Transparent slurry similar simulation material and preparation method thereof

The transparent mud similar simulation material prepared by polyacrylamide, alkali metal salts and rheology modifiers solves the problem that the density, plastic viscosity and yield stress in the existing technology are difficult to approach the real drilling mud, and realizes the density, plastic viscosity and yield stress. The stress is close to the effect of real drilling mud and is suitable for drilling cuttings migration simulation tests.

CN118745337APending Publication Date: 2024-10-08SICHUAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410731025.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

When existing transparent mud materials simulate real drilling mud, the density, plastic viscosity and yield stress are difficult to approach the real drilling mud at the same time, resulting in poor cuttings migration simulation test results.

Method used

Polyacrylamide, alkali metal salts and rheology regulators are used to prepare similar simulation materials for transparent mud. By adjusting the proportion of raw materials and stirring conditions, a transparent mud with density, plastic viscosity and yield stress close to that of real drilling mud is prepared, including polyacrylamide 0.1 -1%, alkali metal salt 5-30%, rheology regulator 0.2-2%, the balance is water, the stirring time and speed can be adjusted to achieve the best effect.

Benefits of technology

A transparent mud with a density, plastic viscosity and yield stress close to that of real drilling mud is achieved, which is suitable for drilling cuttings migration model tests and improves the accuracy and observability of simulation tests.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745337A_ABST
    Figure CN118745337A_ABST
Patent Text Reader

Abstract

The invention discloses a transparent slurry similar simulation material and a preparation method thereof, and belongs to the technical field of drilling engineering. The transparent slurry similar simulation material is prepared from the following raw materials in percentage by weight: 0.1 to 1 percent of polyacrylamide, 5 to 30 percent of alkali metal salt, 0.2 to 2 percent of rheological property regulator and the balance of water. The invention provides a method for preparing a transparent slurry material from polyacrylamide, water, metal salt and nanocellulose, the transparent slurry similar simulation material prepared by the method can simulate real drilling slurry with the density of 1-1.2 g / cm < 3 > and the dynamic-plastic ratio of 0.36-0.48 in an approximate 1: 1 manner, is completely transparent, is a non-Newtonian fluid, and can be applied to the field of drilling fluid. The plastic viscosity, the yield stress, the mud density and the like are very close to those of real drilling mud, the performance of the real drilling mud can be reasonably simulated, and the migration condition of rock debris can be conveniently and visually observed in a drilling experiment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of drilling engineering, and in particular to a transparent mud similar simulation material and a preparation method thereof. Background Art

[0002] In oil and gas resource drilling, cuttings transport efficiency is an important factor affecting drilling efficiency and safety. Large-scale cuttings transport physical simulation test is the main method to evaluate key parameters such as mud return rate, circulating pressure loss, mechanical drilling rate, cuttings return rate, cuttings bed thickness under different well inclination conditions.

[0003] Effectively controlling the movement of cuttings can improve drilling efficiency and ensure drilling safety. If the cuttings are completely transported out of the wellbore during drilling, the cuttings will not accumulate at the bottom of the wellbore or the lower part of the high-angle well to form a cuttings bed. This will reduce the repeated grinding of the drill bit by the cuttings, increase the drilling speed, and reduce the wear of the drilling tool by the cuttings bed, reducing the drilling resistance. In-depth research and understanding of the movement of cuttings in the wellbore circulating mud will help optimize the design of drilling parameters, maximize the drilling speed, and reduce engineering risks and costs.

[0004] In the cuttings transport simulation test, digital imaging technology is usually needed to analyze and evaluate the cuttings transport status. The visualization of drilling tools and mud becomes a prerequisite for the smooth conduct of the simulation test. At present, the transparent mud material used in the cuttings transport simulation test is mainly prepared by polyacrylamide and water. Compared with the real drilling mud, although it has a certain yield stress and plastic viscosity, the mud density is generally close to 1.0g / cm 3 , which is significantly lower than the real drilling mud. Mud density is an important factor affecting drilling hydraulic parameters such as cuttings transport, circulating mud pressure loss, and mud return rate. Without considering transparent mud materials with similar density, it is difficult to simulate the real drilling mud to obtain the state of cuttings transport. Therefore, transparent mud with key parameters such as density, plastic viscosity, and yield stress similar to those of real drilling mud is the prerequisite for scientific cuttings transport simulation experiments. Summary of the invention

[0005] In order to solve the above technical problems, the main purpose of the present invention is to provide a transparent mud similar simulation material and a preparation method thereof, so as to achieve density, plastic viscosity and yield stress similar to those of real drilling mud, so as to solve the problem that transparent mud is difficult to simulate real drilling mud in current cuttings transport simulation test research.

