Method for recycling valuable metal ions in lithium battery diaphragm
Through the three-stage countercurrent acid leaching and roasting steps, the problems of high energy consumption and low extraction rate in lithium battery separator recycling are solved, efficient extraction of lithium, nickel, cobalt, manganese and other metals is achieved, and the recycling efficiency and purity are improved.
Patent Information
- Application Number
- CN202410864292.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-30
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-30
AI Technical Summary
The existing lithium battery separator recycling technology has high energy consumption and low metal extraction rate, and cannot effectively utilize valuable metal materials in used lithium batteries.
The three-stage countercurrent acid leaching method is used to treat the lithium battery separator using a mixed solution of sulfuric acid and hydrochloric acid. The pH value is adjusted to perform a precipitation reaction, and the roasting step is combined to extract lithium, nickel, cobalt, manganese and other metal ions to improve the metal extraction efficiency.
It improves the extraction rate of lithium, nickel, cobalt, manganese and other metal ions, achieves efficient recycling of used lithium battery separators, reduces energy consumption and improves the purity and recycling efficiency of metals.
Smart Images

Figure BDA0004919865300000051 
Figure BDA0004919865300000061 
Figure BDA0004919865300000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of battery recycling, and in particular relates to a method for recycling valuable metal ions in a lithium battery separator. Background Art
[0002] At present, power batteries are mainly lithium batteries. With the increasing use of lithium batteries, the amount of waste lithium batteries is also gradually increasing. A large amount of lithium battery separators will be obtained in the process of processing waste lithium batteries. Lithium battery separators are rich in metallic lithium and also contain valuable metal materials such as nickel, cobalt, and manganese. Therefore, the recycling of lithium battery separators is particularly important.
[0003] Existing lithium battery separators are mainly processed by thermal decomposition, which requires high energy consumption and has a low metal extraction rate. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention proposes a method for recovering valuable metal ions in lithium battery separators, which can improve the extraction rate of lithium ions in the separators, and can also extract metal ions such as nickel, cobalt, and manganese, thereby making full use of the value of waste separators.
[0005] The above technical objectives of the present invention are achieved through the following technical solutions:
[0006] A method for recovering valuable metal ions in a lithium battery separator comprises the following steps: (1) crushing the lithium battery separator and performing three-stage countercurrent acid leaching to separate solid and liquid to obtain waste residue and enriched liquid, wherein the acid used in the three-stage countercurrent acid leaching is a mixed solution of sulfuric acid and hydrochloric acid; (2) adding alkali solution to the enriched liquid obtained in step (1) to adjust the pH to 4-6, causing a precipitation reaction, and then performing solid-liquid separation to obtain a filter cake and a filtrate; (3) adding alkali solution to the filtrate obtained in step (2) to adjust the pH to alkaline, causing a precipitation reaction, and then performing solid-liquid separation to obtain a solid phase, and washing the solid phase to obtain nickel-cobalt-manganese hydroxide; (4) roasting the filter cake obtained in step (2), adding water to dissolve it, and filtering it to obtain a lithium ion-rich solution and iron-aluminum slag.
[0007] Preferably, in step (1), the acid solution used in the tertiary countercurrent acid leaching is a mixture of 20% sulfuric acid and 20% hydrochloric acid in a volume ratio of (20-40):1.
[0008] Preferably, in step (1), the liquid-to-solid ratio of the acid solution used in the three-stage countercurrent acid leaching to the lithium battery separator is (5-20) mL: 1 g.
[0009] Preferably, in step (1), the time of the three-stage countercurrent acid leaching is 1-5 hours.
[0010] Preferably, in step (2) and step (3), the alkali solution is at least one of a sodium hydroxide solution and a potassium hydroxide solution, and the concentration of the alkali solution is 1-3 mol / L.
[0011] Preferably, in step (2), the molar ratio of the metal ions in the enriched solution to the hydroxide ions in the alkaline solution is 1:(1-3).
