Preparation process of high-toughness conductive copper-aluminum electroplating composite belt
By spraying the mesoporous Fe particles and Cr2C-Y2O3 composite layer on the aluminum strip and electroplating copper tempering treatment, the problem of the generation of hard and brittle compounds at the interface of the copper-aluminum composite plate and strip is solved, and its peel strength and tensile strength are improved, extending the Extended service life and expanded application scope.
Patent Information
- Application Number
- CN202410730123.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-06
- Publication Date
- 2024-10-08
AI Technical Summary
Existing copper-aluminum composite plates and strips generate hard and brittle intermetallic compounds at the interface, resulting in low bonding strength and tensile strength, which limits its application and promotion in the industrial field.
Mesoporous Fe particles and Cr2C-Y2O3 composite layer are sprayed on the aluminum tape, and through copper electroplating and tempering treatment, a tight copper film and a dense ultra-fine grain structure are formed, which suppresses the generation of brittle metal phases and enhances peel strength and resistance. Tensile strength.
The peel strength and tensile strength of the copper-aluminum electroplated composite strip are significantly improved, extending its service life and expanding its application scope.
Smart Images

Figure CN118745573A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal plate and strip production, in particular to a preparation process of a high-toughness conductive copper-aluminum electroplated composite strip. Background Art
[0002] Copper has good electrical and thermal conductivity, corrosion resistance and antibacterial properties, while aluminum also has good electrical and thermal conductivity. However, compared with aluminum, copper resources are scarce, while aluminum resources are relatively abundant, and aluminum has a small specific gravity. The copper-aluminum composite strip developed using the "skin effect" combines the advantages of copper's excellent electrical and thermal conductivity and corrosion resistance with aluminum's light weight and low price. It is widely used in connectors, battery columns, communication substrates, etc. Under the same conductivity conditions, compared with copper alloys, the weight of the copper-aluminum composite plate can be reduced by 50%, and its production cost can be reduced by 30-40%. It is the current development direction and research hotspot of new metal materials.
[0003] At present, a variety of preparation methods have been developed at home and abroad for the preparation of copper-aluminum composite plates and strips. Typical preparation methods include continuous casting and cast-rolling composite technology, explosive welding composite process, stir friction welding composite process and cold rolling composite process, but these preparation processes are often prone to generate hard and brittle intermetallic compounds at the interface, resulting in lower bonding strength and tensile strength, lower toughness, affecting their scope of use and life, and thus limiting the further application and promotion of copper-aluminum composite plates and strips in the industrial field. Summary of the invention
[0004] In order to solve the above technical defects, the present invention has developed a preparation process for a high-toughness conductive copper-aluminum electroplated composite tape which can significantly improve the peel strength of the product and make the product have excellent tensile strength.
[0005] A preparation process of a high-toughness conductive copper-aluminum electroplated composite strip comprises the following steps:
[0006] S1: Preparation of mesoporous Fe particles
[0007] Prepare a sodium chloride solution, then drop it into anhydrous ethanol for recrystallization, crush it to obtain recrystallized sodium chloride powder, take Fe(NO3)3·9H2O and completely dissolve it in distilled water, then add tetraethyl silicate, heat it in a constant temperature water bath, then take it out and heat it until solid precipitates, then add recrystallized sodium chloride powder, stir and heat it, then crush it to obtain light yellow particles, sinter the light yellow particles, cool it to room temperature, wrap it with filter paper, and extract it in deionized water to obtain mesoporous Fe particles;
[0008] S2: Preparation of Y / Cr2C-Fe composite layer aluminum strip
[0009] Add Cr2AlC powder to HF solution, then perform ultrasonic treatment, add deionized water and stir and centrifuge, filter and collect the supernatant, dry the supernatant and heat it in a muffle furnace to obtain Cr2C-Mxene, ball-mill Cr2C-Mxene and Y2O3, add them to anhydrous ethanol and perform ultrasonic dispersion to obtain nano Cr2C-Y2O3 slurry, then add the mesoporous Fe particles obtained in step S1, stir, sieve and dry, repeat the process to obtain Y / Cr2C-Fe particles, place an aluminum strip in a fluidized bed and spray the Y / Cr2C-Fe particles to obtain a Y / Cr2C-Fe composite layer aluminum strip;
[0010] S3: Copper electroplating and tempering
[0011] The Y / Cr2C-Fe composite layer aluminum strip is electroplated with copper, and then placed in a shot peening machine for surface shot peening to obtain a shot peened copper-plated aluminum strip. The shot peened copper-plated aluminum strip is electroplated with copper for a second time, rinsed, and tempered to obtain a copper-aluminum electroplated composite strip.
