Flexible self-supporting water-permeable and air-permeable grid electrode and preparation method thereof
By designing a flexible self-supporting water-permeable and breathable grid electrode with a hollow structure and curved grid lines, combined with a nickel layer, a gold layer and a PEDOT polymer layer, the problem of skin being stuffy and airtight after being worn for a long time is solved. It has high conductivity and self-supporting ability, improving wearing comfort and aesthetics.
Patent Information
- Application Number
- CN202410762187.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-11
AI Technical Summary
Existing flexible electrodes cause skin to feel stuffy after being worn for a long time, and are not breathable and may cause skin allergies, affecting aesthetics and comfort.
A flexible self-supporting water-permeable and breathable mesh electrode is designed, which adopts a hollow structure and curved grid lines, combined with a nickel layer, a gold layer and a PEDOT polymer layer, to provide high transparency, air and water permeability and self-supporting ability, through micropores Realize gas exchange between the skin and the outside world, improving wearing comfort.
It improves the wearer's comfort and aesthetics, maintains high conductivity and is stable during deformation, has self-supporting capabilities, avoids detachment of the substrate layer, and enhances the convenience of wearing.
Smart Images

Figure CN118749903A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of flexible electronics, and in particular relates to a flexible self-supporting water-permeable and air-permeable grid electrode and a preparation method thereof. Background Art
[0002] Bioelectric signals are physiological signals that can accurately reflect the condition of the human body. In clinical practice, the patient's physical condition can be determined by collecting and analyzing human physiological signals. Flexible wearable sensors can be in close contact with the human body when worn, and can collect, monitor and analyze human behavior and physiological information data in real time, providing the wearer with interactive functional experience of monitoring, monitoring and active protection from aspects such as body sensation, vision and touch. Today, flexible wearable sensors are widely used in the field of medical rehabilitation. There are higher requirements for related equipment that can be worn for a long time and monitor physiological signals in real time to keep track of the patient's physical condition at any time. Therefore, comfort for long-term wear is an important consideration.
[0003] At present, in order to improve the wearing comfort, a small, thin, flexible electrode that can be attached to the skin surface conformally has been reported. Due to its characteristics of being patternable and well attached, it is called an electronic tattoo, which can have good conductivity while in close contact. At present, the methods for realizing electronic tattoos include directly coating the skin surface with conductive ink or liquid metal (Lee et al., Adv. Mater., 2022, 34, 2204159), or making it on a flexible film and transferring it to the skin by transfer (Gogurla et al., Adv. Mater., 2021, 33, 2008308). However, although the electronic tattoos reported so far reduce the burden of wearing electrodes, the patterned tattoos affect the aesthetics when attached to the face, and still do not solve the problem of stuffy skin after long-term wear. At the same time, airtight tattoos may also cause skin allergies and other phenomena.
[0004] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention
[0005] The object of the present invention is to provide a flexible self-supporting water-permeable and breathable mesh electrode and a preparation method thereof, wherein the mesh electrode has high transparency, air-permeability and water-permeability, high conductivity and self-supporting ability, and can improve the comfort of the wearer.
[0006] In order to achieve the above object, a technical solution provided by a specific embodiment of the present invention is as follows:
[0007] A flexible self-supporting water-permeable and air-permeable grid electrode comprises a self-supporting base layer, an extension layer is coated on the self-supporting base layer, and a flexible polymer layer is coated on the extension layer; the self-supporting base layer has micropores and is hollow.
[0008] In one or more embodiments of the present invention, each grid in the grid electrode is composed of four curved grid lines.
[0009] In one or more embodiments of the present invention, each grid line is composed of two opposite semicircular arcs.
[0010] In one or more embodiments of the present invention, the intersection nodes of the grid lines in the grid electrode are staggered intersections.
[0011] In one or more embodiments of the present invention, the misalignment distance when the misalignment crosses is half the width of the line width.
[0012] In one or more embodiments of the present invention, the width of the grid lines in the grid electrode is 10-100 μm.