[0006] The technical solution of the present invention to solve the above technical problems is as follows:

[0007] A transparent mud-like simulation material comprises the following raw materials in percentage by weight:

[0008] Polyacrylamide 0.1-1%, alkali metal salt 5-30%, rheology regulator 0.2-2%, and the balance is water.

[0009] The beneficial effects of the present invention are as follows: the present invention uses polyacrylamide, alkali metal salt, rheology regulator and water as raw materials to prepare a transparent mud similar simulation material, and the prepared transparent mud material is almost completely transparent, and the plastic viscosity, yield stress and mud density can be simultaneously consistent with the density of 1-1.2g / cm 3 The present invention is very close to the real drilling mud with a dynamic-plastic ratio of 0.36-0.48, and can effectively simulate the real drilling mud for drilling cuttings transport model test. Since the mud is almost completely transparent, it is convenient to use images or video data to visually observe the state of cuttings transport. At the same time, the present invention can also adjust the raw material components and proportions according to actual conditions to simulate real drilling muds of different densities.

[0010] Preferably, the following raw materials are included in weight percentage:

[0011] Polyacrylamide 0.5%, metal salt 26%, nanocellulose 0.45%, and the balance is water.

[0012] Furthermore, the molecular weight of polyacrylamide is 7 million to 25 million.

[0013] Preferably, the molecular weight of polyacrylamide is 10 million.

[0014] Furthermore, the alkali metal salt is any one of sodium chloride, potassium chloride, magnesium chloride, calcium chloride, barium chloride, sodium carbonate, potassium carbonate, sodium sulfate and potassium sulfate.

[0015] Preferably, the alkali metal salt is sodium chloride.

[0016] The beneficial effect of adopting the above-mentioned further technical scheme is: the present application uses sodium chloride as an alkali metal salt and adds it to the polyacrylamide solution, which acts as a weighting agent while not affecting the transparency, effectively increasing the density of the solution to make it close to the density standard of the real drilling mud, and can also adjust the plastic viscosity.

[0017] Furthermore, the rheology regulator is any one of sodium hydroxymethylcellulose, hydroxyethyl nanocellulose, hydroxypropyl nanocellulose, methyl allyl polyoxyethylene ether and triethanolamine.

[0018] The beneficial effect of adopting the above further technical scheme is: the present invention can effectively change the cross-linking density of the polyacrylamide network by adding a rheology regulator, thereby adjusting the yield stress and plastic viscosity of the solution, and making the yield stress and plastic viscosity closer to the standard of real drilling mud while ensuring the density and transparency of the solution.

[0019] Preferably, the rheology modifier is hydroxyethyl nanocellulose.

[0020] The preparation method of the transparent mud-like simulation material comprises the following steps: dissolving polyacrylamide in water, adding alkali metal salt and rheology regulator, and stirring to obtain the transparent mud-like simulation material.

[0021] Furthermore, the stirring speed is 300-900 rpm, and the time is 1-5 h.

[0022] Preferably, the stirring speed is 600 rpm and the time is 3 h.

[0023] The beneficial effects of adopting the above-mentioned further technical scheme are: the preparation method of the present application is simple, the preparation efficiency is high, no large-scale precision instruments are required, it is suitable for large-scale preparation, and it is more conducive to meeting the needs of simulating real drilling mud for large-scale experimental research.

[0024] The transparent mud similarity simulation material is used in simulating real drilling mud.

[0025] The present invention has the following beneficial effects:

[0026] The present invention provides a method for preparing a transparent mud material by using polyacrylamide, water, alkali metal salt and rheology regulator, which can simulate the density of 1-1.2 g / cm 3 The transparent mud material prepared by this method is almost completely transparent and is a non-Newtonian fluid. Its main parameters such as plastic viscosity, yield stress and density are very close to those of real drilling mud. It can effectively simulate the performance of real drilling mud and facilitate the intuitive observation of cuttings migration in the drilling cuttings migration model test. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The results of the effect of the amount of sodium chloride added on the density of the transparent mud-like simulated material in Test Example 2;

[0028] Figure 2 The results of the effect of PAM molecular weight on the plastic viscosity of the transparent mud-like simulation material in Test Example 3;

[0029] Figure 3 The results of the effect of PAM molecular weight on the yield stress of the transparent mud-like simulated material in Experimental Example 3;

[0030] Figure 4 The results of the effect of PAM addition on the plastic viscosity of the transparent mud-like simulation material in Test Example 3;

[0031] Figure 5 The results of the effect of PAM addition on the yield stress of the transparent mud-like simulated material in Experimental Example 3. DETAILED DESCRIPTION

[0032] The principles and features of the present invention are described below. The examples are only used to explain the present invention and are not used to limit the scope of the present invention. If no specific conditions are specified in the examples, the experiment is carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. With a density of 1.16 g / cm 3 The specific implementation method is introduced by taking the drilling mud as an example.