[0012] Furthermore, the preparation of mesoporous Fe particles in step S1 comprises the following steps:
[0013] S1.1: Take 4-6 parts of sodium chloride and add them to 10-12 parts of deionized water, stir until the sodium chloride is completely dissolved to obtain a sodium chloride solution, add the sodium chloride solution dropwise into 25-30 parts of anhydrous ethanol, stir for 30-40 minutes, then filter and separate the generated solid, and crush to obtain recrystallized sodium chloride powder;
[0014] S1.2: Take 1-2 parts of Fe(NO3)3·9H2O and add it to 8-10 parts of distilled water, stir until it is completely dissolved, then add 2-3 parts of tetraethyl silicate, then place it in a constant temperature water bath and stir at 45-50°C for 2-3 hours, take it out and place it in a container and heat it to 75-80°C, keep it warm until solid precipitates, then add 4-6 parts of recrystallized sodium chloride powder, stir for 8-10 minutes, then heat it to 100-110°C, heat it for 1-1.5 hours to obtain a light yellow solid, and crush the light yellow solid to obtain light yellow particles;
[0015] S1.3: Place the light yellow particles in an atmosphere sintering furnace, continuously introduce CO, and heat to 600-650℃ at a heating rate of 10-15℃ / min. Keep warm for 1.5-2 hours. After cooling to room temperature, wrap them with filter paper and put them into a Soxhlet extractor with deionized water as solvent. After extraction for 3-4 hours, take them out and dry them to obtain mesoporous Fe particles.
[0016] Furthermore, step S2 of preparing a Y / Cr2C-Fe composite layer aluminum strip comprises the following steps:
[0017] S2.1: Add 1-2 parts of Cr2AlC powder to 8-10 parts of HF solution, then place in an ultrasonic disperser, adjust the temperature to 35-40°C, the ultrasonic frequency to 18-20KHz, perform ultrasonic treatment for 2-3 hours, add 18-20 parts of deionized water, stir for 18-20 minutes to obtain a mixed solution, place the mixed solution in a centrifuge for centrifugation, filter and collect the supernatant, place the supernatant in a vacuum drying oven and dry for 8-10 hours, place the obtained solid substance in a muffle furnace, adjust the temperature to 200-220°C, and heat for 2-3 hours to obtain Cr2C-Mxene;
[0018] S2.2: Cr2C-Mxene and Y2O3 are placed in a planetary ball mill, stirred at a speed of 1800-2000rpm for 25-30 minutes, then added to anhydrous ethanol, and then placed in an ultrasonic disperser for dispersion at a frequency of 20-25KHz for 1-1.5 hours to obtain nano Cr2C-Y2O3 slurry, and then the mesoporous Fe particles prepared in step S1 are added, stirred for 15-20 minutes, and then sieved with a 40-50 mesh sieve, and then placed in a vacuum drying oven for drying, adjusting the temperature to 80-85°C, drying for 25-30 minutes, and then immersed in nano Cr2C-Y2O3 slurry for stirring, sieve and drying, repeating the above operation 3-4 times to obtain Y / Cr2C-Fe particles;
[0019] S2.3: Place the aluminum strip in a fluidized bed and heat it to 550-600°C, then spray the Y / Cr2C-Fe particles evenly on the surface of the copper strip using a spray gun with a spray thickness of 1-2 mm. After cooling to room temperature, obtain the Y / Cr2C-Fe composite layer aluminum strip.
[0020] Furthermore, step S3 of copper electroplating and tempering treatment includes the following steps:
[0021] S3.1: Place the Y / Cr2C-Fe composite aluminum strip in a copper plating tank filled with electroplating solution for copper plating, adjust the electroplating temperature to 40-45°C, and the current density to 1-3A / dm 2 , electroplating for 3-4 minutes to obtain a pre-copper-plated aluminum strip, and then placing the pre-copper-plated aluminum strip in a shot peening machine, adjusting the nozzle distance to 1000-1500mm, the impact angle to 90°, the input current to 10-15A, and using steel balls with a particle size of 800-1000μm for shot peening for 4-6 minutes to obtain a shot peened copper-plated aluminum strip;
[0022] S3.2: Place the shot-peened copper-plated aluminum strip in a copper plating tank filled with electroplating solution for copper plating. Adjust the electroplating temperature to 45-50°C and the current density to 3-5A / dm 2 , electroplating for 20-30 minutes, then adjusting the current density to 1-3A / dm 2After electroplating for 6-8 minutes, the strip was rinsed with clean water 2-3 times and placed in a box-type tempering furnace, heated at 200-250°C for 30-35 minutes to obtain a copper-aluminum electroplated composite strip.
[0023] Furthermore, the sodium chloride solution in step S1.1 is added dropwise at a speed of 30-45 minutes.
[0024] Furthermore, the particle size of the light yellow particles in step S1.2 is 0.8-1 mm.
[0025] Furthermore, in step S1.3, the gas flow rate of CO is 80-100 mL / min.
[0026] Furthermore, the concentration of the HF solution in step S2.1 is 48-50%.
[0027] Furthermore, in step S2.2, the mass ratio of Cr2C-Mxene, Y2O3 and anhydrous ethanol is 1:(0.8:1):(4-5).
[0028] Furthermore, the plating solution in step S3.1 comprises: 180-200 g / L copper sulfate, 40-50 g / L sulfuric acid, 5-10 g / L phytic acid, 0.1-0.15 g / L brightener, 0.01-0.015 g / L benzotriazole and 0.05-0.1 g / L bipyridine.
