Adsorbent and method for manufacturing adsorbent

By preparing sintered powders with specific particle sizes and pore structures, the problems of durability and uneven adsorption capacity of hydroxyapatite adsorbents are solved, and efficient purification and separation of biological drugs are achieved.

CN118748981APending Publication Date: 2024-10-08HOYA TECHNOSURGICAL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280093377.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-03-11
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

When existing hydroxyapatite is used as an adsorbent, its durability and adsorption capacity are uneven, resulting in uneven column performance of the adsorption device and inability to effectively purify and separate biopharmaceuticals.

Method used

By preparing a sintered powder with a specific particle size and pore structure, the surface is made of hydroxyapatite or fluoroapatite, the average particle size is above 10 μm and below 90 μm, and the pore size distribution modal pore diameter is above 32.0 nm and below 60.0 nm, The calcination temperature is above 480°C and below 645°C to form an adsorbent with improved durability and adsorption capacity.

Benefits of technology

It improves the durability and adsorption capacity of the adsorbent for the substances to be adsorbed, ensures the uniform adsorption and separation effect of the adsorption device on macromolecules such as antibodies, and enhances the stability and efficiency of the adsorbent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118748981A_ABST
    Figure CN118748981A_ABST
Patent Text Reader

Abstract

[Problem] To provide: an adsorbent which adsorbs a substance to be adsorbed, and which has improved durability and improved adsorption capacity; and a method for producing the adsorbent, said method being capable of producing the adsorbent. [Solution] The adsorbent according to the present invention is used when loaded into a column and consists of a powder comprising particles consisting of hydroxyapatite or fluorapatite in which at least some of the hydroxyl groups in the hydroxyapatite are substituted with fluorine atoms, the adsorbent satisfies the following conditions: the powder is composed of a porous body having pores; the average particle size of the powder is 10-90 [mu] m; the average particle compressive strength of the powder is 7.4 MPa to 8.9 MPa; and the highest frequency pore diameter in the pore diameter distribution of the powder is 32.0 nm to 60.0 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an adsorbent having improved durability and improved adsorption capacity for a substance to be adsorbed and a method for producing the adsorbent. Background Art

[0002] In recent years, hydroxyapatite has been widely used as a material for chromatographic stationary layers (ie, adsorbents) for purification and separation of bio-based drugs such as antibodies and vaccines, for example, due to its high biocompatibility and excellent safety.

[0003] For example, hydroxyapatite (HAP) used as a material for a chromatography stationary layer is produced as follows.

[0004] Specifically, a first liquid containing calcium hydroxide and a second liquid containing phosphoric acid are reacted under stirring to obtain primary particles of hydroxyapatite, and a slurry containing the primary particles and aggregates thereof is dried and granulated to obtain secondary particles (powder) of hydroxyapatite.

[0005] The powder (dried powder) is calcined to obtain a sintered powder, and the raw powder or sintered powder is loaded into a column (adsorption device) or the like to be used as a material (adsorbent) of a fixed layer (see, for example, Patent Document 1).

[0006] However, when sintered powder is used as an adsorbent in an adsorption device as described above, there is in fact unevenness in the durability of the adsorbent (i.e., sintered powder) and the adsorption capacity of the biopharmaceutical to be purified and separated (i.e., the substance to be adsorbed). These unevennesses lead to the following problems: the adsorption device including the adsorbent cannot obtain uniform column performance for purifying and separating the substance to be adsorbed, and leads to uneven durability of the adsorbent. The present inventors have found that there is such a problem.

[0007] Citation List

[0008] Patent Literature

[0009] Patent Document 1: JP 2011-68539A Summary of the invention

[0010] Technical issues

[0011] An object of the present invention is to provide an adsorbent having improved durability and improved adsorption capacity for a substance to be adsorbed and a method for producing the adsorbent.

[0012] Solution

[0013] The object is achieved by the present invention described in the following (1) to (19).

[0014] (1) An adsorbent to be loaded into a column and composed of a powder containing particles whose surfaces are made of hydroxyapatite or fluoroapatite in which at least some of the hydroxyl groups in the hydroxyapatite are substituted with fluorine atoms,

[0015] The powder is composed of a porous body having pores,

[0016] The average particle size of the powder is 10 μm or more and 90 μm or less,

[0017] The average particle compressive strength of the powder is 7.4 MPa or more and 8.9 MPa or less, and

[0018] The modal pore diameter in the pore size distribution of the pores of the powder is 32.0 nm or more and 60.0 nm or less.

[0019] Therefore, the sintered powder has an increased durability and an increased adsorption capacity for the substance to be adsorbed.

[0020] (2) The adsorbent as described in (1) above, wherein the specific surface area of ​​the powder is 41 m 2 / g or more and 51m 2 / g or less.

[0021] Therefore, even if the separation material (substance to be adsorbed) is a relatively large protein such as an antibody (antibody molecule), it can be said that the sintered powder has the surface area required to adsorb a sufficient amount of the separation material. Therefore, the sintered powder can further improve the adsorption capacity of the substance to be adsorbed.

[0022] (3) The adsorbent according to (1) above, wherein the surface area of ​​the column per 1 mL of powder is 25.3 m 2 / mL and above 36.0m 2 / mL or less.

[0023] Therefore, even if the separation material (substance to be adsorbed) is a relatively large protein such as an antibody (antibody molecule), it can be said that the sintered powder has the surface area required to adsorb a sufficient amount of the separation material. Therefore, the sintered powder can further improve the adsorption capacity of the substance to be adsorbed.

[0024] (4) An adsorbent to be loaded into a column and composed of a sintered powder obtained by calcining particles, the surfaces of which are made of hydroxyapatite or fluoroapatite in which at least some of the hydroxyl groups in the hydroxyapatite are substituted with fluorine atoms,

[0025] The average particle size of the sintered powder is 10 μm or more and 90 μm or less.

[0026] The specific surface area of ​​the sintered powder is 41 m2 / g or more and 51m 2 / g or less, and

[0027] The modal pore diameter in the pore size distribution of the sintered powder is 32.0 nm or more and 60.0 nm or less.

[0028] Therefore, even relatively large proteins such as antibodies (antibody molecules) can be reliably adsorbed to the sintered powder by capturing them as separation materials in the pores of the sintered powder. In addition, even if the separation material (substance to be adsorbed) is a relatively large protein such as an antibody (antibody molecule), it can be said that the sintered powder has the surface area required to adsorb a sufficient amount of the separation material. Therefore, the sintered powder can further improve the adsorption capacity of the substance to be adsorbed.

[0029] (5) An adsorbent to be loaded into a column and composed of a powder containing particles whose surfaces are made of hydroxyapatite or fluoroapatite in which at least some of the hydroxyl groups in the hydroxyapatite are substituted with fluorine atoms,

[0030] The average particle size of the powder is 10 μm or more and 90 μm or less,

[0031] The surface area of ​​the column per 1 mL of powder is 25.3 m 2 / mL and above 36.0m 2 / mL or less, and

[0032] The modal pore diameter in the pore size distribution of the pores of the powder is 32.0 nm or more and 60.0 nm or less.

[0033] Therefore, even relatively large proteins such as antibodies (antibody molecules) can be reliably adsorbed to the sintered powder by capturing them as separation materials in the pores of the sintered powder. In addition, even if the separation material (substance to be adsorbed) is a relatively large protein such as an antibody (antibody molecule), it can be said that the sintered powder has the surface area required to adsorb a sufficient amount of the separation material. Therefore, the sintered powder can further improve the adsorption capacity of the substance to be adsorbed.

[0034] (6) The adsorbent according to (1), (3) or (5) above, wherein the frequency of the modal pore size is 21.0% or more and 60.0% or less.

[0035] Therefore, even relatively large proteins such as antibodies (antibody molecules) can be reliably adsorbed to the sintered powder by capturing them as separation materials in the pores of the sintered powder.

[0036] (7) The adsorbent according to (1), (3) or (5) above, wherein the half width of a mountain-shaped waveform around a modal pore size in the pore size distribution of the pores is 1.0 nm or more and 10.0 nm or less.

[0037] Therefore, even relatively large proteins such as antibodies (antibody molecules) can be reliably adsorbed to the sintered powder by capturing them as separation materials in the pores of the sintered powder.

[0038] (8) The adsorbent according to (1), (3) or (5) above, wherein the average pore diameter of the pores is 37.0 nm or more and 75.0 nm or less.

[0039] Therefore, even relatively large proteins such as antibodies (antibody molecules) can be reliably adsorbed to the sintered powder by capturing them as separation materials in the pores of the sintered powder.

[0040] (9) The adsorbent according to any one of (1) to (5) above, wherein the powder is a sintered powder calcined at 480° C. or higher and 645° C. or lower.

[0041] Therefore, the obtained sintered powder can relatively easily make the average particle compressive strength 7.4 MPa or more and 8.9 MPa or less, and the modal pore size in the pore size distribution of the pores of the sintered powder is 32.0 nm or more and 60.0 nm or less. Therefore, the sintered powder has improved durability and improved adsorption capacity for substances to be adsorbed.

