Method for improving stability of surface structure of cobalt-free manganese positive electrode material
By introducing the spinel structure LiMn2O4 phase and forming a layered spinel structure composite material, the problem of insufficient surface structure stability of cobalt-free manganese cathode materials is solved, the electrochemical performance and rate performance are significantly improved, and a more ideal Use effect.
Patent Information
- Application Number
- CN202410996619.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-08
AI Technical Summary
The surface structure stability of the existing cobalt-free manganese cathode materials is not high, which makes it difficult to maintain the electrochemical performance during the cycle and the use effect is not ideal.
The spinel structure LiMn2O4 phase is introduced, and the layered spinel structure composite material is formed through autoclave treatment, which increases the lithium ion diffusion rate and alleviates the capacity loss caused by irreversible decomposition.
It significantly improves the surface structure stability and electrochemical performance of cobalt-free manganese cathode materials, improves rate performance and first Coulomb efficiency, and ensures high cycle performance.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of cobalt-free manganese-based positive electrode materials, and more specifically, to a method for improving the surface structure stability of cobalt-free manganese-based positive electrode materials. Background Art
[0002] Cobalt-free manganese-based positive electrode material is an important positive electrode material for lithium-ion batteries. Its main feature is that it does not contain cobalt elements at all. Due to the absence of cobalt elements, cobalt-free manganese-based positive electrode materials have significant cost advantages over traditional cobalt-containing materials. Because cobalt is a scarce and expensive metal, the surface structure stability of existing cobalt-free manganese-based positive electrode materials is not high enough, and high electrochemical performance cannot be maintained during the cycle process, and the actual use effect is not ideal.
[0003] Therefore, there is an urgent need for a method for improving the surface structure stability of cobalt-free manganese-based positive electrode materials to solve the above problems. Summary of the invention
[0004] In order to overcome the above-mentioned defects of the prior art, an embodiment of the present invention provides a method for improving the surface structure stability of a cobalt-free manganese-based positive electrode material. The cobalt-free manganese-based positive electrode material produced by the present invention has high surface structure stability, can maintain high electrochemical performance during the cycle process, and has a relatively ideal actual use effect. The introduction of the spinel structure LiMn2O4 phase can effectively improve the rate performance and the first coulombic efficiency of the lithium-rich manganese-based material, because the three-dimensional lithium ion diffusion channel in the spinel structure can greatly increase the diffusion rate of Li+ and improve its rate performance. At the same time, the 16c octahedral vacancies in the spinel structure can accommodate more Li+ during the first discharge process to alleviate the large capacity loss caused by the irreversible decomposition of Li2MnO3 during the first week of activation, so as to solve the problems raised in the above-mentioned background technology.
[0005] To achieve the above object, the present invention provides the following technical solution: a method for improving the surface structure stability of a cobalt-free manganese-based positive electrode material, comprising the following steps:
[0006] Step (1): preparing the required lithium salt, manganese salt, nickel salt and cobalt salt as well as additives and dopants, and ensuring that the purity and stoichiometric ratio of the raw materials meet the requirements;
[0007] Step (2): mixing the prepared lithium salt, manganese salt, nickel salt and cobalt salt as well as additives and dopants, and adding an appropriate amount of organic solvent to form a uniform reaction precursor solution;
[0008] Step (3): transferring the precursor solution to an autoclave, and treating the precursor solution using the autoclave, with a reaction temperature of 160° C. and a reaction time of 10 h;
[0009] Step (4): then introducing an appropriate amount of spinel structure LiMn2O4 phase into the autoclave to uniformly mix the spinel structure LiMn2O4 phase with the precursor solution, and then using the autoclave again to treat the mixed solution of the precursor solution and the spinel structure LiMn2O4 phase, the reaction temperature is 180°C, and the reaction time is 8h;
[0010] Step (5): taking out the product after the reaction, and obtaining a layered spinel structure composite material;
[0011] Step (6): characterizing the layered spinel structure composite material by X-ray diffraction (XRD), scanning electron microscopy (SEM) and transmission electron microscopy (TEM) to confirm the crystal structure, morphology and element distribution of the layered spinel structure composite material;
[0012] Step (7): The electrochemical performance of the layered spinel structure composite material is tested by charge and discharge test, cycle performance test and rate performance test to confirm the electrochemical performance of the layered spinel structure composite material.
[0013] In a preferred embodiment, the lithium salt in step (1) is LiOH, and the manganese salt in step (1) is MnO2.
[0014] In a preferred embodiment, the nickel salt in step (1) is Ni(NO3)2, and the cobalt salt in step (1) is Co(NO3)2.