[0029] The beneficial effects are as follows: 1. The present invention prepares Cr2AlC into Cr2C-Mxene, then ball-mills the Cr2AlC with Y2O3 and disperses the Cr2C-Y2O3 slurry, and then repeatedly immerses the mesoporous Fe particles in the Cr2C-Y2O3 slurry and performs a stirring, mesh sieving and drying process to obtain Y / Cr2C-Fe particles. The Y / Cr2C-Fe particles are sprayed on the surface of an aluminum strip and then electroplated with copper, which can not only enhance the effect of electroplating copper and make the copper film more closely attached to the Y / Cr2C-Fe composite layer aluminum strip, but also Y and Cr2C can synergistically diffuse Fe to the copper-aluminum interface in the subsequent tempering process, inhibit the generation of a brittle metal phase, so that the prepared copper-aluminum electroplated composite strip has excellent peel strength and tensile strength, and the obtained copper-aluminum electroplated composite strip has high toughness.
[0030] 2. The present invention prepares mesoporous Fe particles with a grid-like distribution inside. When immersed in Cr2C-Y2O3 slurry, Cr2C-Y2O3 can be fully loaded, so that Y / Cr2C generated in the subsequent drying process can better combine with Fe. In the tempering stage, the Y / Cr2C-Fe particle layer between the aluminum strip and the copper film can make the Fe element better diffuse into the copper and aluminum and generate Al / Fe interface and Cu / Fe interface, thereby greatly inhibiting the formation of brittle intermetallic compound AlCu phase, thereby increasing the tensile strength of the interface between Cu and Al, and further improving the overall tensile strength and peel strength of the copper-aluminum electroplated composite strip.
[0031] 3. The present invention performs shot peening on the pre-copper-plated aluminum strip after the first copper electroplating. The copper-aluminum matrix is fully contacted and bonded to the Y / Cr2C-Fe particle layer under the pressure of the impact. The mechanical energy is converted into deformation energy to stimulate a large amount of dislocation movement on the bonding surface, and more dense ultrafine grains are formed on the contact surface, forming a strain strengthening effect, thereby improving the peel strength of the copper-aluminum electroplated composite strip, making its application range more extensive and its service life increased. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a process flow chart for preparing the high-toughness conductive copper-aluminum electroplated composite strip used in an embodiment of the present invention. DETAILED DESCRIPTION
[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Example 1
[0035] A preparation process of a high-toughness conductive copper-aluminum electroplated composite strip, such as Figure 1 As shown, the following steps are included:
[0036] S1: Preparation of mesoporous Fe particles
[0037] S1.1: Take 4 parts of sodium chloride and add them to 10 parts of deionized water, stir until the sodium chloride is completely dissolved to obtain a sodium chloride solution, add the sodium chloride solution dropwise into 25 parts of anhydrous ethanol within 30 minutes, stir for 30 minutes, then filter and separate the generated solid, and crush to obtain recrystallized sodium chloride powder;
[0038] S1.2: Take 1 part of Fe(NO3)3·9H2O and add it to 8 parts of distilled water, stir until it is completely dissolved, then add 2 parts of tetraethyl silicate, then place it in a constant temperature water bath and stir at 45°C for 2 hours, take it out and place it in a container and heat it to 75°C, keep it warm until solid precipitates, then add 4 parts of recrystallized sodium chloride powder, stir for 8 minutes, then heat it to 100°C, heat it for 1 hour to obtain a light yellow solid, and crush the light yellow solid to obtain light yellow particles with a particle size of 0.8 mm;
[0039] S1.3: Place the light yellow particles in an atmosphere sintering furnace, continuously introduce CO with a CO gas flow rate of 80 mL / min, heat to 600°C at a heating rate of 10°C / min, keep warm for 1.5 hours, cool to room temperature, wrap with filter paper, put into a Soxhlet extractor, use deionized water as solvent, extract for 3 hours, then take out and dry to obtain mesoporous Fe particles.
[0040] S2: Preparation of Y / Cr2C-Fe composite layer aluminum strip
[0041] S2.1: Add 1 part of Cr2AlC powder to 8 parts of HF solution with a concentration of 48%, then place it in an ultrasonic disperser, adjust the temperature to 35°C, the ultrasonic frequency to 18KHz, perform ultrasonic treatment for 2 hours, add 18 parts of deionized water, stir for 18 minutes to obtain a mixed solution, place the mixed solution in a centrifuge for centrifugation, filter and collect the supernatant, place the supernatant in a vacuum drying oven and dry it for 8 hours, place the obtained solid substance in a muffle furnace, adjust the temperature to 200°C, and heat it for 2 hours to obtain Cr2C-Mxene;
[0042] S2.2: Cr2C-Mxene and Y2O3 are placed in a planetary ball mill, stirred at a speed of 1800rpm for 25 minutes, and then added to anhydrous ethanol, wherein the mass ratio of Cr2C-Mxene, Y2O3 and anhydrous ethanol is 1:0.8:4, and then placed in an ultrasonic disperser for dispersion at a frequency of 20KHz for 1 hour to obtain nano Cr2C-Y2O3 slurry, and then the mesoporous Fe particles prepared in step S1 are added, stirred for 15 minutes, and then passed through a 40-mesh sieve, and then placed in a vacuum drying oven for drying, adjusting the temperature to 80°C, drying for 25 minutes, and then immersed in nano Cr2C-Y2O3 slurry for stirring, passing through a mesh sieve and drying, repeating the above operation 3 times to obtain Y / Cr2C-Fe particles;
[0043] S2.3: Place the aluminum strip in a fluidized bed and heat it to 550°C. Then, spray the Y / Cr2C-Fe particles evenly on the surface of the copper strip using a spray gun. The spraying thickness is 1 mm. After cooling to room temperature, a Y / Cr2C-Fe composite layer aluminum strip is obtained.