[0042] (10) A method for producing an adsorbent, comprising:

[0043] The first step is to prepare particles, the surfaces of which are made of hydroxyapatite or fluoroapatite in which at least some of the hydroxyl groups in the hydroxyapatite are substituted with fluorine atoms; and

[0044] The second step: calcining the particles prepared in the first step at a temperature T in the range of 480° C. to 645° C. to obtain a sintered powder of the particles;

[0045] The sintered powder obtained in the second step has an average particle size of 10 μm or more and 90 μm or less, an average particle compressive strength of 7.4 MPa or more and 8.9 MPa or less, and a pore diameter of 32.0 nm or more and 60.0 nm or less.

[0046] Therefore, the obtained sintered powder has improved durability and improved adsorption capacity for the substance to be adsorbed.

[0047] (11) A method for producing an adsorbent, comprising:

[0048] The first step is to prepare particles, the surfaces of which are made of hydroxyapatite or fluoroapatite in which at least some of the hydroxyl groups in the hydroxyapatite are substituted with fluorine atoms; and

[0049] The second step: calcining the particles prepared in the first step at a temperature T in the range of 480° C. to 645° C. to obtain a sintered powder of the particles;

[0050] The average particle size of the sintered powder obtained in the second step is 10 μm or more and 90 μm or less, and the specific surface area is 41 m 2 / g or more and 51m 2 / g or less, and the pore diameter is 32.0nm or more and 60.0nm or less.

[0051] Therefore, the obtained sintered powder has improved durability and improved adsorption capacity for the substance to be adsorbed.

[0052] (12) A method for producing an adsorbent, comprising:

[0053] The first step is to prepare particles, the surfaces of which are composed of hydroxyapatite or fluoroapatite in which at least some of the hydroxyl groups in the hydroxyapatite are substituted with fluorine atoms; and

[0054] The second step: calcining the particles prepared in the first step at a temperature T in the range of 480° C. to 645° C. to obtain a sintered powder of the particles;

[0055] The average particle size of the sintered powder obtained in the second step is 10 μm or more and 90 μm or less,

[0056] When the sintered powder was loaded into the column, the surface area of ​​the column per 1 mL of sintered powder was 25.3 m 2 / mL and above 36.0m 2 / mL or less, and

[0057] The pore diameter is 32.0 nm or more and 60.0 nm or less.

[0058] Therefore, the obtained sintered powder has improved durability and improved adsorption capacity for the substance to be adsorbed.

[0059] (13) An adsorbent to be loaded into a column and composed of a powder containing particles whose surfaces are made of hydroxyapatite or fluoroapatite in which at least some of the hydroxyl groups in the hydroxyapatite are substituted with fluorine atoms, wherein

[0060] When γ-globulin from bovine blood as a substance to be adsorbed was dissolved in 10 mM sodium phosphate buffer (pH 6.5), when a sample liquid is prepared so as to have a concentration of 1.0 mg / mL and the prepared sample liquid is supplied to the column (φ6.0×35 mm) at flow rates of 150 cm / h and 300 cm / h, and when, for each flow rate, an absorbance value X (280 nm) of the sample liquid to be supplied to the column and an absorbance value Y (wavelength: 280 nm) of an eluent eluted from the column are measured, and based on the amount of the sample liquid transported until the absorbance value Y (wavelength: 280 nm) becomes 10% of the absorbance value X (wavelength: 280 nm), an adsorption amount A (mg / mL) and D (mg / mL) of the substance to be adsorbed on the powder are calculated, the powder satisfies at least one of A ≥ 31 mg / mL or more and 0.60 ≤ D / A ≤ 1.00, and 0.60 ≤ D / A ≤ 0.92.

[0061] Therefore, it can be said that the adsorption amount of the antibody to the sintered powder is independent of the flow rate at which the test liquid containing the antibody is supplied to the column. Therefore, during separation and purification of the antibody using an adsorption device including the sintered powder as an adsorbent, when a sample liquid containing the antibody is supplied to the adsorption device, even if the sample liquid cannot be supplied at a constant rate and thus non-uniformity occurs in the initial stage and the final stage, the antibody can be reliably adsorbed to the sintered powder within a constant range of adsorption amount.

[0062] (14) An adsorbent to be loaded into a column and composed of a powder obtained by baking particles whose surfaces are made of hydroxyapatite or fluoroapatite in which at least some of the hydroxyl groups in the hydroxyapatite are substituted with fluorine atoms, wherein

[0063] When γ-globulin from bovine blood as a substance to be adsorbed was dissolved in 10 mM sodium phosphate buffer (pH 6.5), when a sample liquid is prepared so as to have a concentration of 1.0 mg / mL and the prepared sample liquid is supplied to the column (φ6.0×35 mm) at flow rates of 200 cm / h and 300 cm / h, and when, for each flow rate, an absorbance value X (280 nm) of the sample liquid to be supplied to the column and an absorbance value Y (wavelength: 280 nm) of an eluent eluted from the column are measured, and based on the amount of the sample liquid transported until the absorbance value Y (wavelength: 280 nm) becomes 10% of the absorbance value X (wavelength: 280 nm), an adsorption amount B (mg / mL) and D (mg / mL) of the substance to be adsorbed on the powder are calculated, the powder satisfies at least one of B ≥ 30 mg / mL or more and 0.75 ≤ D / B ≤ 1.00, and 0.75 ≤ D / B ≤ 0.96.

[0064] Therefore, it can be said that the adsorption amount of the antibody to the sintered powder is independent of the flow rate at which the test liquid containing the antibody is supplied to the column. Therefore, during separation and purification of the antibody using an adsorption device including the sintered powder as an adsorbent, when a sample liquid containing the antibody is supplied to the adsorption device, even if the sample liquid cannot be supplied at a constant rate and thus non-uniformity occurs in the initial stage and the final stage, the antibody can be reliably adsorbed to the sintered powder within a constant range of adsorption amount.

[0065] (15) An adsorbent to be loaded into a column and composed of a powder obtained by baking particles whose surfaces are made of hydroxyapatite or fluoroapatite in which at least some of the hydroxyl groups in the hydroxyapatite are substituted with fluorine atoms, wherein

[0066] When γ-globulin from bovine blood as a substance to be adsorbed was dissolved in 10 mM sodium phosphate buffer (pH 6.5), when a sample liquid is prepared so as to have a concentration of 1.0 mg / mL and the prepared sample liquid is supplied to the column (φ6.0×35 mm) at flow rates of 200 cm / h and 250 cm / h, and when, for each flow rate, an absorbance value X (280 nm) of the sample liquid to be supplied to the column and an absorbance value Y (wavelength: 280 nm) of an eluent eluted from the column are measured, and an adsorption amount B (mg / mL) and C (mg / mL) of the substance to be adsorbed on the powder are calculated based on the amount of the sample liquid transported until the absorbance value Y (wavelength: 280 nm) becomes 10% of the absorbance value X (wavelength: 280 nm), the powder satisfies at least one of B ≥ 30 mg / mL or more and 0.89 ≤ C / B ≤ 1.00, and 0.89 ≤ C / B ≤ 0.96.

[0067] Therefore, it can be said that the adsorption amount of the antibody to the sintered powder is independent of the flow rate at which the test liquid containing the antibody is supplied to the column. Therefore, during separation and purification of the antibody using an adsorption device including the sintered powder as an adsorbent, when a sample liquid containing the antibody is supplied to the adsorption device, even if the sample liquid cannot be supplied at a constant rate and thus non-uniformity occurs in the initial stage and the final stage, the antibody can be reliably adsorbed to the sintered powder within a constant range of adsorption amount.

[0068] (16) The adsorbent according to any one of (13) to (15) above, wherein:

[0069] When a durability test of the powder is performed, in the durability test, the column (φ4.0×100 mm) is dry-packed with the powder as the adsorbent, and each buffer is transported through the column in the order of the step numbers shown in Table 1, and steps 1 to 5 shown in Table 1 are counted as one cycle, and the cycle is repeated until the pressure inside the column exceeds 200 psi, and the number of repeated cycles is 60 times or more.

[0070] [Table 1]

[0071]

[0072] As described above, the sintered powder has improved durability because the sintered powder can perform 60 cycles or more in the durability test.

[0073] (17) The adsorbent according to any one of (13) to (15) above, wherein the substance to be adsorbed is an antibody.

[0074] In the adsorbent of the present invention, antibodies are preferably selected as the substance to be adsorbed.

[0075] Effects of the Invention

[0076] The adsorbent of the present invention has improved durability and improved adsorption capacity for substances to be adsorbed. In addition, the adsorbent production method of the present invention can produce the adsorbent. BRIEF DESCRIPTION OF THE DRAWINGS

[0077] Figure 1 is a vertical cross-sectional view illustrating an example of an adsorption device including the adsorbent of the present invention.

[0078] Figure 2 is a flow chart of a method for producing an adsorbent according to the present invention.

[0079] Figure 3 : is a graph showing the relationship between the adsorption amounts A to D of bIgG by the sintered hydroxyapatite powder and the flow rate of the sample liquid in each of Examples and Comparative Examples. DETAILED DESCRIPTION

[0080] The adsorbent and the method for producing the adsorbent according to the present invention will be described in detail below based on the preferred embodiments shown in the accompanying drawings.