[0012] Preferably, in step (3), adjusting the pH to be alkaline means adjusting the pH to 10-12.
[0013] Preferably, in step (3), the molar ratio of the metal ions in the filtrate to the hydroxide ions in the alkali solution is 1:(1-4).
[0014] Preferably, in step (4), the calcination temperature is 400-600° C., and the calcination time is 1-3 h.
[0015] Preferably, in step (4), the mass ratio of the filter cake to the water added for dissolution is 1:(10-100).
[0016] Further preferably, in step (4), the mass ratio of the filter cake to the water added for dissolution is 1:(10-50).
[0017] Preferably, in step (4), the ferroaluminum slag is a mixed solid of iron oxide and aluminum oxide.
[0018] The beneficial effects of the present invention are:
[0019] (1) In the method for recovering valuable metal ions in the lithium battery separator of the present invention, a small amount of hydrochloric acid is added to the sulfuric acid used in the three-stage countercurrent acid leaching to make the aluminum foil dissolve quickly, and at the same time provide chloride ions for the subsequent precipitation of lithium ions, thereby avoiding the direct use of sulfuric acid resulting in poor dissolution effect of the aluminum sheet, the direct use of low-concentration hydrochloric acid resulting in poor leaching effect, and the violent reaction of high-concentration hydrochloric acid being unsafe;
[0020] (2) In the method for recovering valuable metal ions in the lithium battery separator of the present invention, three-stage countercurrent acid leaching is used to ensure that the residual valuable metals in the lithium battery separator are fully leached, and at the same time, the metal ions in the leachate can be enriched;
[0021] (3) In the method for recovering valuable metal ions in lithium battery separators of the present invention, sodium hydroxide is added to adjust the pH of the leaching solution to 4-6. Aluminum ions react with lithium ions and chloride ions under the action of sodium hydroxide to form LiCl·2Al(OH)3·nH2O co-precipitates. At the same time, iron ions react with sodium hydroxide to form iron hydroxide precipitates. After filtration, an aqueous solution containing nickel, cobalt and manganese ions is obtained. Sodium hydroxide is continued to be added to adjust the pH to 10-12 to obtain nickel, cobalt and manganese hydroxide precipitates, which can be used as raw materials for ternary precursor production after acid dissolution.
[0022] (4) The method of the present invention for recovering valuable metal ions in lithium battery separators has a high extraction rate for nickel, cobalt and lithium, and can efficiently recover valuable metals from materials with low valuable metal content. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a schematic diagram of the process of Example 1 of the present invention;
[0024] Figure 2 This is a three-stage countercurrent acid leaching flow chart in Example 1 of the present invention. DETAILED DESCRIPTION
[0025] The present invention will be further described below in conjunction with specific embodiments.
[0026] The main components of the lithium battery separators used in Examples 1-13 of the present invention are shown in Table 1 below.
[0027] Table 1: Main components of lithium battery separators (%)
[0028] Separator paper Aluminum foil Copper foil Black powder 86.30 3.34 2.38 7.98
[0029] The main components of the black powder in Table 1 are shown in Table 2 below.
[0030] Table 2: Main components of black powder (%)
[0031] Fe Ni Co Mn Li Acid insoluble matter 0.62 0.28 0.10 0.65 0.96 5.37
[0032] Embodiment 1:
[0033] A method for recovering valuable metal ions in lithium battery separators, such as Figure 1 As shown, the following steps are included:
[0034] (1) After the lithium battery separator is crushed, 6 groups of samples are taken, each group of samples has 20g, and 300g of mixed acid prepared by mixing 20% sulfuric acid and 20% hydrochloric acid in a volume ratio of 30:1 is added to perform three-stage countercurrent acid leaching (such as Figure 2As shown), the liquid-solid ratio of the mixed acid to the lithium battery separator is 300:20 (ml:g). If the filtrate is less than 300ml, the mixed acid is added to 300ml. The leaching time for each group of samples is 2h. After enrichment, the waste residue and enrichment solution are obtained by filtration.