[0044] S3: Copper electroplating and tempering
[0045] S3.1: Place the Y / Cr2C-Fe composite layer aluminum strip in a copper plating tank filled with electroplating solution for copper plating. The electroplating solution contains 180 g / L copper sulfate, 40 g / L sulfuric acid, 5 g / L phytic acid, 0.1 g / L brightener, 0.01 g / L benzotriazole and 0.05 g / L bipyridine. The electroplating temperature is adjusted to 40 °C and the current density is 1 A / dm 2 , electroplating for 3 minutes to obtain a pre-copper-plated aluminum strip, and then placing the pre-copper-plated aluminum strip in a shot peening machine, adjusting the nozzle distance to 1000 mm, the impact angle to 90°, the input current to 10 A, and using a steel ball with a particle size of 800 μm for shot peening for 4 minutes to obtain a shot-peened copper-plated aluminum strip;
[0046] S3.2: Place the shot-peened copper-plated aluminum strip in the copper plating tank containing the electroplating solution in step S3.1 for copper plating. Adjust the electroplating temperature to 45°C and the current density to 3A / dm 2 , electroplating for 20 minutes, and then adjusting the current density to 1A / dm 2 The strip was electroplated for 6 minutes, rinsed with clean water twice, and placed in a box-type tempering furnace, heated at 200°C for 30 minutes to obtain a copper-aluminum electroplated composite strip.
[0047] Example 2
[0048] A preparation process of a high-toughness conductive copper-aluminum electroplated composite strip, such as Figure 1 As shown, the following steps are included:
[0049] S1: Preparation of mesoporous Fe particles
[0050] S1.1: Take 6 parts of sodium chloride and add them to 10 parts of deionized water, stir until the sodium chloride is completely dissolved to obtain a sodium chloride solution, add the sodium chloride solution dropwise into 30 parts of anhydrous ethanol within 30 minutes, stir for 30 minutes, then filter and separate the generated solid, and crush to obtain recrystallized sodium chloride powder;
[0051] S1.2: Take 2 parts of Fe(NO3)3·9H2O and add them to 10 parts of distilled water, stir until completely dissolved, then add 3 parts of tetraethyl silicate, then place in a constant temperature water bath and stir at 45°C for 2 hours, take out and place in a container and heat to 75°C, keep warm until solid precipitates, then add 6 parts of recrystallized sodium chloride powder, stir for 8 minutes, then heat to 100°C, heat for 1 hour to obtain a light yellow solid, crush the light yellow solid to obtain light yellow particles with a particle size of 0.8 mm;
[0052] S1.3: Place the light yellow particles in an atmosphere sintering furnace, continuously introduce CO with a CO gas flow rate of 80 mL / min, heat to 600°C at a heating rate of 10°C / min, keep warm for 1.5 hours, cool to room temperature, wrap with filter paper, put into a Soxhlet extractor, use deionized water as solvent, extract for 3 hours, then take out and dry to obtain mesoporous Fe particles.
[0053] S2: Preparation of Y / Cr2C-Fe composite layer aluminum strip
[0054] S2.1: Add 2 parts of Cr2AlC powder to 10 parts of HF solution with a concentration of 48%, then place it in an ultrasonic disperser, adjust the temperature to 35°C, the ultrasonic frequency to 18KHz, perform ultrasonic treatment for 2 hours, add 20 parts of deionized water, stir for 18 minutes to obtain a mixed solution, place the mixed solution in a centrifuge for centrifugation, filter and collect the supernatant, place the supernatant in a vacuum drying oven and dry it for 8 hours, place the obtained solid substance in a muffle furnace, adjust the temperature to 200°C, and heat it for 2 hours to obtain Cr2C-Mxene;
[0055] S2.2: Cr2C-Mxene and Y2O3 are placed in a planetary ball mill, stirred at a speed of 1800rpm for 25 minutes, and then added to anhydrous ethanol, wherein the mass ratio of Cr2C-Mxene, Y2O3 and anhydrous ethanol is 1:1:5, and then placed in an ultrasonic disperser for dispersion at a frequency of 20KHz for 1 hour to obtain nano Cr2C-Y2O3 slurry, and then the mesoporous Fe particles prepared in step S1 are added, stirred for 15 minutes, and then passed through a 40-mesh sieve, and then placed in a vacuum drying oven for drying, adjusting the temperature to 80°C, drying for 25 minutes, and then immersed in nano Cr2C-Y2O3 slurry for stirring, passing through a mesh sieve and drying, repeating the above operation 3 times to obtain Y / Cr2C-Fe particles;
[0056] S2.3: Place the aluminum strip in a fluidized bed and heat it to 550°C. Then, spray the Y / Cr2C-Fe particles evenly on the surface of the copper strip using a spray gun. The spraying thickness is 1 mm. After cooling to room temperature, a Y / Cr2C-Fe composite layer aluminum strip is obtained.