[0081] First, before describing the adsorbent of the present invention and a method for producing the adsorbent, an example of an adsorption device (separation device) including the adsorbent of the present invention will be described.

[0082] <Adsorption device>

[0083] Figure 1is a vertical cross-sectional view illustrating an example of an adsorption device including the adsorbent of the present invention. Figure 1 The upper side in is referred to as the "inflow side", and the lower side is referred to as the "outflow side".

[0084] Herein, the inflow side refers to a side on which a liquid such as a sample liquid (a liquid containing a substance to be adsorbed) or an eluent (such as a phosphate-based buffer solution or water) is supplied to the adsorption device, and the outflow side refers to a side opposite to the inflow side, i.e., a side on which the liquid flows out of the adsorption device when the substance to be adsorbed (i.e., a protein to be separated) as a separation material (such as a biopharmaceutical) is separated (purified).

[0085] like Figure 1 As shown, the adsorption device 1 is used to separate (purify) a separation material (substance to be adsorbed), such as protein, from a sample liquid. The adsorption device 1 includes a column 2 , a particulate adsorbent 3 (filler), and two filter members 4 and 5 .

[0086] The column 2 includes a column body 21 , and a cover portion 22 (first port) and a cover portion 23 (second port) respectively attached to an inflow-side end and an outflow-side end of the column body 21 .

[0087] For example, the column body 21 is constituted by a cylindrical member. Examples of the constituent material of each component (each member) constituting the column 2 including the column body 21 include various glass materials, various resin materials, various metal materials, and various ceramic materials.

[0088] In the column body 21 , covers 22 , 23 are attached to the inflow side end and the outflow side end of the column body 21 respectively in a state where the filter members 4 and 5 are provided so as to close the inflow side opening and the outflow side opening of the column body 21 respectively.

[0089] In the column 2 having such a configuration, the column body 21 and the filter members 4 and 5 define the adsorbent filling space 20. In addition, the column body 21 and the lids 22 and 23 ensure the liquid tightness of the adsorbent filling space 20. The adsorbent 3 is filled into at least a part of the adsorbent filling space 20 (in this embodiment, substantially the entire volume).

[0090] The inner diameter (column inner diameter) of the adsorbent-filled space 20 is appropriately set according to the volume of the sample liquid, and is not particularly limited, but is preferably about 3.0 mm or more and 70.0 mm or less, and more preferably about 5.0 mm or more and 50.0 mm or less, for example. In other words, the lower limit value of the inner diameter of the adsorbent-filled space 20 is preferably 3.0 mm or more, more preferably 5.0 mm or more, and the upper limit value of the inner diameter is preferably 70.0 mm or less, more preferably 50.0 mm or less. In addition, the length (column length) of the adsorbent-filled space 20 is preferably about 10.0 mm or more and 300.0 mm or less, and more preferably about 20.0 mm or more and 200.0 mm or less, for example. In other words, the lower limit value of the length (column length) of the adsorbent-filled space 20 is preferably 10.0 mm or more, more preferably 20.0 mm or more, and the upper limit value of the length is preferably 300.0 mm or less, more preferably 200.0 mm or less. By separating the separation material contained in the sample liquid using the column 2 having the adsorbent-filled space 20 of such sizes (inner diameter and length), the separation material can be purified with excellent accuracy.

[0091] By setting the size of the adsorbent filling space 20 to the above-mentioned value and setting the size of the adsorbent 3 to be described later to the value to be described below, the target substance to be separated can be selectively separated (purified) from the sample liquid, that is, the separation material (substance to be adsorbed) such as protein and the contaminants other than the separation material contained in the sample liquid can be reliably separated from each other.

[0092] Note that the separation material to be separated (purified) using the adsorbent 3 is not limited to proteins (such as albumin), acidic proteins (such as antibodies (antibody molecules)), and basic proteins, and examples thereof include: negatively charged substances (such as acidic amino acids, DNA, RNA, and negatively charged liposomes); and positively charged substances (such as basic amino acids, positively charged cholesterol, and positively charged liposomes), among which proteins are preferably selected. That is, various substances including bio-based drugs (such as antibodies and vaccines) can be purified and separated as substances to be adsorbed by using the adsorbent 3.

[0093] In addition, the cover portions 22 , 23 are attached to the column main body 21 to ensure liquid-tightness between the cover portions 22 , 23 .

[0094] The cover portion 22 (first port) and the cover portion 23 (second port) include caps 28 and 29 , the inlet pipe 24 (first flow path) and the outlet pipe 25 (second flow path), and covers 26 and 27 , respectively.

[0095] Caps 28 and 29 are attached to the inflow side end (one end) and the outflow side end (the other end) of the column body 21 by threading, wherein the inflow side end of the column body 21 is located above in the vertical direction, and the outflow side end is located below in the vertical direction. Caps 28 and 29 and the column body 21 ensure liquid tightness between them.

[0096] The inlet tube 24 and the outlet tube 25 are respectively constituted of a tube body through which a liquid flows, and are respectively bonded (fixed) to the approximate center of the cap 28 and the cap 29 in a liquid-tight manner. The caps 26 and the caps 27 include flow paths 41 and 51, which are provided between the filter members 4 and 5 and the caps 28 and 29, and communicate with the inlet tube 24 and the outlet tube 25. The liquid is supplied to the adsorbent 3 via the inlet tube 24, the cap 26, and the filter member 4. The sample liquid supplied to the adsorbent 3 passes between (gaps) of the adsorbent 3, and flows out of the column 2 via the filter member 5, the cap 27, and the outlet tube 25. At this time, the separation material (substance to be adsorbed) contained in the sample liquid (sample) and the contaminant other than the separation material are separated from each other based on the difference in adsorption capacity to the adsorbent 3 and the difference in affinity to the eluent.

[0097] In other words, when the cover 22 is located above the cover 23 in the vertical direction, the adsorption device 1 supplies liquid to the adsorbent filling space 20 via the inlet pipe 24, adsorbs the separation material through the adsorbent 3 loaded in the adsorbent filling space 20, and separates the separation material using the adsorption effect of the separation material.

[0098] Each of the filter members 4 and 5 has a function of preventing the adsorbent 3 from flowing out of the adsorbent filling space 20, that is, a function of retaining the adsorbent 3 in the adsorbent filling space 20. Each of these filter members 4 and 5 is composed of, for example, a polypropylene mesh, a sintered filter of polyethylene particles, a stainless steel mesh filter, or a sintered filter of stainless steel particles.

[0099] In the adsorption device 1, the adsorbent 3 is made of sintered powder, which is obtained by sintering unfired powder (unsintered powder) including primary particles and secondary particles of hydroxyapatite into a powder formed of a large number of fine particles with a non-constant particle size, and thus has adsorption capacity for the separation material (substance to be adsorbed) contained in the sample liquid (sample).

[0100] Herein, the unfired powder (unsintered powder) including hydroxyapatite primary particles and secondary particles is referred to as "hydroxyapatite powder" (or simply "powder (unsintered powder)"), and the fired hydroxyapatite powder is referred to as "sintered hydroxyapatite powder" (or simply "sintered powder").

[0101] The sintered hydroxyapatite powder is loaded as the adsorbent 3 into the adsorbent filling space 20 of the column main body 21. In the present invention, the sintered hydroxyapatite powder is obtained by roasting the hydroxyapatite powder at a sintering temperature (calcination temperature) of 480 °C or higher and 645 °C or lower. Therefore, the sintered hydroxyapatite powder (i.e., the adsorbent 3) has improved durability and improved adsorption capacity for the substance to be adsorbed.

[0102] The sintered hydroxyapatite powder (sintered powder) as the adsorbent 3 will be described in detail below.

[0103] As described above, the sintered hydroxyapatite powder is obtained by roasting the hydroxyapatite powder at a sintering temperature of 480 °C or higher and 645 °C or lower. The hydroxyapatite powder (powder) is a porous body having fine pores, and the hydroxyapatite powder contains its secondary particles, and also contains primary particles and multi-stage particles, and is mainly composed of its secondary particles.

[0104] The secondary particles of hydroxyapatite (Ca 10 (PO4)6(OH)2) (i.e., the hydroxyapatite powder) are porous bodies mainly composed of hydroxyapatite, and the secondary particles of hydroxyapatite are obtained by drying a slurry containing primary particles and their aggregates to form particles. Hydroxyapatite has a chemically stable apatite structure. Desirably, the Ca / P ratio of hydroxyapatite is about 1.64 or higher and 1.70 or lower.

[0105] The hydroxyapatite secondary particles may be composed of fluorapatite [Ca 10 (PO4)6(OH) 2-2x F 2x , where x is 0 < x ≤ 1], and the secondary particles of the fluorapatite are formed by substituting at least a part of the hydroxy groups on its surface with fluorine atoms. Herein, hydroxyapatite (Ca 10 (PO4)6(OH)2) and fluorapatite [Ca 10 (PO4)6(OH) 2-2x F 2x , where x is 0 < x ≤ 1] are collectively referred to as "hydroxyapatite", as described above.