[0033] Embodiment 1:

[0034] A transparent mud-like simulation material comprises the following raw materials in percentage by weight:

[0035] Polyacrylamide (molecular weight 10 million) 0.5%, sodium chloride 26%, hydroxyethyl nanocellulose 0.4%, and the balance is water.

[0036] The preparation method comprises the following steps:

[0037] (1) Add polyacrylamide into water and stir at 600 rpm for 3 h to fully dissolve to obtain a polyacrylamide aqueous solution;

[0038] (2) Sodium chloride and hydroxyethyl nanocellulose were added to the polyacrylamide aqueous solution, and the mixture was stirred at 600 rpm for 3 h to obtain a transparent mud-like simulation material.

[0039] Embodiment 2:

[0040] A transparent mud-like simulation material comprises the following raw materials in percentage by weight:

[0041] Polyacrylamide (molecular weight 10 million) 0.5%, sodium chloride 26%, hydroxyethyl nanocellulose 0.45%, and the balance is water.

[0042] The preparation method comprises the following steps:

[0043] (1) Add polyacrylamide into water and stir at 600 rpm for 3 h to fully dissolve to obtain a polyacrylamide aqueous solution;

[0044] (2) Sodium chloride and hydroxyethyl nanocellulose were added to the polyacrylamide aqueous solution, and the mixture was stirred at 600 rpm for 3 h to obtain a transparent mud-like simulation material.

[0045] Embodiment 3:

[0046] A transparent mud-like simulation material comprises the following raw materials in percentage by weight:

[0047] Polyacrylamide (molecular weight 10 million) 0.5%, sodium chloride 26%, hydroxyethyl nanocellulose 0.50%, and the balance is water.

[0048] The preparation method comprises the following steps:

[0049] (1) Add polyacrylamide into water and stir at 600 rpm for 3 h to fully dissolve to obtain a polyacrylamide aqueous solution;

[0050] (2) Sodium chloride and hydroxyethyl nanocellulose were added to the polyacrylamide aqueous solution, and the mixture was stirred at 600 rpm for 3 h to obtain a transparent mud-like simulation material.

[0051] Embodiment 4:

[0052] A transparent mud-like simulation material comprises the following raw materials in percentage by weight:

[0053] Polyacrylamide (molecular weight 10 million) 0.5%, sodium chloride 26%, sodium hydroxymethyl cellulose 0.5%, and the balance is water.

[0054] The preparation method comprises the following steps:

[0055] (1) Add polyacrylamide into water and stir at 600 rpm for 3 h to fully dissolve to obtain a polyacrylamide aqueous solution;

[0056] (2) Sodium chloride and sodium hydroxymethyl cellulose were added to the polyacrylamide aqueous solution, and the mixture was stirred at 600 rpm for 3 h to obtain a transparent mud-like simulation material.

[0057] Embodiment 5:

[0058] A transparent mud-like simulation material comprises the following raw materials in percentage by weight:

[0059] Polyacrylamide (molecular weight 10 million) 0.5%, sodium chloride 26%, sodium hydroxymethyl cellulose 1%, and the balance is water.

[0060] The preparation method comprises the following steps:

[0061] (1) Add polyacrylamide into water and stir at 600 rpm for 3 h to fully dissolve to obtain a polyacrylamide aqueous solution;

[0062] (2) Sodium chloride and sodium hydroxymethyl cellulose were added to the polyacrylamide aqueous solution, and the mixture was stirred at 600 rpm for 3 h to obtain a transparent mud-like simulation material.

[0063] Embodiment 6:

[0064] A transparent mud-like simulation material comprises the following raw materials in percentage by weight:

[0065] Polyacrylamide (molecular weight 10 million) 0.5%, sodium chloride 26%, sodium hydroxymethyl cellulose 1.5%, and the balance is water.