[0013] In one or more embodiments of the present invention, the micropore size of the grid electrode is 0.1-4 mm.
[0014] In one or more embodiments of the present invention, the self-supporting substrate layer is a nickel layer, and / or the extension layer is a gold layer, and / or the flexible polymer layer is a PEDOT polymer layer;
[0015] The thickness of the nickel layer is 20-30 μm, and / or the thickness of the gold layer is 400-600 nm, and / or the thickness of the flexible polymer layer is 200-1000 nm.
[0016] Another specific embodiment of the present invention provides a technical solution as follows:
[0017] A method for preparing a flexible self-supporting water-permeable and air-permeable grid electrode, comprising:
[0018] depositing an extension layer on the self-supporting substrate layer;
[0019] A flexible polymer layer is deposited on the ductile layer.
[0020] In one or more embodiments of the present invention, the preparation of the self-supporting substrate layer comprises:
[0021] Cleaning the substrate;
[0022] coating a sacrificial layer of adhesion promoter and photoresist on the substrate and drying;
[0023] Performing photolithography and development on the photoresist to achieve grid patterning on the photoresist;
[0024] removing the sacrificial layer of the adhesion promoter remaining at the bottom of the pattern by using oxygen plasma to expose the substrate;
[0025] depositing nickel metal in the photoresist pattern;
[0026] The substrate is immersed in a stripping agent to remove the photoresist and obtain a self-supporting substrate layer.
[0027] Compared with the prior art, the flexible self-supporting water-permeable and breathable mesh electrode of the present invention is air-permeable and water-permeable, which can improve the comfort of the wearer; it has high transparency, which improves the aesthetics of facial attachment; it has high conductivity, and its resistance value is stable during deformation without obvious changes, and it can work stably when worn; it has self-supporting ability and no substrate layer, which avoids the detachment of the substrate layer due to bending during use, and can be used at any time, avoiding the inconvenience caused by real-time coating or transfer. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 This is a SEM image of a flexible self-supporting water-permeable and air-permeable mesh electrode in one embodiment of the present invention.
[0030] Figure 2 FIG. 4 is a schematic diagram of a cross-shaped grid line in an embodiment of the present invention.
[0031] Figure 3 It is a schematic diagram of the staggered and crossed grid lines in one embodiment of the present invention.
[0032] Figure 4 This is a flow chart of preparing a flexible self-supporting water-permeable and air-permeable mesh electrode in one embodiment of the present invention;
[0033] Figure 5 This is a structural diagram of the preparation process of a flexible self-supporting water-permeable and air-permeable grid electrode in one embodiment of the present invention;
[0034] Figure 6 Schematic diagram of dripping deionized water onto a flexible self-supporting water-permeable and air-permeable mesh electrode in one embodiment of the present invention.
[0035] Figure 7 Schematic diagram of deionized water passing through a flexible self-supporting water-permeable and air-permeable mesh electrode in one embodiment of the present invention.
[0036] Description of main reference numerals:
[0037] 1-ITO substrate, 2-adhesion promoter sacrificial layer, 3-photoresist, 4-nickel layer, 5-gold layer, 6-PEDOT polymer layer. DETAILED DESCRIPTION
[0038] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments.
[0039] Unless explicitly stated otherwise, throughout the specification and claims, the term “comprise” or variations such as “include” or “comprising”, etc., will be understood to include the stated elements or components but not to exclude other elements or components.
[0040] A specific embodiment of the present invention provides a flexible self-supporting water-permeable and air-permeable grid electrode, wherein the self-supporting base layer is coated with an extension layer, and the extension layer is coated with a flexible polymer layer; the self-supporting base layer has micropores and is hollow.
[0041] In one embodiment, each grid in the grid electrode is composed of four curved grid lines.
[0042] In one embodiment, each grid line consists of two opposite semicircular arcs.
[0043] In one embodiment, the intersection nodes of the grid lines in the grid electrode are staggered intersections.
[0044] In one embodiment, the offset distance is half the line width.