[0106] In the present invention, hydroxyapatite secondary particles (i.e., hydroxyapatite powder) are obtained by calcining hydroxyapatite powder at a sintering temperature of 480° C. or higher and 645° C. or lower. The obtained sintered hydroxyapatite powder (i.e., adsorbent 3 composed of a porous body having fine pores) has improved durability and improved adsorption capacity for a substance to be adsorbed, and specifically has the following configuration.

[0107] That is, the average particle compression strength of the sintered powder (adsorbent 3) satisfies the range of 7.4 MPa to 8.9 MPa, and the modal pore size in the pore size distribution of the pores of the sintered powder satisfies the range of 32.0 nm to 60.0 nm.

[0108] When the average particle compressive strength and modal pore size of the sintered powder are within the above ranges, the average particle size of the sintered powder is set within the range of 10 μm or more and 90 μm or less, preferably within the range of 20 μm or more and 80 μm or less, and more preferably within the range of 40 μm or more and 70 μm or less. When the average particle size of the sintered powder is within the above range, and when the average particle compressive strength and modal pore size are set within the above ranges, the effect obtained by setting the average particle compressive strength and modal pore size within the above ranges can be more significantly achieved.

[0109] The average particle compressive strength of the sintered powder may be 7.4 MPa or more and 8.9 MPa or less, but is preferably 8.0 MPa or more and 8.9 MPa or less, and more preferably 8.2 MPa or more and 8.7 MPa or less. In other words, the lower limit value of the average particle compressive strength of the sintered powder may be 7.4 MPa or more, but is preferably 8.0 MPa or more, and more preferably 8.2 MPa or more, and the upper limit value of the average particle compressive strength of the sintered powder may be 8.9 MPa or less, but is preferably 8.9 MPa or less, and more preferably 8.7 MPa or less. Therefore, it can be said that the sintered powder (ie, adsorbent 3) has further improved durability.

[0110] The modal pore size in the pore size distribution of the pores of the sintered powder (porous body) may be 32.0 nm or more and 60.0 nm or less, but preferably 35.0 nm or more and 60.0 nm or less, and more preferably 42.0 nm or more and 58.0 nm or less. In other words, the lower limit value of the modal pore size may be 32.0 nm or more, but preferably 35.0 nm or more, and more preferably 42.0 nm or more, and the upper limit value of the modal pore size may be 60.0 nm or less, but preferably 60.0 nm or less, and more preferably 58.0 nm or less. By setting the modal pore size within the above range, even relatively large proteins such as antibodies (antibody molecules) can be reliably adsorbed to the sintered powder by capturing them as separation materials in the pores of the sintered powder. Therefore, it can be said that the adsorption capacity of the sintered powder (i.e., the adsorbent 3) for the separation material (substance to be adsorbed) is further improved.

[0111] The frequency of the modal pore size in the pore size distribution of the pores of the sintered powder (porous body) is preferably 21.0% or more and 60.0% or less, more preferably 25.0% or more and 55.0% or less. In other words, the lower limit value of the frequency of the modal pore size is preferably 21.0% or more, more preferably 25.0% or more, and the upper limit value of the frequency of the modal pore size is preferably 60.0% or less, more preferably 55.0% or less.

[0112] The half width of the mountain-shaped waveform around the modal aperture (half width of the modal aperture) is 1.0 nm or more and 10.0 nm or less, more preferably 2.0 nm or more and 10.0 nm or less, further preferably 3.0 nm or more and 10.0 nm or less, and particularly preferably 5.0 nm or more and 10.0 nm or less. In other words, the lower limit value of the half width is preferably 1.0 nm or more, more preferably 2.0 nm or more, further preferably 3.0 nm or more, and particularly preferably 5.0 nm or more, and the upper limit value of the half width is preferably 10.0 nm or less.

[0113] By setting various values ​​in the pore size distribution of the pores of the sintered powder (porous body) within the above range, the effect obtained by setting the modal pore size within the above range can be more significantly achieved.

[0114] The average pore size of the pores of the sintered powder is preferably 37.0 nm or more and 75.0 nm or less, more preferably 41.0 nm or more and 58.0 nm or less. In other words, the lower limit value of the average pore size is preferably 37.0 nm or more, more preferably 41.0 nm or more, and the upper limit value of the average pore size is preferably 75.0 nm or less, more preferably 58.0 nm or less. Therefore, the effect obtained by setting the modal pore size within the above range can be more significantly achieved.

[0115] The specific surface area of ​​the sintered powder can be 41m 2 / g or more and 51m 2 / g or less, preferably 41m 2 / g or more and 49m 2 / g or less, more preferably 41m 2 / g or more and 47m 2 In other words, the lower limit of the specific surface area can be 41 m 2 / g or more, and the upper limit value of the specific surface area may be 51m 2 / g or less, preferably 49m 2 / g or less, more preferably 47m 2 / g or less. In addition, the surface area of ​​each 1mL of sintered powder in the column can be 25.3m 2 / mL and above 36.0m 2 / mL or less, but preferably 25.3m / mL 2 / mL and above 34.0m 2 / mL or less, more preferably 25.3m / mL 2 / mL and above 33.0m 2 / mL or less. In other words, the lower limit of the surface area can be 5.3m 2 / mL or more, and the upper limit can be 36.0m 2 / mL or less, but the upper limit is preferably 34.0m 2 / mL or less, more preferably 33.0m 2 / mL or less. By setting the specific surface area of ​​the sintered powder and the surface area per 1mL of the sintered powder of the column within the above ranges, respectively, even if the separation material (substance to be adsorbed) is a relatively large protein such as an antibody (antibody molecule), it can be said that the sintered powder has the surface area necessary to adsorb a sufficient amount of the separation material. Therefore, the sintered powder (i.e., the adsorbent 3) can have an improved adsorption capacity for the separation material (substance to be adsorbed).

[0116] The hydroxyapatite powder (i.e., the secondary particles of hydroxyapatite) that is calcined to obtain the sintered hydroxyapatite powder is not particularly limited, but its bulk density is preferably set to 0.65 g / mL or more, more preferably about 0.70 g / mL or more and 0.95 g / mL or less. In other words, the lower limit value of the bulk density is preferably 0.65 g / mL or more, more preferably 0.70 g / mL or more, and the upper limit value of the bulk density is more preferably 0.95 g / mL or less. Secondary particles having a bulk density within this range are considered to be heavier, have fewer voids in the particles, and it can be said that the packing density of the particles is higher, and therefore exhibit higher strength. Therefore, the hydroxyapatite powder obtained by calcining the hydroxyapatite powder containing the secondary particles also has a higher strength, so that the average particle compressive strength of the sintered powder can be relatively easily set within the above range.

[0117] The specific surface area of ​​the hydroxyapatite powder (hydroxyapatite secondary particles) is preferably set to 70 m 2 / g or more, more preferably about 75m 2 / g or more and 100m 2 In other words, the lower limit of the specific surface area is preferably 70 m 2 / g or more, more preferably 75m 2 / g or more, and the upper limit value of the specific surface area is more preferably about 100m 2 By calcining the hydroxyapatite powder having a high specific surface area within such a range, the specific surface area of ​​the resulting sintered hydroxyapatite powder can be set within the above range relatively easily.

[0118] In addition, the morphology (shape) of the hydroxyapatite powder is preferably granular (particle-like), but its sphericity or spherical diameter sphericity is more preferably about 0.95 or more and 1.00 or less, and further preferably 0.97 or more and 1.00 or less. In other words, the lower limit value of the spherical diameter sphericity is preferably 0.95 or more, more preferably 0.97 or more, and the upper limit value of the spherical diameter sphericity is preferably 1.00 or less. In this way, when a sintered powder made of a hydroxyapatite powder having a higher spherical diameter sphericity is applied as the adsorbent 3, the filling rate of the adsorbent 3 into the adsorbent filling space 20 can be increased.

[0119] As described above, in the present invention, the sintered powder (adsorbent 3) satisfies the average particle compressive strength of 7.4 MPa or more and 8.9 MPa or less, and the modal pore size in the pore size distribution of the pores of the sintered powder is 32.0 nm or more and 60.0 nm or less, thereby having improved durability and improved adsorption capacity for substances to be adsorbed. Specifically, the durability and adsorption capacity show the following characteristics.

[0120] In other words, when the durability test shown below was performed on the sintered hydroxyapatite powder, the durability test could be performed 60 cycles or more, so it can be said that the sintered hydroxyapatite powder has improved durability.

[0121] Specifically, the durability test includes preparing a column (φ4.0×100 mm) dry-packed with sintered hydroxyapatite powder as an adsorbent, and feeding each buffer into the column in the order of the step numbers shown in Table 2 below. Steps 1 to 5 in Table 2 below count as one cycle, and the cycle is repeated until the pressure inside the column exceeds 200 psi. When the durability test is performed on sintered hydroxyapatite powder (adsorbent of the present invention), the number of cycles repeated may be 60 times or more.

[0122] [Table 2]

[0123]

[0124] As described above, the sintered hydroxyapatite powder has improved durability because it can perform 60 cycles or more in the durability test. The number of cycles may be 60 times or more, but is preferably 80 times or more, more preferably 100 times or more, which indicates that the sintered hydroxyapatite powder has improved durability.