[0057] S3: Copper electroplating and tempering
[0058] S3.1: Place the Y / Cr2C-Fe composite layer aluminum strip in a copper plating tank filled with electroplating solution for copper plating. The electroplating solution contains 180 g / L copper sulfate, 40 g / L sulfuric acid, 5 g / L phytic acid, 0.1 g / L brightener, 0.01 g / L benzotriazole and 0.05 g / L bipyridine. The electroplating temperature is adjusted to 40 °C and the current density is 1 A / dm 2, electroplating for 3 minutes to obtain a pre-copper-plated aluminum strip, and then placing the pre-copper-plated aluminum strip in a shot peening machine, adjusting the nozzle distance to 1000 mm, the impact angle to 90°, the input current to 10 A, and using a steel ball with a particle size of 800 μm for shot peening for 4 minutes to obtain a shot-peened copper-plated aluminum strip;
[0059] S3.2: Place the shot-peened copper-plated aluminum strip in the copper plating tank containing the electroplating solution in step S3.1 for copper plating. Adjust the electroplating temperature to 45°C and the current density to 3A / dm 2 , electroplating for 20 minutes, and then adjusting the current density to 1A / dm 2 The strip was electroplated for 6 minutes, rinsed with clean water twice, and placed in a box-type tempering furnace, heated at 200°C for 30 minutes to obtain a copper-aluminum electroplated composite strip.
[0060] Example 3
[0061] A preparation process of a high-toughness conductive copper-aluminum electroplated composite strip, such as Figure 1 As shown, the following steps are included:
[0062] S1: Preparation of mesoporous Fe particles
[0063] S1.1: Take 4 parts of sodium chloride and add them to 10 parts of deionized water, stir until the sodium chloride is completely dissolved to obtain a sodium chloride solution, add the sodium chloride solution dropwise into 25 parts of anhydrous ethanol within 45 minutes, stir for 40 minutes, then filter and separate the generated solid, and crush to obtain recrystallized sodium chloride powder;
[0064] S1.2: Take 1 part of Fe(NO3)3·9H2O and add it to 8 parts of distilled water, stir until it is completely dissolved, then add 2 parts of tetraethyl silicate, then place it in a constant temperature water bath and stir at 50°C for 3 hours, take it out and place it in a container and heat it to 80°C, keep it warm until solid precipitates, then add 4 parts of recrystallized sodium chloride powder, stir for 10 minutes, then heat it to 110°C, heat it for 1.5 hours to obtain a light yellow solid, and crush the light yellow solid to obtain light yellow particles with a particle size of 0.8 mm;
[0065] S1.3: Place the light yellow particles in an atmosphere sintering furnace, continuously introduce CO with a CO gas flow rate of 100 mL / min, heat to 650°C at a heating rate of 15°C / min, keep warm for 2 hours, cool to room temperature, wrap with filter paper, put into a Soxhlet extractor, use deionized water as solvent, extract for 4 hours, then take out and dry to obtain mesoporous Fe particles.
[0066] S2: Preparation of Y / Cr2C-Fe composite layer aluminum strip
[0067] S2.1: Add 1 part of Cr2AlC powder to 8 parts of HF solution with a concentration of 50%, then place it in an ultrasonic disperser, adjust the temperature to 40°C, the ultrasonic frequency to 20KHz, perform ultrasonic treatment for 3 hours, add 18 parts of deionized water, stir for 20 minutes to obtain a mixed solution, place the mixed solution in a centrifuge for centrifugation, filter and collect the supernatant, place the supernatant in a vacuum drying oven and dry it for 10 hours, place the obtained solid substance in a muffle furnace, adjust the temperature to 220°C, and heat for 3 hours to obtain Cr2C-Mxene;
[0068] S2.2: Cr2C-Mxene and Y2O3 are placed in a planetary ball mill, stirred at a speed of 2000rpm for 30 minutes, and then added to anhydrous ethanol, wherein the mass ratio of Cr2C-Mxene, Y2O3 and anhydrous ethanol is 1:0.8:4, and then placed in an ultrasonic disperser for dispersion at a frequency of 25KHz for 1.5 hours to obtain nano-Cr2C-Y2O3 slurry, and then the mesoporous Fe particles prepared in step S1 are added, stirred for 20 minutes, and then sieved with a 50-mesh sieve, and then placed in a vacuum drying oven for drying, adjusting the temperature to 85°C, drying for 30 minutes, and then immersed in nano-Cr2C-Y2O3 slurry for stirring, sieve and drying, repeating the above operation 4 times to obtain Y / Cr2C-Fe particles;
[0069] S2.3: Place the aluminum strip in a fluidized bed, heat it to 600°C, and then use a spray gun to evenly spray the Y / Cr2C-Fe particles on the surface of the copper strip with a spraying thickness of 2 mm. After cooling to room temperature, a Y / Cr2C-Fe composite layer aluminum strip is obtained.