[0045] In one embodiment, the width of the grid lines in the grid electrode is 10-100 μm.
[0046] In one embodiment, the pore size of the grid electrode is 0.1-4 mm.
[0047] Specific, combined Figure 1 , Figure 2 and Figure 3 The mesh electrode adopts a hollow design. After it is attached to the surface of human skin, the micropores in the mesh electrode provide a channel for the skin to exchange gas with the outside world, which is conducive to perspiration, thereby improving the comfort of long-term wearing of the mesh electrode. The mesh electrode adopts a curved grid line design. Compared with a straight grid, the mesh electrode composed of curved grid lines has a higher tolerance for deformation and can achieve a larger range of stretching, which is more conducive to deformation when worn; at the same time, compared with a cross, the intersection of the grid lines is staggered. Under the same stretching range, the two ends of the mesh electrode have less force and are easier to deform; the appropriate line width of the grid line also ensures that the mesh electrode can have good deformation ability and strength at the same time.
[0048] In one embodiment, the self-supporting substrate layer is a nickel layer, the extension layer is a gold layer, and the flexible polymer layer is a PEDOT polymer layer; the nickel layer has a thickness of 20-30 μm, the gold layer has a thickness of 400-600 nm, and the flexible polymer layer has a thickness of 200-1000 nm.
[0049] Specifically, nickel metal has high optical transmittance, excellent conductivity, excellent structural stability and mechanical bendability. Using nickel metal as the base layer of the grid electrode can ensure that the grid electrode can withstand certain deformations such as bending, folding and stretching, while also ensuring the conductivity of the grid electrode. Gold has good conductivity and flexibility, and has tensile resistance. In addition, gold is an inert metal and has high stability. The use of gold-coated nickel layer can improve the chemical stability of the grid electrode and ensure the stability of the grid electrode during use. PEDOT polymer has high conductivity, flexibility and good strength, good electrochemical stability, and certain corrosion resistance. Coating PEDOT polymer on the surface of the gold layer can simultaneously ensure the conductivity, flexibility and stability of the grid electrode. The grid electrode is composed of a nickel layer, a gold layer and a flexible polymer layer, so that the grid electrode has high conductivity and self-supporting ability.
[0050] In addition, by controlling the thickness of the nickel layer, the gold layer and the flexible polymer layer, not only can the grid electrode have better conductivity, but the grid electrode can also be miniaturized and lightweight, making it easier to adhere to the surface of human skin.
[0051] Another specific embodiment of the present invention provides a method for preparing a flexible self-supporting water-permeable and air-permeable grid electrode, comprising:
[0052] Step 1, depositing an extension layer on a self-supporting substrate layer;
[0053] Step 2: depositing a flexible polymer layer on the stretch layer.
[0054] Specifically, in step 1, the platinum electrode and the self-supporting substrate layer, i.e., the pure nickel grid, are electroplated in a gold electroplating solution; the electroplating solution is an aqueous solution of potassium gold cyanide with a concentration of 0.03-0.05 mol / L; the electroplating time is 10 min; and the current density is 1.02 A / dm 2 The thickness of the gold layer is 400-600nm. By controlling the concentration of the electroplating solution, the electroplating temperature and the current time, the deposition rate is moderate, and a stable gold layer can be formed on the surface of the pure nickel grid, so that the gold layer can stably cover the pure nickel grid.
[0055] In step 2, a platinum electrode is used as a counter electrode and a silver / silver chloride electrode is used as a reference electrode to deposit a flexible polymer layer by electrochemical polymerization; the electrolyte is an aqueous solution of 3,4-ethylenedioxythiophene with lithium perchlorate added, the concentration of the aqueous solution of 3,4-ethylenedioxythiophene is 0.01-0.03 mol / L, and the amount of lithium perchlorate added is 0.1 mol / L; the polymerization time is 1-3 min; and the polymerization voltage is 2-3 V. By controlling the electrochemical polymerization conditions, 3,4-ethylenedioxythiophene is polymerized on the surface of the gold layer to form a flexible polymer layer, thereby achieving the purpose of firmly coating the gold layer.