[0125] In addition, when the antibody adsorption amount measurement test shown below is performed, the sintered hydroxyapatite powder satisfies the following relationship, and the adsorption amount of the antibody as a substance to be adsorbed by the sintered hydroxyapatite powder is independent of the flow rate (flow rate) of the test liquid containing the antibody supplied to the column, so it can be said that the sintered hydroxyapatite powder has an improved adsorption capacity for the substance to be adsorbed.

[0126] Specifically, in this antibody adsorption amount measurement test, a column (φ6.0×35 mm) in which sintered hydroxyapatite powder as an adsorbent was dry-packed was prepared, and a sample liquid was prepared by dissolving γ-globulin from bovine blood (as a substance to be adsorbed) in 10 mM sodium phosphate buffer (pH 6.5) so that the concentration was 1.0 mg / mL. Then, the prepared sample liquid was supplied to the column at flow rates of 150 cm / h, 200 cm / h, 250 cm / h, and 300 cm / h. For each flow rate, the absorbance value X (280 nm) of the sample liquid supplied to the column and the absorbance value Y (wavelength: 280 nm) of the eluate eluted from the column were measured, and the adsorption amounts A (mg / mL), B (mg / mL), C (mg / mL), and D (mg / mL) of the substance adsorbed to the sintered hydroxyapatite powder were calculated based on the amount of the sample liquid transported until the absorbance value Y (wavelength: 280 nm) became 10% of the absorbance value X (wavelength: 280 nm). When such an antibody adsorption amount measurement test was performed on the sintered hydroxyapatite powder (the adsorbent of the present invention), the relational expressions D / A, D / B, and C / B were determined based on the adsorption amounts A to D (mg / mL) of the substance to be adsorbed calculated in the antibody adsorption amount measurement test. The relationship D / A satisfies at least one of A≥31 mg / mL or greater and 0.60≤D / A≤1.00, and 0.60≤D / A≤0.92, the relationship D / B satisfies at least one of B≥30 mg / mL or greater and 0.75≤D / B≤1.00, and 0.75≤D / B≤0.96, and the relationship C / B satisfies at least one of B≥30 mg / mL or greater and 0.89≤C / B≤1.00, and 0.89≤C / B≤0.96.

[0127] In this way, the sintered hydroxyapatite powder can make the relationship equations D / A, D / B, and C / B calculated in the antibody adsorption amount measurement test satisfy the above relationship, respectively. Therefore, it can be said that the adsorption amount of the antibody (substance to be adsorbed) by the sintered hydroxyapatite powder is independent of the flow rate (flow rate) of the test liquid containing the antibody supplied to the column. Therefore, during the separation and purification of the antibody using the adsorption device 1 including the sintered hydroxyapatite powder as the adsorbent 3, for example, when the sample liquid containing the antibody is supplied to the adsorption device 1, even if the sample liquid cannot be supplied at a constant rate and thus non-uniformity occurs in the initial stage and the final stage, the antibody can be reliably adsorbed to the sintered hydroxyapatite powder within a constant adsorption amount range.

[0128] The relationship D / A may satisfy at least one of A≥31 mg / mL or more and 0.60≤D / A≤1.00, and 0.60≤D / A≤0.92, but preferably satisfies 0.61≤D / A≤0.88. The relationship D / B may satisfy at least one of B≥30 mg / mL or more and 0.75≤D / B≤1.00, and 0.75≤D / B≤0.96, but preferably satisfies 0.76≤D / B≤0.90. The relationship C / B satisfies at least one of B≥30 mg / mL or more and 0.89≤C / B≤1.00, and 0.89≤C / B≤0.96, but preferably satisfies 0.89≤C / B≤0.95. It can be said that these relationships allow the sintered hydroxyapatite powder to have an improved adsorption capacity for substances to be adsorbed.

[0129] In this antibody adsorption amount measurement test, the adsorption amount A to D of the substance to be adsorbed is preferably about 30 mg / mL to 31 mg / mL or more, more preferably about 34 mg / mL or more, and further preferably about 37 mg / mL or more and 45 mg / mL or less. In other words, the lower limit value of each of the adsorption amounts A to D is preferably about 30 mg / mL to 31 mg / mL or more, more preferably about 34 mg / mL or more, and further preferably about 37 mg / mL, and the upper limit value of each of the adsorption amounts A to D is further preferably about 45 mg / mL or less. Therefore, even if the separation material (substance to be adsorbed) to be separated using the adsorbent 3 is a relatively large protein such as an antibody (antibody molecule), it can be said that the adsorbent 3 is capable of adsorbing a sufficient amount of the separation material.

[0130] <Method for producing sintered hydroxyapatite powder>

[0131] For example, the above-mentioned sintered hydroxyapatite powder (ie, adsorbent 3) is produced by the following adsorbent production method.

[0132] Note that the following case is used as an example to explain: hydroxyapatite powder is used to obtain sintered hydroxyapatite powder, and a bulk density of 0.65 g / mL or more and a specific surface area of ​​70 m 2 / g or more of hydroxyapatite powder.

[0133] In this embodiment, the method for manufacturing powder includes: step [S1A], reacting a first liquid containing a calcium source (such as calcium hydroxide) with a second liquid containing a phosphorus source (such as phosphoric acid) while stirring to obtain a slurry containing primary particles of hydroxyapatite and aggregates thereof; step [S2A], physically crushing the aggregates contained in the slurry and dispersing the crushed aggregates in the slurry; step [S3A], drying the slurry to granulate the crushed aggregates to obtain hydroxyapatite powder composed of particles mainly containing secondary particles of hydroxyapatite; and step [S4A]: calcining the hydroxyapatite powder to obtain sintered hydroxyapatite powder.

[0134] These steps are described below in order.

[0135] Note that the description is given taking as an example the case where calcium hydroxide is used as a calcium source, and phosphoric acid is used as a phosphorus source.

[0136] [S1A: Step of forming a slurry containing hydroxyapatite aggregates]

[0137] In this step, a calcium hydroxide dispersion (first liquid) containing calcium hydroxide and a phosphoric acid solution (second liquid) containing phosphoric acid are stirred to react calcium hydroxide with phosphoric acid to form a slurry containing primary hydroxyapatite particles and aggregates thereof. That is, a slurry containing primary hydroxyapatite particles and aggregates thereof is prepared.

[0138] Specifically, for example, by stirring the calcium hydroxide dispersion (first liquid) in a container (not shown), a phosphoric acid solution (second liquid) is added dropwise to the calcium hydroxide dispersion (first liquid) to form a mixed liquid of the calcium hydroxide dispersion and the phosphoric acid solution, so that the calcium hydroxide reacts with the phosphoric acid in the mixed liquid.

[0139] This method adopts a wet synthesis method using a phosphoric acid solution containing phosphoric acid, which does not require expensive manufacturing equipment and can synthesize hydroxyapatite (compound) more simply and efficiently. In addition, the reaction has the advantage that since the reaction between calcium hydroxide and phosphoric acid produces only water as a by-product, no by-products remain in the obtained secondary particles and sintered powder. In addition, since the reaction is an acid-base reaction, the reaction can be simply controlled by adjusting the pH value of the calcium hydroxide dispersion and the phosphoric acid solution.

[0140] The phosphoric acid solution containing phosphoric acid may be an aqueous phosphoric acid solution to which a small amount of other liquid such as alcohol may be added.

[0141] Stirring can effectively promote the reaction between calcium hydroxide and phosphoric acid, that is, can enhance the efficiency of the reaction.

[0142] The power of stirring the mixed solution containing calcium hydroxide dispersion and phosphoric acid solution is not particularly limited, but preferably about 0.75W or more and 2.0W or less per 1L mixed solution (slurry), more preferably about 0.925W or more and 1.85W or less. In other words, the lower limit of the stirring power per 1L mixed solution (slurry) is preferably 0.75W or more, more preferably 0.925W or more, and the upper limit of the stirring power is preferably 2.0W or less, more preferably 1.85W or less. By setting the stirring power within this range, the reaction efficiency between calcium hydroxide and phosphoric acid can be further improved.

[0143] The content of calcium hydroxide in the calcium hydroxide dispersion is preferably about 5% by mass or more and 15% by mass or about 5% by mass or more and 15% by mass, more preferably about 10% by mass or more and 12% by mass or less. In other words, the lower limit of the content of calcium hydroxide is preferably 5% by mass or more, more preferably 10% by mass or more, and the upper limit of the content of calcium hydroxide is preferably 15% by mass or less, more preferably 12% by mass or less. The content of phosphoric acid in the phosphoric acid solution is preferably about 10% by mass or more and 25% by mass or less, more preferably about 15% by mass or more and 20% by mass or less. In other words, the lower limit of the content of phosphoric acid is preferably 10% by mass or more, more preferably 15% by mass or more, and the upper limit of the content of phosphoric acid is preferably 25% by mass or less, more preferably 20% by mass or less. By setting the contents of calcium hydroxide and phosphoric acid within these ranges, when the phosphoric acid solution is added dropwise to the calcium hydroxide dispersion while stirring the calcium hydroxide dispersion, the contact opportunity between calcium hydroxide and phosphoric acid increases, so calcium hydroxide can efficiently react with phosphoric acid, thereby reliably synthesizing hydroxyapatite.