[0070] S3: Copper electroplating and tempering
[0071] S3.1: Place the Y / Cr2C-Fe composite layer aluminum strip in a copper plating tank filled with electroplating solution for copper plating. The electroplating solution contains 200 g / L copper sulfate, 50 g / L sulfuric acid, 10 g / L phytic acid, 0.15 g / L brightener, 0.015 g / L benzotriazole and 0.1 g / L bipyridine. The electroplating temperature is adjusted to 45 °C and the current density is 3 A / dm 2 , electroplating for 4 minutes to obtain a pre-copper-plated aluminum strip, and then placing the pre-copper-plated aluminum strip in a shot peening machine, adjusting the nozzle distance to 1500 mm, the impact angle to 90°, the input current to 15 A, and using a steel ball with a particle size of 1000 μm for shot peening for 6 minutes to obtain a shot peened copper-plated aluminum strip;
[0072] S3.2: Place the shot-peened copper-plated aluminum strip in the copper plating tank containing the electroplating solution in step S3.1 for copper plating. Adjust the electroplating temperature to 50°C and the current density to 5A / dm 2 , electroplating for 30 minutes, and then adjusting the current density to 3A / dm 2The strip was electroplated for 8 minutes, rinsed with clean water 3 times, placed in a box-type tempering furnace, and heated at 250°C for 35 minutes to obtain a copper-aluminum electroplated composite strip.
[0073] Comparative Example 1
[0074] Compared with Example 1, the difference of Comparative Example 1 is that Comparative Example 1 removes step S2.1 and step S2.2, and replaces the Y / Cr2C-Fe particles with mesoporous Fe particles in step S2.3. The remaining steps are the same as those in Example 1. The prepared copper-aluminum electroplated composite strip is recorded as Comparative Example 1.
[0075] Comparative Example 2
[0076] Compared with Example 1, the difference of Comparative Example 2 is that Comparative Example 2 removes step S2.1, does not add Cr2C-Mxene to S2.2, and in the subsequent steps, the nano Cr2C-Y2O3 slurry is replaced by Y2O3 slurry, and the Y / Cr2C-Fe particles are replaced by Y / Fe particles. The remaining steps are the same as those in Example 1, and the obtained copper-aluminum electroplated composite strip is recorded as Comparative Example 2.
[0077] Comparative Example 3
[0078] Compared with Example 1, the difference of Comparative Example 3 is that Y2O3 is not added in step S2.2, and in the subsequent steps, the nano Cr2C-Y2O3 slurry is replaced by Cr2C slurry, and the Y / Cr2C-Fe particles are replaced by Cr2C / Fe particles. The remaining steps are the same as those in Example 1, and the obtained copper-aluminum electroplated composite strip is recorded as Comparative Example 3.
[0079] Comparative Example 4
[0080] Compared with Example 1, the difference of Comparative Example 4 is that Comparative Example 4 removes step S1 and replaces the subsequent mesoporous Fe particles with Fe particles with a particle size of 1 mm. The remaining steps are the same as Example 1, and the obtained copper-aluminum electroplated composite strip is recorded as Comparative Example 4.
[0081] Comparative Example 5
[0082] Compared with Example 1, the difference of Comparative Example 5 is that, in Comparative Example 5, the operation of placing the pre-copper-plated aluminum strip in a shot peening machine for shot peening in step S3.1 is removed, and the subsequent shot peening copper-plated aluminum strip is replaced with the pre-copper-plated aluminum strip, and the remaining steps are the same as in Example 1. The prepared copper-aluminum electroplated composite strip is recorded as Comparative Example 5.
[0083] The copper-aluminum electroplated composite tape prepared in Example, Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4 and Comparative Example 5 were cut into three samples with a length and width of 3 cm, and the peel strength of the metallized layer was measured respectively using a Shimadzu tensile tester. The data were recorded and tabulated, as shown in Table 1. It can be seen that the peel strength of the copper-aluminum electroplated composite tape prepared in Example is greater than the peel strength of Comparative Example 5, greater than the peel strength of Comparative Example 3, greater than the peel strength of Comparative Example 2, greater than the peel strength of Comparative Example 1, and greater than the peel strength of Comparative Example 4.
[0084] The copper-aluminum electroplated composite tape prepared in Example, Comparative Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 4 were cut into three samples with a length and width of 3 cm, and the tensile strength of each sample was tested using a tensile strength testing machine. The data were recorded and tabulated, as shown in Table 2. It can be seen that the tensile strength of the copper-aluminum electroplated composite tape prepared in Example is greater than the tensile strength of Comparative Example 3, greater than the tensile strength of Comparative Example 2, greater than the tensile strength of Comparative Example 1, and greater than the tensile strength of Comparative Example 4.