[0066] The preparation method comprises the following steps:

[0067] (1) Add polyacrylamide into water and stir at 600 rpm for 3 h to fully dissolve to obtain a polyacrylamide aqueous solution;

[0068] (2) Sodium chloride and sodium hydroxymethyl cellulose were added to the polyacrylamide aqueous solution, and the mixture was stirred at 600 rpm for 3 h to obtain a transparent mud-like simulation material.

[0069] Embodiment 7:

[0070] A transparent mud-like simulation material comprises the following raw materials in percentage by weight:

[0071] Polyacrylamide (molecular weight 10 million) 0.5%, sodium chloride 26%, hydroxypropyl nanocellulose 0.5%, and the balance is water.

[0072] The preparation method comprises the following steps:

[0073] (1) Add polyacrylamide into water and stir at 600 rpm for 3 h to fully dissolve to obtain a polyacrylamide aqueous solution;

[0074] (2) Sodium chloride and hydroxypropyl nanocellulose were added to the polyacrylamide aqueous solution, and the mixture was stirred at 600 rpm for 3 h to obtain a transparent mud-like simulation material.

[0075] Embodiment 8:

[0076] A transparent mud-like simulation material comprises the following raw materials in percentage by weight:

[0077] Polyacrylamide (molecular weight 10 million) 0.5%, sodium chloride 26%, hydroxypropyl nanocellulose 1%, and the balance is water.

[0078] The preparation method comprises the following steps:

[0079] (1) Add polyacrylamide into water and stir at 600 rpm for 3 h to fully dissolve to obtain a polyacrylamide aqueous solution;

[0080] (2) Sodium chloride and hydroxypropyl nanocellulose were added to the polyacrylamide aqueous solution, and the mixture was stirred at 600 rpm for 3 h to obtain a transparent mud-like simulation material.

[0081] Embodiment 9:

[0082] A transparent mud-like simulation material comprises the following raw materials in percentage by weight:

[0083] Polyacrylamide (molecular weight 10 million) 0.5%, sodium chloride 26%, hydroxypropyl nanocellulose 1.5%, and the balance is water.

[0084] The preparation method comprises the following steps:

[0085] (1) Add polyacrylamide into water and stir at 600 rpm for 3 h to fully dissolve to obtain a polyacrylamide aqueous solution;

[0086] (2) Sodium chloride and hydroxypropyl nanocellulose were added to the polyacrylamide aqueous solution, and the mixture was stirred at 600 rpm for 3 h to obtain a transparent mud-like simulation material.

[0087] Comparative Example 1:

[0088] A transparent mud-like simulation material comprises the following raw materials in percentage by weight:

[0089] Polyacrylamide (molecular weight 10 million) 0.5%, sodium chloride 26%, and the balance is water.

[0090] The preparation method comprises the following steps:

[0091] (1) Add polyacrylamide into water and stir at 600 rpm for 3 h to fully dissolve to obtain a polyacrylamide aqueous solution;

[0092] (2) Sodium chloride was added to the polyacrylamide aqueous solution and stirred at 600 rpm for 3 h to fully mix the mixture. The transparent mud was similar to the simulated material.

[0093] Comparative Example 2:

[0094] A transparent mud-like simulation material comprises the following raw materials in percentage by weight:

[0095] Polyacrylamide (molecular weight 10 million) 0.5%, sodium chloride 26%, hydroxyethyl nanocellulose 0.1%, and the balance is water.

[0096] The preparation method comprises the following steps:

[0097] (1) Add polyacrylamide into water and stir at 600 rpm for 3 h to fully dissolve to obtain a polyacrylamide aqueous solution;

[0098] (2) Sodium chloride and hydroxyethyl nanocellulose were added to the polyacrylamide aqueous solution, and stirring was continued at 600 rpm for 3 h to fully mix, and a transparent mud similar to the simulated material was obtained.

[0099] Comparative Example 3:

[0100] A transparent mud-like simulation material comprises the following raw materials in percentage by weight:

[0101] Polyacrylamide (molecular weight 10 million) 0.5%, sodium chloride 26%, hydroxyethyl nanocellulose 3%, and the balance is water.

[0102] The preparation method comprises the following steps:

[0103] (1) Add polyacrylamide into water and stir at 600 rpm for 3 h to fully dissolve to obtain a polyacrylamide aqueous solution;

[0104] (2) Sodium chloride and hydroxyethyl nanocellulose were added to the polyacrylamide aqueous solution, and stirring was continued at 600 rpm for 3 h to fully mix, and a transparent mud similar to the simulated material was obtained.