[0144] The dropping speed of phosphoric acid solution is preferably about 1L / hour or more and 40L / hour or less, more preferably about 3L / hour or more and 30L / hour or less. In other words, the lower limit of the dropping speed of phosphoric acid solution is preferably 1L / hour or more, and more preferably 3L / hour or more, and the upper limit of the dropping speed of phosphoric acid solution is preferably 40L / hour or less, more preferably 30L / hour or less. By mixing (adding) phosphoric acid solution in the calcium hydroxide dispersion liquid with this dropping speed, calcium hydroxide and phosphoric acid can be reacted under milder conditions.

[0145] In this case, the dropping time (addition time) of phosphoric acid solution is preferably about 5 hours or more and 32 hours or less, more preferably about 6 hours or more and 30 hours or less. In other words, the lower limit of the dropping time of phosphoric acid solution is preferably 5 hours or more, more preferably 6 hours or more, and the upper limit of the dropping time of phosphoric acid solution is preferably 32 hours or less, and more preferably 30 hours or less. By reacting calcium hydroxide with phosphoric acid for this dropping time, hydroxyapatite can be fully synthesized. It is noted that even if the dropping time is made longer than the above-mentioned upper limit, the reaction between calcium hydroxide and phosphoric acid cannot be expected to proceed further.

[0146] As the reaction between calcium hydroxide and phosphoric acid gradually proceeds, fine particles of hydroxyapatite (compound) (hereinafter, referred to as "fine particles") are generated in the slurry. Then, the fine particles aggregate by the van der Waals force (intermolecular force) generated between the positively charged part of one fine particle (primary particle) and the negatively charged part of another fine particle, thereby forming aggregates of hydroxyapatite (compound) (hereinafter, referred to as aggregates). As the aggregates are formed, the viscosity of the slurry gradually increases.

[0147] In addition, as the reaction between calcium hydroxide and phosphoric acid proceeds, the ratio of positive charge to negative charge in the slurry tends to be equal. At this time, the repulsive force applied to the fine particles in the slurry decreases, thereby accelerating the aggregation of the fine particles to form aggregates with larger particle size.

[0148] [S2A: Step of comminuting and dispersing aggregates]

[0149] In this step, aggregates of primary particles of hydroxyapatite contained in the slurry obtained in step [S1A] are physically pulverized, and the pulverized aggregates are dispersed in the slurry.

[0150] By pulverizing the aggregates contained in the slurry as described above, the particle size of the aggregates contained in the slurry becomes smaller, so that the secondary particles of hydroxyapatite obtained in the subsequent step [S3A] can have a bulk density of 0.65 g / mL or more and a particle size of 70 m / s. 2 / g or greater specific surface area.

[0151] The method for physically pulverizing the aggregates of primary particles of hydroxyapatite is not particularly limited, but includes, for example, a wet jet milling method (in which droplets of a slurry jetted under high pressure are caused to collide with each other) and a ball milling method (in which a slurry is placed in a closed container in the form of a sphere made of ceramics such as zirconia, and the closed container is rotated). Among them, the wet jet milling method is preferred.

[0152] The wet jet milling method is a method in which high pressure is applied to a slurry in which aggregates of primary particles of hydroxyapatite are dispersed, and the slurry is sprayed into droplets, which are then introduced into an opposed collision chamber, a ball collision chamber, or a single nozzle chamber, where the aggregates are crushed by causing collisions between the aggregates.

[0153] According to this method, aggregates of primary particles of hydroxyapatite can be reliably pulverized. Therefore, the secondary particles of hydroxyapatite obtained in the subsequent step [S3A] can be set to have a bulk density of 0.65 g / mL or more.

[0154] In addition, the average particle size of the pulverized aggregates is preferably 1 μm or less, more preferably 0.1 μm or more and 0.6 μm or less. By controlling the average particle size of the pulverized aggregates within this range, the volume density and specific surface area of ​​the secondary particles of hydroxyapatite obtained in the subsequent step [S3A] can be set within the above range.

[0155] As in this embodiment, when the secondary particles of hydroxyapatite obtained in the subsequent step [S3A] are not set to have a bulk density of 0.65 g / mL or more and a particle size of 70 m 2 / g or more, the physical pulverization of the aggregates in step [S2A] can be omitted. However, by physically pulverizing the aggregates to set the bulk density of the secondary particles to 0.65 g / mL or more and the specific surface area to 70 m 2 / g or more, when the hydroxyapatite powder is calcined at a sintering temperature of about 480°C or more and 645°C or less in the subsequent step [S4A], the resulting sintered hydroxyapatite powder can reliably have both improved durability and improved adsorption capacity for the substance to be adsorbed. In other words, the sintered hydroxyapatite powder can satisfy an average particle compressive strength of 7.4 MPa or more and 8.9 MPa or less, and a modal pore size of 32.0 nm or more and 60.0 nm or less.

[0156] [S3A: Step of drying the slurry to obtain hydroxyapatite powder]

[0157] In this step, the slurry containing the pulverized aggregates prepared in step [S2A] is dried to granulate the pulverized aggregates into an unsintered powder (dry powder) mainly composed of hydroxyapatite secondary particles, ie, hydroxyapatite powder.

[0158] In this embodiment, in step [S2A], the aggregates of the primary particles of hydroxyapatite are crushed, so the size of the aggregates is small, which can provide the hydroxyapatite powder obtained in step [S3A] with a volume density of 0.65 g / mL or more and a volume density of 70 m / mL or more. 2 / g or greater specific surface area.

[0159] The method of drying the slurry is not particularly limited, but a spray drying method is preferred. According to this method, the pulverized aggregate is granulated, so that a powder having a desired particle size can be obtained more reliably and in a shorter time.

[0160] The temperature at which the slurry is dried is preferably about 75° C. or more and 250° C. or less, more preferably about 95° C. or more and 220° C. or less. In other words, the lower limit value of the drying temperature is preferably 75° C. or more, more preferably 95° C. or more, and the upper limit value of the drying temperature is preferably 250° C. or less, more preferably 220° C. or less. By setting the drying temperature within this range, secondary particles having a higher bulk density and a larger specific surface area can be obtained.

[0161] The above steps [S1A] to [S3A] constitute the first step of preparing hydroxyapatite powder.

[0162] Note that, unlike this embodiment, when the hydroxyapatite secondary particles obtained in the subsequent step [S3A] are not set to have a bulk density of 0.65 g / mL or more and a particle size of 70 m 2 When the specific surface area is 0.17777 W / g or more, the hydroxyapatite powder does not need to be adjusted through the above steps [S1A] to [S3A] and can be prepared, for example, according to the method described in the specification of JP7-88205A.

[0163] [S4A: Step of calcining hydroxyapatite powder to obtain sintered hydroxyapatite powder]

[0164] In this step, the hydroxyapatite powder produced in the above step [S3A] is sintered by firing to produce a sintered powder composed of hydroxyapatite powder secondary particles, ie, sintered hydroxyapatite powder (second step).

[0165] In this case, the sintering temperature for calcining the powder may be set to about 480° C. or more and 645° C. or less, but preferably about 500° C. or more and 630° C. or less, more preferably 550° C. or more and 610° C. or less. In other words, the lower limit value of the sintering temperature may be 480° C. or more, but preferably 500° C. or more, more preferably 550° C. or more, and the upper limit value of the sintering temperature may be 645° C. or less, but preferably 630° C. or less, more preferably 610° C. or less.

[0166] The time for maintaining the sintering temperature for calcining the powder is not particularly limited, but is preferably about 60 minutes or more and 230 minutes or less, more preferably about 90 minutes or more and 180 minutes or less. In other words, the lower limit value of the holding time is preferably 60 minutes or more, more preferably 90 minutes or more, and the upper limit value of the holding time is preferably 230 minutes or less, and more preferably 180 minutes or less.

[0167] By setting the conditions for calcining the powder within the above range, it is relatively easy to make the average particle compressive strength of the obtained sintered hydroxyapatite powder (adsorbent 3) be greater than 7.4 MPa and less than 8.9 MPa, and the modal pore size in the pore size distribution of the pores of the sintered powder be greater than 32.0 nm and less than 60.0 nm.

[0168] Through the above steps, a sintered powder consisting of sintered particles mainly containing hydroxyapatite secondary particles, that is, sintered hydroxyapatite powder is obtained.

[0169] By loading the sintered hydroxyapatite powder as the adsorbent 3 into the adsorbent loading space 20 of the column 2, the adsorption device 1 can be obtained. When the sintered hydroxyapatite powder to be loaded is classified, the average particle size and particle size distribution of the sintered hydroxyapatite powder can be, for example, 20±4μm, 40±4μm, 60±4μm, 80±4μm, etc.

[0170] Although the adsorbent of the present invention and the method for producing the same are described above, the present invention is not limited thereto.

[0171] For example, various components of the adsorbent of the present invention may be replaced with any component that performs the same function, and the adsorbent of the present invention may be supplemented with any component. In addition, in the method for producing the adsorbent of the present invention, one or more steps may be added for any purpose.

[0172] Example

[0173] Next, specific embodiments of the present invention will be described.