[0085] Table 1: Peel strength of copper-aluminum electroplated composite tape
[0086] Peel strength / N / mm The first Second copy The third Example 1 25.1 25.7 25.5 Example 2 26.4 26.2 26.5 Example 3 25.1 24.8 24.6 Comparative Example 1 17.3 17.2 17.5 Comparative Example 2 18.8 19.1 18.7 Comparative Example 3 19.6 19.5 19.8 Comparative Example 4 15.3 15.6 15.9 Comparative Example 5 23.6 23.4 23.8
[0087] Table 2: Tensile strength of copper-aluminum electroplated composite strip
[0088]
[0089]
[0090] It can be seen from the data of the embodiments, comparative examples 1, 2 and 3 in Table 1 and Table 2 that when Cr2C and Y2O3 are removed in Comparative Examples 2 and 3, the peel strength and tensile strength of the aluminum electroplated composite tape are greatly reduced, proving that Y and Cr2C in Y / Cr2C-Fe can inhibit the formation of brittle metal phases through synergistic effects, thereby greatly improving the peel strength and tensile strength of the copper-aluminum electroplated composite tape;
[0091] It can also be seen from the data of the embodiment and comparative example 4 in Table 1 and Table 2 that the peel strength and tensile strength of the copper-aluminum electroplated composite tape are significantly reduced when the mesoporous Fe particles are not prepared, proving that the preparation of mesoporous Fe particles can improve the overall tensile strength and peel strength of the copper-aluminum electroplated composite tape;
[0092] It can be seen from the data of the embodiment and comparative example 5 in Table 1 that when the pre-plated copper-aluminum strip is not shot peened, the peel strength of the copper-aluminum electroplated composite strip decreases to a certain extent, which can prove that shot peening the pre-plated copper-aluminum strip can also improve the peel strength of the copper-aluminum electroplated composite strip.
[0093] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A process for preparing a high-toughness conductive copper-aluminum electroplated composite strip, characterized in that: The following steps are involved: S1: Preparation of mesoporous Fe particles Prepare a sodium chloride solution, then drop it into anhydrous ethanol for recrystallization, crush it to obtain recrystallized sodium chloride powder, take Fe(NO3)3·9H2O and completely dissolve it in distilled water, then add tetraethyl silicate, heat it in a constant temperature water bath, then take it out and heat it until solid precipitates, then add recrystallized sodium chloride powder, stir and heat it, then crush it to obtain light yellow particles, sinter the light yellow particles, cool it to room temperature, wrap it with filter paper, and extract it in deionized water to obtain mesoporous Fe particles; S2: Preparation of Y / Cr2C-Fe composite layer aluminum strip Add Cr2AlC powder to HF solution, then perform ultrasonic treatment, add deionized water and stir and centrifuge, filter and collect the supernatant, dry the supernatant and heat it in a muffle furnace to obtain Cr2C-Mxene, ball-mill Cr2C-Mxene and Y2O3, add them to anhydrous ethanol and perform ultrasonic dispersion to obtain nano Cr2C-Y2O3 slurry, then add the mesoporous Fe particles obtained in step S1, stir, sieve and dry, repeat the process to obtain Y / Cr2C-Fe particles, place an aluminum strip in a fluidized bed and spray the Y / Cr2C-Fe particles to obtain a Y / Cr2C-Fe composite layer aluminum strip; S3: Copper electroplating and tempering The Y / Cr2C-Fe composite layer aluminum strip is electroplated with copper, and then placed in a shot peening machine for surface shot peening to obtain a shot peened copper-plated aluminum strip. The shot peened copper-plated aluminum strip is electroplated with copper for a second time, rinsed, and tempered to obtain a copper-aluminum electroplated composite strip.
2. The process for preparing a high-toughness conductive copper-aluminum electroplated composite strip according to claim 1, characterized in that: Step S1: Preparation of mesoporous Fe particles, comprising the following steps: S1.1: Take 4-6 parts of sodium chloride and add them to 10-12 parts of deionized water, stir until the sodium chloride is completely dissolved to obtain a sodium chloride solution, add the sodium chloride solution dropwise into 25-30 parts of anhydrous ethanol, stir for 30-40 minutes, then filter and separate the generated solid, and crush to obtain recrystallized sodium chloride powder; S1.2: Take 1-2 parts of Fe(NO3)3·9H2O and add it to 8-10 parts of distilled water, stir until it is completely dissolved, then add 2-3 parts of tetraethyl silicate, then place it in a constant temperature water bath and stir at 45-50°C for 2-3 hours, take it out and place it in a container and heat it to 75-80°C, keep it warm until solid precipitates, then add 4-6 parts of recrystallized sodium chloride powder, stir for 8-10 minutes, then heat it to 100-110°C, heat it for 1-1.5 hours to obtain a light yellow solid, and crush the light yellow solid to obtain light yellow particles; S1.3: Place the light yellow particles in an atmosphere sintering furnace, continuously introduce CO, and heat to 600-650℃ at a heating rate of 10-15℃ / min. Keep warm for 1.5-2 hours. After cooling to room temperature, wrap them with filter paper and put them into a Soxhlet extractor with deionized water as solvent. After extraction for 3-4 hours, take them out and dry them to obtain mesoporous Fe particles.