[0015] In a preferred embodiment, the additive in step (1) includes an oxidant and a pH adjuster.
[0016] In a preferred embodiment, the dopant in step (1) includes Al, Mg and Cr.
[0017] In a preferred embodiment, the organic solvent in step (2) is ethylene glycol.
[0018] Technical effects and advantages of the present invention:
[0019] The present invention first prepares the required lithium salt, manganese salt, nickel salt and cobalt salt as well as additives and dopants, and ensures that the purity and stoichiometric ratio of the raw materials meet the requirements, then mixes the prepared lithium salt, manganese salt, nickel salt and cobalt salt as well as the additives and dopants, and adds an appropriate amount of organic solvent to form a uniform reaction precursor solution, transfers the precursor solution to an autoclave, and uses the autoclave to treat the precursor solution at a reaction temperature of 160° C. for a reaction time of 10 hours, then introduces an appropriate amount of spinel structure LiMn2O4 phase into the autoclave to uniformly mix the spinel structure LiMn2O4 phase with the precursor solution, and then uses the autoclave again to treat the precursor solution and the mixed solution of the spinel structure LiMn2O4 phase at a reaction temperature of 180° C. for a reaction time of 8 hours, and takes out the product after the reaction to obtain a layered spinel structure composite material, which is characterized by X-ray diffraction (XRD), scanning electron microscopy (SEM) and transmission electron microscopy. (TEM) is used to characterize the layered spinel structure composite material to confirm the crystal structure, morphology and element distribution of the layered spinel structure composite material. The electrochemical properties of the layered spinel structure composite material are tested by charge and discharge test, cycle performance test and rate performance test to confirm the electrochemical properties of the layered spinel structure composite material. The cobalt-free manganese-based positive electrode material produced by the present invention has high surface structure stability, can maintain high electrochemical performance during the cycle process, and has a relatively ideal actual use effect. The introduction of the spinel structure LiMn2O4 phase can effectively improve the rate performance and the first coulomb efficiency of the lithium-rich manganese-based material, because the three-dimensional lithium ion diffusion channel in the spinel structure can greatly increase the diffusion rate of Li+ and improve its rate performance. At the same time, the 16c octahedral vacancies in the spinel structure can accommodate more Li+ during the first discharge process to alleviate the large capacity loss caused by the irreversible decomposition of Li2MnO3 during the first week of activation. DETAILED DESCRIPTION
[0020] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] Example 1
[0022] The present invention provides a method for improving the surface structure stability of a cobalt-free manganese-based positive electrode material, comprising the following steps:
[0023] Step (1): preparing the required lithium salt, manganese salt, nickel salt and cobalt salt as well as additives and dopants, and ensuring that the purity and stoichiometric ratio of the raw materials meet the requirements;
[0024] Step (2): mixing the prepared lithium salt, manganese salt, nickel salt and cobalt salt as well as additives and dopants, and adding an appropriate amount of organic solvent to form a uniform reaction precursor solution;
[0025] Step (3): transferring the precursor solution to an autoclave, and treating the precursor solution using the autoclave, with a reaction temperature of 160° C. and a reaction time of 10 h;
[0026] Step (4): then introducing an appropriate amount of spinel structure LiMn2O4 phase into the autoclave to uniformly mix the spinel structure LiMn2O4 phase with the precursor solution, and then using the autoclave again to treat the mixed solution of the precursor solution and the spinel structure LiMn2O4 phase, the reaction temperature is 180°C, and the reaction time is 8h;
[0027] Step (5): taking out the product after the reaction, and obtaining a layered spinel structure composite material;
[0028] Step (6): characterizing the layered spinel structure composite material by X-ray diffraction (XRD), scanning electron microscopy (SEM) and transmission electron microscopy (TEM) to confirm the crystal structure, morphology and element distribution of the layered spinel structure composite material;
[0029] Step (7): The electrochemical performance of the layered spinel structure composite material is tested by charge and discharge test, cycle performance test and rate performance test to confirm the electrochemical performance of the layered spinel structure composite material.
[0030] The lithium salt in step (1) is set to LiOH, and the manganese salt in step (1) is set to MnO2.
[0031] The nickel salt in step (1) is set to Ni(NO3)2, and the cobalt salt in step (1) is set to Co(NO3)2.
[0032] The additives in step (1) include an oxidant and a pH adjuster.
[0033] The dopant in step (1) includes Al, Mg and Cr.
[0034] The organic solvent in step (2) is set to ethylene glycol.