[0174] Note that the present invention is not limited to the description of these embodiments.

[0175] 1. Preparation of sintered hydroxyapatite powder

[0176] (Example 1)

[0177] [1A] 2400 g of calcium hydroxide was dispersed in 60 L of pure water, and the obtained calcium hydroxide dispersion was supplied to a tank. While the calcium hydroxide dispersion was stirred, 4 L of an aqueous phosphoric acid solution (phosphoric acid concentration: 85% by mass) was added dropwise to the calcium hydroxide dispersion at a rate of 1 L / hour to obtain a slurry containing 10% by mass of aggregates of hydroxyapatite primary particles.

[0178] The atmospheric temperature during the dropwise addition was room temperature (25° C.).

[0179] The force for stirring the mixed liquid (in which the phosphoric acid aqueous solution was dropped into the dispersion liquid) was 1.7 W per 1 L of the mixed liquid (slurry).

[0180] [2A] The aggregates contained in the obtained slurry were pulverized at a high pressure of 245 MPa using a wet jet mill ("Star Burst" manufactured by Suyoshino Machinery Co., Ltd.) to obtain a slurry containing pulverized aggregates having an average particle size of 1.3 μm.

[0181] The average particle size of aggregates contained in the slurry after the pulverization was measured using a particle size distribution analyzer ("MT3300" manufactured by Microtrac Inc.).

[0182] [3A] The slurry containing the pulverized (dispersed) aggregates was spray-dried at 210° C. using a spray dryer (“MAD-6737R” manufactured by Panasonic Corporation) to form hydroxyapatite contained in the slurry into particles, thereby obtaining spherical secondary particles (dried powder). The obtained dry powder (i.e., hydroxyapatite powder) was classified using an ultrasonic sieve to obtain a hydroxyapatite powder having an average particle size of about 40 μm, more specifically, a hydroxyapatite powder having a particle size of 40 μm±4.0 μm.

[0183] The powder (secondary particles) was confirmed to be hydroxyapatite by powder X-ray diffraction.

[0184] [4A] The classified hydroxyapatite powder was calcined at a sintering temperature of 500° C. to obtain the sintered hydroxyapatite powder of Example 1.

[0185] (Example 2)

[0186] The sintered hydroxyapatite powder of Example 2 was obtained in the same manner as in Example 1, except that the sintering temperature for calcining the hydroxyapatite powder was changed to 600° C. in step [4A].

[0187] (Comparative Example 1)

[0188] The sintered hydroxyapatite powder of Comparative Example 1 was obtained in the same manner as in Example 1, except that the sintering temperature for calcining the hydroxyapatite powder was changed to 400° C. in step [4A].

[0189] (Comparative Example 2)

[0190] The sintered hydroxyapatite powder of Comparative Example 2 was obtained in the same manner as in Example 1, except that the sintering temperature for calcining the hydroxyapatite powder was changed to 700° C. in step [4A].

[0191] 2. Evaluation of sintered hydroxyapatite powder

[0192] 2-1. Evaluation of average particle compressive strength

[0193] The average particle compressive strength of the sintered hydroxyapatite powder of each of Examples and Comparative Examples was determined using a micro compression tester ("MCT-W200-J" manufactured by Shimadzu Corporation).

[0194] The average particle compressive strength of the sintered hydroxyapatite powder of each example and comparative example was obtained by measuring the particle compressive strength 10 times and calculating the average value. The calculation results are shown in Table 3.

[0195] [Table 3]

[0196]

[0197] As can be seen from Table 3, for the sintered powders of the examples and comparative examples, by setting the sintering temperature of the hydroxyapatite powder to a high level, a sintered hydroxyapatite powder having excellent particle compressive strength can be obtained.

[0198] 2-2. Evaluation of pore size

[0199] For the sintered hydroxyapatite powder of each example and comparative example, the pore size distribution on the surface of the pores was measured by the mercury pressure difference method using a pore size distribution measuring device ("Micromeritics Auto Pore 9200" manufactured by Shimadzu Corporation). From the pore size distribution, the modal pore size, the frequency of the modal pore size, the half width of the mountain-shaped waveform around the modal pore size (half width of the modal pore size), and the average pore size were calculated. The calculation results are shown in Table 4.

[0200] [Table 4]

[0201]

[0202] As can be seen from Table 4, for the sintered powders of the examples and comparative examples, by setting the sintering temperature of the hydroxyapatite powder to a high level, a sintered hydroxyapatite powder having a larger pore size was obtained.

[0203] 2-3. Evaluation of specific surface area

[0204] The specific surface area (average specific surface area) of the sintered hydroxyapatite powder of each example and comparative example was measured using a fully automatic BET specific surface area measuring device ("Macsorb HM1201" manufactured by Mountech Co., Ltd.).

[0205] [Table 5]

[0206]

[0207] As can be seen from Table 5, for the sintered powders of the examples and comparative examples, the specific surface area tends to decrease as the sintering temperature of the hydroxyapatite powder is set higher.

[0208] 2-4. Evaluation of the surface area of ​​sintered powder per 1 mL of column

[0209] The surface area per 1 mL of the column of the sintered powder of each example and comparative example was calculated from the data obtained by the evaluation of the specific surface area.

[0210] [Table 6]

[0211]

[0212] As can be seen from Table 6, for the sintered powders of the examples and comparative examples, the surface area and specific surface area per 1 mL of the column tend to decrease by setting the sintering temperature of the hydroxyapatite powder to a higher level.

[0213] 2-5. Evaluation of antibody adsorption

[0214] For a column filled with sintered hydroxyapatite powder of each example and comparative example as an adsorbent, a sample liquid containing an antibody was supplied to the column at a flow rate of 150 cm / hour, 200 cm / hour, 250 cm / hour, and 300 cm / hour, respectively, and the amount of antibody adsorbed by the adsorbent was measured using the method shown below.

[0215] First, γ-globulin (bIgG) from bovine blood was dissolved in 10 mM NaP (sodium phosphate buffer) at pH 6.5 so that the concentration became 1.0 mg / mL to prepare a sample liquid (bIgG solution).

[0216] Next, a column (φ6.0×35 mm) was prepared, the sintered hydroxyapatite powder of each example and comparative example was dry-packed as an adsorbent in the column, and the prepared sample liquid was transferred and supplied to the column from a chromatography pump at flow rates of 150 cm / hour, 200 cm / hour, 250 cm / hour, and 300 cm / hour, respectively. Then, the absorbance value X (wavelength: 280 nm) of the sample liquid supplied to the column and the absorbance value Y (wavelength: 280 nm) of the eluate eluted from the column were measured, and the sample liquid was transferred until the absorbance value Y (wavelength: 280 nm) reached 10% of the absorbance value X (wavelength: 280 nm).

[0217] Based on the amount of sample liquid, the adsorption amounts A to D (mg / mL) of the sintered hydroxyapatite powders of each example and comparative example on bIgG were calculated. Based on the calculated adsorption amounts A to D (mg / mL), the adsorption amount ratios D / A, D / B, and C / B were also calculated. The calculation results are shown in Tables 7 and Figure 3 shown.

[0218] [Table 7]

[0219]

[0220] Note*1: Adsorption amount at a flow rate of 150 cm / hour

[0221] Note*2: Adsorption amount at a flow rate of 200 cm / hour

[0222] Note*3: Adsorption amount at a flow rate of 250 cm / hour

[0223] Note*4: Adsorption amount at a flow rate of 300 cm / hour

[0224] As can be seen from Table 7, the sintered powder of each example is not affected by the flow rate (flow rate) of supplying the antibody-containing test liquid to the column, as compared with the sintered powder of each comparative example.

[0225] 2-6. Durability evaluation

[0226] The durability of the adsorbent in the column containing the sintered hydroxyapatite powder as the adsorbent of each of the Examples and Comparative Examples was evaluated using the following method.

[0227] First, a column (φ4.0×100 mm) was prepared, and the sintered hydroxyapatite powder of each example and comparative example was dry-packed as an adsorbent in the column. Herein, dry packing means that the dry sintered hydroxyapatite powder was added to the column and tapped 120 times by hand to tightly pack the sintered powder without breaking the sintered powder.

[0228] Next, each buffer was supplied to the columns in the order of the step numbers shown in Table 8. Steps 1 to 5 were counted as one cycle, and the cycles were repeated until the pressure inside the column exceeded 200 psi. The results of the cycle are shown in Table 9.

[0229] [Table 8]

[0230]

[0231] [Table 9]

[0232]

[0233] As can be seen from Table 9, the sintered powder of each example has improved durability compared with the sintered powder of each comparative example.

[0234] 2-7. Summary

[0235] As described above, in step [4A], by setting the sintering temperature during sintering of the hydroxyapatite powder to a temperature range of greater than 480°C and less than 645°C, it has been found that the resulting sintered powder has an average particle compressive strength of 7.4 MPa or greater, and the modal pore size in the pore size distribution of the pores of the sintered powder is greater than 32.0 nm and less than 60.0 nm.

[0236] It has also been shown that by using sintered powder having both an average particle compressive strength and a modal pore size within the above ranges as the adsorbent 3 in the adsorption device 1 , the adsorbent 3 in the adsorption device 1 has improved durability and improved adsorption capacity for substances to be adsorbed.