[0056] In one embodiment, the preparation of the self-supporting substrate layer comprises:
[0057] (1) cleaning the substrate;
[0058] (2) coating a sacrificial layer of an adhesion promoter and a photoresist on the substrate and drying;
[0059] (3) performing photolithography and development on the photoresist to achieve grid patterning on the photoresist;
[0060] (4) using oxygen plasma to remove the sacrificial layer of the adhesion promoter remaining at the bottom of the pattern to expose the substrate;
[0061] (5) depositing nickel metal in the photoresist pattern;
[0062] (6) The substrate is immersed in a debonding agent to remove the photoresist and obtain a self-supporting substrate layer.
[0063] Specific, combined Figure 4 In step (1), the ITO substrate is ultrasonically cleaned with acetone, ethanol and deionized water in sequence, and the ultra-clear cleaning time is 30 minutes, and then treated with 30W power for 15 minutes under oxygen plasma. By cleaning, dust on the ITO surface can be removed, the water cleanliness of the ITO substrate surface can be improved, and it is beneficial to apply glue on the ITO substrate surface.
[0064] In step (2), a tackifier is spin-coated on the surface of the ITO substrate with a coating thickness of 17-30 nm, and baked at 200° C. for 1 min to form a sacrificial tackifier layer; a negative photoresist is spin-coated on the sacrificial tackifier layer with a coating thickness of 20-30 μm, and baked at 95° C. for 15 min.
[0065] In step (3), the photoresist is exposed using a grid mask, the exposure time is 7.7s, the post-baking is carried out at 95°C for 3min, the mixed light intensity is 350W, and after the post-baking, the ITO substrate is placed in an alkaline propylene glycol methyl ether acetate solution for development, so that the grid pattern emerges on the photoresist surface. By selecting the appropriate exposure time and intensity, a specific target structure pattern can be formed, and then the photoresist in the exposed area is removed by the developer, so that the target pattern structure appears on the photoresist surface.
[0066] Specifically, in step (4), oxygen plasma is used to strike the patterned part of the tackifier layer exposed at the bottom of the photoresist to remove it, exposing the ITO substrate. The tackifier is selected as a sacrificial layer to help promote the detachment of the photoresist from the ITO substrate.
[0067] Specifically, in step (5), the nickel plate and the ITO substrate are heated and electroplated in a nickel electroplating solution so that the nickel layer grows inside the pattern; the electroplating solution is a nickel sulfate aqueous solution with a concentration of 1.5-2.3 mol / L; the electroplating temperature is 50-55°C; the electroplating time is 30 min; and the current density is 2.05 A / dm 2 The thickness of the nickel layer is 20-30 μm. By controlling the concentration of the electroplating solution, the electroplating temperature and the current time, the deposition rate is moderate, and a structurally stable nickel layer can be formed in the grooves of the photoresist pattern; at the same time, the thickness of the nickel layer is controlled so that the nickel layer has independent self-supporting ability.
[0068] Specifically, in step (6), the ITO substrate with the nickel-plated layer is immersed in a debonding agent at 50° C. for 30 minutes to remove the photoresist and obtain an independent nickel layer. The debonding agent is used to dissolve the sacrificial layer of the adhesion promoter so that the photoresist can be separated from the ITO substrate, thereby obtaining an independent nickel layer grid structure.
[0069] The present invention is further described below in conjunction with specific embodiments.
[0070] Example 1
[0071] A flexible self-supporting water-permeable and air-permeable grid electrode comprises a self-supporting substrate layer, which is a nickel layer with a thickness of 20 μm; the surface of the nickel layer is coated with an extension layer with a thickness of 500 nm, which is a gold layer; the surface of the gold layer is coated with a flexible polymer layer with a thickness of 300 nm, which is a PEDOT polymer layer.