[0035] The present invention first prepares the required lithium salt, manganese salt, nickel salt and cobalt salt as well as additives and dopants, and ensures that the purity and stoichiometric ratio of the raw materials meet the requirements, then mixes the prepared lithium salt, manganese salt, nickel salt and cobalt salt as well as the additives and dopants, and adds an appropriate amount of organic solvent to form a uniform reaction precursor solution, transfers the precursor solution to an autoclave, and uses the autoclave to treat the precursor solution at a reaction temperature of 160° C. for a reaction time of 10 hours, then introduces an appropriate amount of spinel structure LiMn2O4 phase into the autoclave to uniformly mix the spinel structure LiMn2O4 phase with the precursor solution, and then uses the autoclave again to treat the precursor solution and the mixed solution of the spinel structure LiMn2O4 phase at a reaction temperature of 180° C. for a reaction time of 8 hours, and takes out the product after the reaction to obtain a layered spinel structure composite material, which is characterized by X-ray diffraction (XRD), scanning electron microscopy (SEM) and transmission electron microscopy. (TEM) is used to characterize the layered spinel structure composite material to confirm the crystal structure, morphology and element distribution of the layered spinel structure composite material. The electrochemical properties of the layered spinel structure composite material are tested by charge and discharge test, cycle performance test and rate performance test to confirm the electrochemical properties of the layered spinel structure composite material. The cobalt-free manganese-based positive electrode material produced by the present invention has high surface structure stability, can maintain high electrochemical performance during the cycle process, and has a relatively ideal actual use effect. The introduction of the spinel structure LiMn2O4 phase can effectively improve the rate performance and the first coulomb efficiency of the lithium-rich manganese-based material, because the three-dimensional lithium ion diffusion channel in the spinel structure can greatly increase the diffusion rate of Li+ and improve its rate performance. At the same time, the 16c octahedral vacancies in the spinel structure can accommodate more Li+ during the first discharge process to alleviate the large capacity loss caused by the irreversible decomposition of Li2MnO3 during the first week of activation.
[0036] Finally: The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for improving the surface structure stability of cobalt-free manganese-based positive electrode materials, It is characterized in that The following steps are involved: Step (1): preparing the required lithium salt, manganese salt, nickel salt and cobalt salt as well as additives and dopants, and ensuring that the purity and stoichiometric ratio of the raw materials meet the requirements; Step (2): mixing the prepared lithium salt, manganese salt, nickel salt and cobalt salt as well as additives and dopants, and adding an appropriate amount of organic solvent to form a uniform reaction precursor solution; Step (3): transferring the precursor solution to an autoclave, and treating the precursor solution using the autoclave, with a reaction temperature of 160° C. and a reaction time of 10 h; Step (4): Then introduce an appropriate amount of spinel structure LiMn into the autoclave 2 O 4 phase, making the spinel structure LiMn 2 O 4 The phase was uniformly mixed with the precursor solution, and then the precursor solution and the spinel structure LiMn were subjected to autoclave again. 2 O 4 The mixed solution of the phases was treated at a reaction temperature of 180°C and a reaction time of 8h; Step (5): taking out the product after the reaction, and obtaining a layered spinel structure composite material; Step (6): characterizing the layered spinel structure composite material by X-ray diffraction (XRD), scanning electron microscopy (SEM) and transmission electron microscopy (TEM) to confirm the crystal structure, morphology and element distribution of the layered spinel structure composite material; Step (7): The electrochemical performance of the layered spinel structure composite material is tested by charge and discharge test, cycle performance test and rate performance test to confirm the electrochemical performance of the layered spinel structure composite material.
2. A method for improving the surface structure stability of a cobalt-free manganese-based positive electrode material according to claim 1, Features: The lithium salt in step (1) is set to LiOH, and the manganese salt in step (1) is set to MnO 2 .
3. A method for improving the surface structure stability of a cobalt-free manganese-based positive electrode material according to claim 1, Features: The nickel salt in step (1) is set to Ni(NO 3 ) 2 The cobalt salt in step (1) is set to Co(NO 3 ) 2 .
4. A method for improving the surface structure stability of a cobalt-free manganese-based positive electrode material according to claim 1, Features: The additives in step (1) include an oxidant and a pH adjuster.
5. A method for improving the surface structure stability of a cobalt-free manganese-based positive electrode material according to claim 1, Features: The dopant in step (1) includes Al, Mg and Cr.
6. A method for improving the surface structure stability of a cobalt-free manganese-based positive electrode material according to claim 1, Features: The organic solvent in step (2) is set to ethylene glycol.