[0105] Comparative Example 4:

[0106] A transparent mud-like simulation material comprises the following raw materials in percentage by weight:

[0107] Polyacrylamide (molecular weight 10 million) 0.5%, sodium chloride 26%, sodium hydroxymethyl cellulose 0.1%, and the balance is water.

[0108] The preparation method comprises the following steps:

[0109] (1) Add polyacrylamide into water and stir at 600 rpm for 3 h to fully dissolve to obtain a polyacrylamide aqueous solution;

[0110] (2) Sodium chloride and sodium hydroxymethyl cellulose were added to the polyacrylamide aqueous solution, and the mixture was stirred at 600 rpm for 3 h to obtain a transparent slurry similar to the simulated material.

[0111] Comparative Example 5:

[0112] A transparent mud-like simulation material comprises the following raw materials in percentage by weight:

[0113] Polyacrylamide (molecular weight 10 million) 0.5%, sodium chloride 26%, sodium hydroxymethyl cellulose 3%, and the balance is water.

[0114] The preparation method comprises the following steps:

[0115] (1) Add polyacrylamide into water and stir at 600 rpm for 3 h to fully dissolve to obtain a polyacrylamide aqueous solution;

[0116] (2) Sodium chloride and sodium hydroxymethyl cellulose were added to the polyacrylamide aqueous solution, and the mixture was stirred at 600 rpm for 3 h to obtain a transparent slurry similar to the simulated material.

[0117] Comparative Example 6:

[0118] A transparent mud-like simulation material comprises the following raw materials in percentage by weight:

[0119] Polyacrylamide (molecular weight 10 million) 0.5%, sodium chloride 26%, hydroxypropyl nanocellulose 0.1%, and the balance is water.

[0120] The preparation method comprises the following steps:

[0121] (1) Add polyacrylamide into water and stir at 600 rpm for 3 h to fully dissolve to obtain a polyacrylamide aqueous solution;

[0122] (2) Sodium chloride and hydroxypropyl nanocellulose were added to the polyacrylamide aqueous solution, and stirring was continued at 600 rpm for 3 h to fully mix, and a transparent mud similar to the simulated material was obtained.

[0123] Comparative Example 7:

[0124] A transparent mud-like simulation material comprises the following raw materials in percentage by weight:

[0125] Polyacrylamide (molecular weight 10 million) 0.5%, sodium chloride 26%, hydroxypropyl nanocellulose 3%, and the balance is water.

[0126] The preparation method comprises the following steps:

[0127] (1) Add polyacrylamide into water and stir at 600 rpm for 3 h to fully dissolve to obtain a polyacrylamide aqueous solution;

[0128] (2) Sodium chloride and hydroxypropyl nanocellulose were added to the polyacrylamide aqueous solution, and stirring was continued at 600 rpm for 3 h to fully mix, and a transparent mud similar to the simulated material was obtained.

[0129] Test example: Performance characterization

[0130] The transparent mud similar to the simulated material prepared in Examples 1-9 and Comparative Examples 1-7 was used for the experiment, and a density of 1.16 g / cm 3 Real drilling mud (formula ratio: water 1000g, soil powder 300g, soda ash 10g, caustic soda 30g, polyanionic cellulose 100g, xanthan gum 5g, IND-30 admixture 10g and barite 1800g) was used as a comparison; the plastic viscosity and yield stress were tested and analyzed using a NXS-11B rotational viscometer, and the density was measured using an XYM-3 liquid densitometer. The experimental results are shown in Table 1.

[0131] Table 1 Rheological properties of transparent mud similar simulation materials (temperature 20°C)

[0132]

[0133] According to the data in the above table, the density, plastic viscosity and yield stress of the transparent mud similar material prepared by the present application with polyacrylamide, sodium chloride, nanocellulose and water as raw materials are very close to the parameters of the real drilling mud, and the deviation does not exceed 10%. The main reason is that the soluble alkali metal salt can be completely dissolved in the polyacrylamide solution, improve the solution density, and maintain high transparency; the introduction of nanocellulose can change the cross-linking density of the polymer network and then adjust the yield stress and plastic viscosity of the solution. In the embodiment of the present application, sodium hydroxymethyl cellulose, hydroxyethyl nanocellulose and hydroxypropyl nanocellulose effectively play a thickening role through hydration and entanglement between molecules, and improve the plastic viscosity of the solution. At the same time, through the aggregation effect itself, a dense structure is formed, and hydrogen bonding is simultaneously generated between the molecules and the water molecules, which effectively increases the adhesive effect between the solutions and increases the yield stress of the solution.

