steel is 40 to 60 meters, the opening angles of the heat preservation covers at both ends of the cooling bed are 0 to 30 degrees, and the opening angle of the heat preservation cover in the middle is 30 degrees to 60 degrees.

9. The method according to claim 1, characterized in that: The step S5 is also included, in which the flat steel is cut into designed lengths by shears after cooling on the cooling bed, and bundled off the line by roller conveyors. The bundled weight is less than 3 tons, and the bundles are hoisted to the finished product stacking site by slings.

Citation Information

Patent Citations

  • Rolling device and method for flat-bulb steel

    CN107803401A

  • Hot rolling wire rod production method for improving surface quality

    CN110125177A

  • High-precision right-angle flat steel continuous rolling process method

    CN110560481A

  • Method for producing high-accuracy cathode flat steel by universal rolling mill

    CN111604371A

  • Rolling and cooling method for flat spring steel

    CN112893490A