[0237] Reference numerals list

[0238] 1 Adsorption device

[0239] 2 columns

[0240] 3 Adsorbent

[0241] 4 Filter components

[0242] 5 Filter components

[0243] 20 Adsorbent filling space

[0244] 21 Column body

[0245] 22 cover

[0246] 23 cover

[0247] 24 Inlet pipe

[0248] 25 outlet pipe

[0249] 26 Cover

[0250] 27 Cover

[0251] 28 Cap

[0252] 29 Cap

[0253] 41 flow path

[0254] 51 flow path

Claims

1. An adsorbent to be loaded into a column and composed of a powder containing particles whose surfaces are made of hydroxyapatite or fluoroapatite in which at least some of the hydroxyl groups in the hydroxyapatite are substituted with fluorine atoms, The powder is composed of a porous body having pores, The average particle size of the powder is 10 μm or more and 90 μm or less, The average particle compressive strength of the powder is 7.4 MPa or more and 8.9 MPa or less, and The modal pore diameter in the pore size distribution of the pores of the powder is 32.0 nm or more and 60.0 nm or less.

2. The adsorbent according to claim 1, wherein the specific surface area of ​​the powder is 41 m 2 / g or more and 51m 2 / g or less.

3. The adsorbent according to claim 1, wherein the surface area of ​​the column per 1 mL of powder is 25.3 m 2 / mL and above 36.0m 2 / mL or less.

4. An adsorbent to be loaded into a column and composed of a sintered powder obtained by calcining particles, the surfaces of which are made of hydroxyapatite or fluoroapatite in which at least some of the hydroxyl groups in the hydroxyapatite are substituted with fluorine atoms, The average particle size of the sintered powder is 10 μm or more and 90 μm or less. The specific surface area of ​​the sintered powder is 41 m 2 / g or more and 51m 2 / g or less, and The modal pore diameter in the pore size distribution of the sintered powder is 32.0 nm or more and 60.0 nm or less.

5. An adsorbent to be loaded into a column and composed of a powder containing particles whose surfaces are made of hydroxyapatite or fluoroapatite in which at least some of the hydroxyl groups in the hydroxyapatite are substituted with fluorine atoms, The average particle size of the powder is 10 μm or more and 90 μm or less, The surface area of ​​the column per 1 mL of powder is 25.3 m 2 / mL and above 36.0m 2 / mL or less, and The modal pore diameter in the pore size distribution of the pores of the powder is 32.0 nm or more and 60.0 nm or less. 6 . The adsorbent according to claim 1 , wherein the frequency of the modal pore size is 21.0% or more and 60.0% or less. 7 . The adsorbent according to claim 1 , wherein a half width of a mountain-shaped waveform around a modal pore size in a pore size distribution of the pores is 1.0 nm or more and 10.0 nm or less. 8 . The adsorbent according to claim 1 , wherein an average pore diameter of the pores is 37.0 nm or more and 75.0 nm or less. 9 . The adsorbent according to claim 1 , wherein the powder is a sintered powder calcined at 480° C. or higher and 645° C. or lower.

10. A method for making an adsorbent, comprising: The first step is to prepare particles, wherein the surface of the particles is made of hydroxyapatite or fluoroapatite in which at least some hydroxyl groups in the hydroxyapatite are substituted with fluorine atoms; and The second step: calcining the particles prepared in the first step at a temperature T in the range of 480° C. to 645° C. to obtain a sintered powder of the particles; The sintered powder obtained in the second step has an average particle size of 10 μm or more and 90 μm or less, an average particle compressive strength of 7.4 MPa or more and 8.9 MPa or less, and a pore diameter of 32.0 nm or more and 60.0 nm or less.

11. A method for making an adsorbent, comprising: The first step is to prepare particles, wherein the surface of the particles is made of hydroxyapatite or fluoroapatite in which at least some hydroxyl groups in the hydroxyapatite are substituted with fluorine atoms; and The second step: calcining the particles prepared in the first step at a temperature T in the range of 480° C. to 645° C. to obtain a sintered powder of the particles; The average particle size of the sintered powder obtained in the second step is 10 μm or more and 90 μm or less, and the specific surface area is 41 m 2 / g or more and 51m 2 / g or less, and the pore diameter is 32.0nm or more and 60.0nm or less.

12. A method for making an adsorbent, comprising: The first step is to prepare particles, wherein the surface of the particles is made of hydroxyapatite or fluoroapatite in which at least some hydroxyl groups in the hydroxyapatite are substituted with fluorine atoms; and The second step: calcining the particles prepared in the first step at a temperature T in the range of 480° C. to 645° C. to obtain a sintered powder of the particles; The average particle size of the sintered powder obtained in the second step is 10 μm or more and 90 μm or less, When the sintered powder was loaded into the column, the surface area of ​​the column per 1 mL of sintered powder was 25.3 m 2 / mL and above 36.0m 2 / mL or less, and The pore diameter is 32.0 nm or more and 60.0 nm or less.

13. An adsorbent to be loaded into a column and composed of a powder containing particles whose surfaces are made of hydroxyapatite or fluoroapatite in which at least some of the hydroxyl groups in the hydroxyapatite are substituted with fluorine atoms, wherein When a sample liquid was prepared by dissolving γ-globulin from bovine blood as a substance to be adsorbed in 10 mM sodium phosphate buffer (pH 6.5) so that the concentration was 1.0 mg / mL, and the prepared sample liquid was supplied to the column (φ6.0×35 mm) at flow rates of 150 cm / h and 300 cm / h, and when for each flow rate, the absorbance value X (280 nm) of the sample liquid to be supplied to the column and the absorbance of the eluate eluted from the column were measured. When the absorbance value Y (wavelength: 280 nm) is measured and the adsorption amount A (mg / mL) and D (mg / mL) of the substance to be adsorbed on the powder are calculated based on the amount of the sample liquid transported until the absorbance value Y (wavelength: 280 nm) becomes 10% of the absorbance value X (wavelength: 280 nm), the powder satisfies at least one of A ≥ 31 mg / mL or more, 0.60 ≤ D / A ≤ 1.00, and 0.60 ≤ D / A ≤ 0.

92.

14. An adsorbent to be loaded into a column and composed of a powder obtained by baking particles whose surfaces are made of hydroxyapatite or fluoroapatite in which at least some of the hydroxyl groups in the hydroxyapatite are substituted with fluorine atoms, wherein When a sample liquid was prepared by dissolving γ-globulin from bovine blood as a substance to be adsorbed in 10 mM sodium phosphate buffer (pH 6.5) so that the concentration was 1.0 mg / mL, and the prepared sample liquid was supplied to the column (φ6.0×35 mm) at flow rates of 200 cm / h and 300 cm / h, and when for each flow rate, the absorbance value X (280 nm) of the sample liquid to be supplied to the column and the absorbance value X (280 nm) of the eluate eluted from the column were measured. When the absorbance value Y (wavelength: 280 nm) is measured and the adsorption amount B (mg / mL) and D (mg / mL) of the substance to be adsorbed on the powder are calculated based on the amount of the sample liquid transported until the absorbance value Y (wavelength: 280 nm) becomes 10% of the absorbance value X (wavelength: 280 nm), the powder satisfies at least one of B ≥ 30 mg / mL or more, 0.75 ≤ D / B ≤ 1.00, and 0.75 ≤ D / B ≤ 0.

96.

15. An adsorbent to be loaded into a column and composed of a powder obtained by baking particles whose surfaces are made of hydroxyapatite or fluoroapatite in which at least some of the hydroxyl groups in the hydroxyapatite are substituted with fluorine atoms, wherein When a sample liquid was prepared by dissolving γ-globulin from bovine blood as a substance to be adsorbed in 10 mM sodium phosphate buffer (pH 6.5) so that the concentration was 1.0 mg / mL, and the prepared sample liquid was supplied to the column (φ6.0×35 mm) at flow rates of 200 cm / h and 250 cm / h, and when for each flow rate, the absorbance value X (280 nm) of the sample liquid to be supplied to the column and the absorbance of the eluate eluted from the column were measured. When the absorbance value Y (wavelength: 280 nm) is measured and the adsorption amount B (mg / mL) and C (mg / mL) of the substance to be adsorbed on the powder are calculated based on the amount of the sample liquid transported until the absorbance value Y (wavelength: 280 nm) becomes 10% of the absorbance value X (wavelength: 280 nm), the powder satisfies at least one of B ≥ 30 mg / mL or more, 0.89 ≤ C / B ≤ 1.00, and 0.89 ≤ C / B ≤ 0.

96.

16. The adsorbent according to any one of claims 13 to 15, wherein When a durability test of the powder is performed, in which the column (φ4.0×100 mm) is dry-packed with the powder as the adsorbent, and each buffer is sent through the column in the order of the step numbers shown in Table 1, and steps 1 to 5 shown in Table 1 are counted as one cycle, and the cycle is repeated until the pressure inside the column exceeds 200 psi, and the number of repeated cycles is 60 times or more, [Table 1] 。 17. The adsorbent according to any one of claims 13 to 15, wherein The substance to be adsorbed is an antibody.