[0035] (2) adding 1 mol / l sodium hydroxide solution to the enriched solution obtained in step (1), adjusting the pH to 5, causing a precipitation reaction, filtering, and obtaining a filter cake containing LiCl·2Al(OH)3·nH2O and ferric hydroxide and a filtrate L;
[0036] (3) adding a 2 mol / l sodium hydroxide solution to the filtrate L obtained in step (2), adjusting the pH to 11 to produce a precipitation reaction, filtering to obtain a solid phase, and washing the solid phase with clean water to obtain nickel-cobalt-manganese hydroxide, which can be subsequently used as a raw material for generating a ternary positive electrode material;
[0037] (4) The filter cake obtained in step (2) is washed with clean water, and then placed in an electric furnace and roasted at 500° C. for 2 h to obtain aluminum oxide, iron oxide, and lithium oxide. After the roasted filter cake is cooled, water is added to dissolve it in a mass ratio of 1:20, and a high-purity lithium ion solution and an iron-aluminum slag composed of a mixed solid of iron oxide and aluminum oxide are obtained after filtering.
[0038] Embodiment 2:
[0039] A method for recovering valuable metal ions in a lithium battery separator, which differs from Example 1 only in that 20% sulfuric acid is used instead of the mixed acid in step (1).
[0040] Embodiment 3:
[0041] A method for recovering valuable metal ions in a lithium battery separator, which differs from Example 1 only in that the time for the three-stage countercurrent acid leaching in step (1) is 1 hour.
[0042] Embodiment 4:
[0043] A method for recovering valuable metal ions in a lithium battery separator, which differs from Example 1 only in that the time for the three-stage countercurrent acid leaching in step (1) is 3 hours.
[0044] Embodiment 5:
[0045] A method for recovering valuable metal ions in a lithium battery separator, which differs from Example 1 only in that the liquid-to-solid ratio of the mixed acid to the lithium battery separator in step (1) is 100:20 (ml:g).
[0046] Embodiment 6:
[0047] A method for recovering valuable metal ions in a lithium battery separator, which differs from Example 1 only in that the liquid-to-solid ratio of the mixed acid to the lithium battery separator in step (1) is 200:20 (ml:g).
[0048] Embodiment 7:
[0049] A method for recovering valuable metal ions in a lithium battery separator, which differs from Example 1 only in that the liquid-to-solid ratio of the mixed acid to the lithium battery separator in step (1) is 400:20 (ml:g).
[0050] Embodiment 8:
[0051] A method for recovering valuable metal ions in a lithium battery separator, the difference from Example 1 being that the calcination temperature in step (4) is 400°C.
[0052] Embodiment 9:
[0053] A method for recovering valuable metal ions in a lithium battery separator, the difference from Example 1 being that the calcination temperature in step (4) is 600°C.
[0054] Embodiment 10:
[0055] A method for recovering valuable metal ions in a lithium battery separator, the difference from Example 1 being that the calcination time in step (4) is 1 hour.
[0056] Embodiment 11:
[0057] A method for recovering valuable metal ions in a lithium battery separator, the difference from Example 1 being that the calcination time in step (4) is 3 hours.
[0058] Embodiment 12:
[0059] A method for recovering valuable metal ions in a lithium battery separator, the difference from Example 1 being that water is added in step (4) at a solid-liquid ratio of 1:10.
[0060] Embodiment 13:
[0061] A method for recovering valuable metal ions in a lithium battery separator, which differs from Example 1 only in that in step (4), water is added to dissolve the filter cake in a mass ratio of 1:30.