[0134] According to the comparison of parameters between the embodiment and the comparative example, when the amount of nanocellulose added is too low, the plastic viscosity and yield stress will be low, which is far lower than the level of real drilling mud; and when the amount of nanocellulose added is too high, the plastic viscosity and yield stress will increase significantly, which is far higher than the level of real drilling mud, and it is difficult to simulate the performance of real drilling mud. 3 The parameters of the actual drilling mud are closest and it is the best embodiment under the given conditions of this application.

[0135] Test Example 2: Effect of sodium chloride addition on the density of transparent mud-like simulated materials

[0136] Transparent mud-like simulation materials were prepared by the formula and preparation method in Example 2, except that the addition amount of sodium chloride was changed to 5%, 10%, 15%, 25% and 30% respectively, and the density was measured using an XYM-3 liquid densitometer.

[0137] The experimental results are as follows Figure 1 shown.

[0138] according to Figure 1 The experimental results show that the present invention can achieve a 1:1 simulated density of 1-1.2 g / cm by adjusting the amount of alkali metal salt sodium chloride added. 3 The real drilling mud realizes the adjustable density performance of transparent mud-like simulation materials, which can meet the simulation experiment needs of drilling mud at different densities.

[0139] Test Example 3: Effect of PAM molecular weight and addition amount on plastic viscosity and yield stress of transparent mud-like simulation materials

[0140] A similar simulation material of transparent mud was prepared by the formula and preparation method in Example 2, except that the molecular weight of PAM was changed to 7 million, 15 million, 10 million, 20 million and 25 million, respectively, and the addition amount of PAM was changed to 0.1%, 0.3%, 0.5%, 0.7% and 0.9%, respectively. The plastic viscosity and yield stress were tested and analyzed using a NXS-11B rotational viscometer.

[0141] The experimental results are as follows Figure 2-Figure 5 shown.

[0142] according to Figure 2 and Figure 3 The experimental results show that with the increase of PAM molecular weight, the plastic viscosity of the prepared transparent mud-like simulation material decreases and the yield stress increases, and the change in yield stress is not significant, indicating that changing the PAM molecular weight cannot significantly increase the yield stress of the simulation material.

[0143] according to Figure 4 and Figure 5 The experimental results show that with the increase of PAM addition, the plastic viscosity and yield stress of the transparent mud-like simulation material obtained are significantly increased. The main reason is that PAM, as a polymer material, presents a branched structure when dissolved in water. When the PAM concentration increases, the degree of cross-linking and aggregation will also increase, making the intermolecular force stronger, thereby causing the plastic viscosity and yield stress of the solution to increase significantly.

[0144] In summary, the plastic viscosity and yield stress of the transparent mud-like simulation material can be adjusted by adjusting the molecular weight of PAM, the amount of PAM added, and the type and amount of rheological modifier added. The density can be adjusted by combining the amount of alkali metal salt NaCl added, and the simulated density of 1-1.2 g / cm can be achieved in an approximate 1:1 ratio. 3 , and the real drilling mud with a dynamic-plastic ratio of 0.36-0.48 can effectively simulate the performance of real drilling mud and facilitate the intuitive observation of cuttings migration in the drilling cuttings migration model test.

[0145] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A transparent mud-like simulation material, characterized in that: The following raw materials are included in weight percentage: Polyacrylamide 0.1-1%, alkali metal salt 5-30%, rheology regulator 0.2-2%, and the balance is water.

2. The transparent mud-like simulation material according to claim 1, characterized in that: The molecular weight of the polyacrylamide is 7 million to 25 million.

3. The transparent mud-like simulation material according to claim 1, characterized in that: The alkali metal salt is any one of sodium chloride, potassium chloride, magnesium chloride, calcium chloride, barium chloride, sodium carbonate, potassium carbonate, sodium sulfate and potassium sulfate.

4. The transparent mud-like simulation material according to claim 1, characterized in that: The rheology regulator is any one of sodium hydroxymethylcellulose, hydroxyethyl nanocellulose, hydroxypropyl nanocellulose, methyl allyl polyoxyethylene ether and triethanolamine.

5. The method for preparing the transparent mud-like simulation material according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: dissolving polyacrylamide in water, adding alkali metal salt and rheology regulator, and stirring to obtain the product.

6. The method for preparing the transparent mud-like simulation material according to claim 5, characterized in that: The stirring speed is 300-900rpm and the time is 1-5h.

7. Use of the transparent mud similar simulation material according to any one of claims 1 to 5 in simulating real drilling mud.