3. The process for preparing a high-toughness conductive copper-aluminum electroplated composite strip according to claim 1, characterized in that: Step S2 is to prepare a Y / Cr2C-Fe composite layer aluminum strip, comprising the following steps: S2.1: Add 1-2 parts of Cr2AlC powder to 8-10 parts of HF solution, then place in an ultrasonic disperser, adjust the temperature to 35-40°C, the ultrasonic frequency to 18-20KHz, perform ultrasonic treatment for 2-3 hours, add 18-20 parts of deionized water, stir for 18-20 minutes to obtain a mixed solution, place the mixed solution in a centrifuge for centrifugation, filter and collect the supernatant, place the supernatant in a vacuum drying oven and dry for 8-10 hours, place the obtained solid substance in a muffle furnace, adjust the temperature to 200-220°C, and heat for 2-3 hours to obtain Cr2C-Mxene; S2.2: Cr2C-Mxene and Y2O3 are placed in a planetary ball mill, stirred at a speed of 1800-2000rpm for 25-30 minutes, then added to anhydrous ethanol, and then placed in an ultrasonic disperser for dispersion at a frequency of 20-25KHz for 1-1.5 hours to obtain nano Cr2C-Y2O3 slurry, and then the mesoporous Fe particles prepared in step S1 are added, stirred for 15-20 minutes, and then sieved with a 20-30 mesh sieve, and then placed in a vacuum drying oven for drying, adjusting the temperature to 80-85°C, drying for 25-30 minutes, and then immersed in nano Cr2C-Y2O3 slurry for stirring, sieve and drying, repeating the above operation 3-4 times to obtain Y / Cr2C-Fe particles; S2.3: Place the aluminum strip in a fluidized bed and heat it to 550-600°C, then spray the Y / Cr2C-Fe particles evenly on the surface of the copper strip using a spray gun with a spray thickness of 1-2 mm. After cooling to room temperature, obtain the Y / Cr2C-Fe composite layer aluminum strip.
4. The process for preparing a high-toughness conductive copper-aluminum electroplated composite strip according to claim 1, characterized in that: Step S3 copper electroplating and tempering treatment includes the following steps: S3.1: Place the Y / Cr2C-Fe composite aluminum strip in a copper plating tank filled with electroplating solution for copper plating, adjust the electroplating temperature to 40-45°C, and the current density to 1-3A / dm 2 , electroplating for 3-4 minutes to obtain a pre-copper-plated aluminum strip, and then placing the pre-copper-plated aluminum strip in a shot peening machine, adjusting the nozzle distance to 1000-1500mm, the impact angle to 90°, the input current to 10-15A, and using steel balls with a particle size of 800-1000μm for shot peening for 4-6 minutes to obtain a shot peened copper-plated aluminum strip; S3.2: Place the shot-peened copper-plated aluminum strip in a copper plating tank filled with electroplating solution for copper plating. Adjust the electroplating temperature to 45-50°C and the current density to 3-5A / dm 2 , electroplating for 20-30 minutes, then adjusting the current density to 1-3A / dm 2 After electroplating for 6-8 minutes, the strip was rinsed with clean water 2-3 times and placed in a box-type tempering furnace, heated at 200-250°C for 30-35 minutes to obtain a copper-aluminum electroplated composite strip.
5. The process for preparing a high-toughness conductive copper-aluminum electroplated composite strip according to claim 2, characterized in that: The sodium chloride solution in step S1.1 is added dropwise at a speed of 30-45 minutes.
6. The process for preparing a high-toughness conductive copper-aluminum electroplated composite strip according to claim 2, characterized in that: The particle size of the light yellow particles in step S1.2 is 0.8-1 mm.
7. The process for preparing a high-toughness conductive copper-aluminum electroplated composite strip according to claim 2, characterized in that: The gas flow rate of CO in step S1.3 is 80-100 mL / min.
8. The process for preparing a high-toughness conductive copper-aluminum electroplated composite strip according to claim 3, characterized in that: The concentration of the HF solution in step S2.1 is 48-50%.
9. The process for preparing a high-toughness conductive copper-aluminum electroplated composite strip according to claim 3, characterized in that: The mass ratio of Cr2C-Mxene, Y2O3 and anhydrous ethanol in step S2.2 is 1:(0.8:1):(4-5).
10. The process for preparing a high-toughness conductive copper-aluminum electroplated composite strip according to claim 4, characterized in that: The components of the electroplating solution in step S3.1 are: 150-180 g / L copper sulfate, 40-60 g / L sulfuric acid, 5-10 g / L phytic acid, 0.05-0.15 g / L brightener, 0.005-0.015 g / L benzotriazole and 0.05-0.1 g / L bipyridine.