[0062] Test example:
[0063] The filtrate L, the iron oxide and aluminum oxide mixed solid (iron aluminum slag) and the lithium ion solution obtained in the recovery method of Examples 1-13 were subjected to elemental analysis. The results are shown in Table 3:
[0064] Table 3: Element detection results
[0065]
[0066]
[0067]
[0068]
[0069]
[0070] It can be seen from Table 3 that in the iron oxide and aluminum oxide mixed solid obtained in Examples 1-13, the nickel content is less than 0.1%, the cobalt content is less than 0.04%, the manganese content is less than 0.4%, the lithium content is less than 0.6%, the extraction rate of valuable metals such as nickel, cobalt, manganese and lithium is high, there are no other metal ions in the lithium ion solution, and the purity is relatively high; the present invention realizes the efficient recovery of low-content valuable metal ions, and metal ions such as nickel, cobalt and manganese are simultaneously recovered in the process of obtaining a high-purity lithium ion solution, thereby reducing the loss of valuable metals.
[0071] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for recovering valuable metal ions in lithium battery separators, characterized in that: The following steps are involved: (1) crushing the lithium battery diaphragm and performing three-stage countercurrent acid leaching to separate the solid and liquid to obtain waste residue and enriched liquid, wherein the acid used in the three-stage countercurrent acid leaching is a mixed solution of sulfuric acid and hydrochloric acid; (2) adding alkaline solution to the enriched solution obtained in step (1) to adjust the pH to 4-6, causing a precipitation reaction, and then performing solid-liquid separation to obtain a filter cake and a filtrate; (3) adding alkali solution to the filtrate obtained in step (2) to adjust the pH to alkaline, causing a precipitation reaction, and then performing solid-liquid separation to obtain a solid phase, and washing the solid phase to obtain nickel-cobalt-manganese hydroxide; (4) The filter cake obtained in step (2) is calcined, dissolved in water, and filtered to obtain a lithium ion-rich solution and iron-aluminum slag.
2. A method for recovering valuable metal ions in a lithium battery separator according to claim 1, characterized in that: In step (1), the acid solution used in the three-stage countercurrent acid leaching is a mixture of 20% sulfuric acid and 20% hydrochloric acid in a volume ratio of (20-40):
1.
3. A method for recovering valuable metal ions in a lithium battery separator according to claim 1, characterized in that: In step (1), the liquid-to-solid ratio of the acid solution used in the three-stage countercurrent acid leaching to the lithium battery separator is (5-20) mL: 1 g.
4. A method for recovering valuable metal ions in a lithium battery separator according to claim 1, characterized in that: In step (1), the time of the three-stage countercurrent acid leaching is 1-5 hours.
5. A method for recovering valuable metal ions in a lithium battery separator according to claim 1, characterized in that: In step (2), the molar ratio of the metal ions in the enriched solution to the hydroxide ions in the alkaline solution is 1:(1-3).
6. A method for recovering valuable metal ions in a lithium battery separator according to claim 1, characterized in that: In step (3), adjusting the pH to be alkaline means adjusting the pH to 10-12.
7. A method for recovering valuable metal ions in a lithium battery separator according to claim 1, characterized in that: In step (3), the molar ratio of the metal ions in the filtrate to the hydroxide ions in the alkali solution is 1:(1-4).
8. A method for recovering valuable metal ions in a lithium battery separator according to claim 1, characterized in that: In step (4), the calcination temperature is 400-600° C., and the calcination time is 1-3 hours.
9. A method for recovering valuable metal ions in a lithium battery separator according to claim 1, characterized in that: In step (4), the mass ratio of the filter cake to the water added for dissolution is 1:(10-100).
10. A method for recovering valuable metal ions in lithium battery separators according to claim 1, characterized in that: In step (4), the ferroaluminum slag is a mixed solid of iron oxide and aluminum oxide.
Citation Information
Patent Citations
Method for preparing granular adsorbent used for extracting lithium from lithium-containing brine
CN106622103A
Method for preparing battery grade lithium carbonate by recovering lithium from lithium iron phosphate waste battery
CN106785166A
Recycling method of positive electrode material of waste lithium ion battery
CN107732352A
Method for intensifying leaching of active matter in positive electrode of waste lithium ion battery
CN108504865A
Method for extracting lithium from salt lake brine and preparing aluminum hydroxide simultaneously
CN109336142A