[0072] like Figure 1 As shown, the grid electrode has micropores as a whole, which are hollowed out, and the size of the micropores is 2mm*2mm. Each grid in the grid electrode is composed of four curved grid lines, each grid line is composed of two opposite semicircular arcs, the grid line width in the grid electrode is 15μm, and the intersection nodes of the grid lines in the grid electrode are staggered intersections, and the staggered distance is about half the distance of the line width, that is, the intersection is at 7-8μm of the line width.
[0073] The method for preparing a flexible self-supporting water-permeable and air-permeable grid electrode specifically comprises the following steps:
[0074] (1) Cleaning ITO substrate
[0075] Specific combination Figure 5In (a), the ITO substrate was ultrasonically cleaned with acetone, ethanol and deionized water in sequence, with the ultra-clear cleaning time being 30 min each, and then treated in oxygen plasma at 30 W power for 15 min.
[0076] (2) Coating a sacrificial layer of adhesion promoter and photoresist on the substrate and drying
[0077] Specific combination Figure 5 In (b), Omnicoat adhesion promoter is spin-coated on the surface of the ITO substrate with a coating thickness of 20 nm, and baked at 200°C for 1 min to form a adhesion promoter sacrificial layer; negative photoresist is spin-coated on the adhesion promoter sacrificial layer, the negative photoresist model is SU-83050, the coating thickness is 30 μm, and baked at 95°C for 15 min.
[0078] (3) Photolithography and development of the photoresist to achieve grid patterning on the photoresist
[0079] Specific combination Figure 5 In (c), the photoresist is exposed using a grid mask with an exposure time of 7.7 s, and post-baked at 95°C for 3 min with a mixed light intensity of 350 W. After post-baking, the ITO substrate is developed in an alkaline propylene glycol methyl ether acetate solution to make the grid pattern appear on the photoresist surface.
[0080] (4) Use oxygen plasma to remove the residual sacrificial layer of adhesion promoter at the bottom of the pattern to expose the substrate
[0081] Specific combination Figure 5 In (d), oxygen plasma is used to strike with a power of 30 W to remove the patterned part of the adhesion promoter layer exposed at the bottom of the photoresist, exposing the ITO substrate.
[0082] (5) Depositing nickel metal in the photoresist pattern
[0083] Specific combination Figure 5 In (e), the nickel plate and the ITO substrate are heated and electroplated in a nickel electroplating solution to grow a nickel layer inside the pattern; the electroplating solution is a nickel sulfate aqueous solution purchased from Dongguan Beichen Hardware, model BC112; the electroplating temperature is 55°C; the electroplating time is 30 min; the current density is 2.05 A / dm 2 ; The thickness of the nickel layer is 20μm.
[0084] (6) Soak the substrate in a degumming agent to remove the photoresist and obtain a nickel layer
[0085] Specific combination Figure 5 In (f), the ITO substrate with the nickel-plated layer is immersed in an N-methylpyrrolidone solution at 50° C. for 30 min to remove the photoresist and obtain a self-supporting substrate layer, namely, an independent nickel grid.
[0086] (7) Depositing gold on the nickel layer to form a gold layer
[0087] Specific combination Figure 5 In (g), the platinum electrode and the nickel layer are electroplated in a gold electroplating solution to form an extended layer and obtain a gold / nickel grid. The electroplating solution is a potassium cyanide gold aqueous solution purchased from Dongguan Beichen Hardware, model BC122; the electroplating time is 10 min; the current density is 1.02 A / dm 2 ; The thickness of the gold layer is 500nm.
[0088] (8) Depositing a flexible polymer layer on the gold layer to obtain a grid electrode
[0089] Specific combination Figure 5 In (h), a platinum electrode was used as the counter electrode and a silver / silver chloride electrode was used as the reference electrode, and a flexible polymer layer with a thickness of 300 nm was deposited by electrochemical polymerization; the electrolyte was an aqueous solution of 3,4-ethylenedioxythiophene with lithium perchlorate added, the concentration of the aqueous solution of 3,4-ethylenedioxythiophene was 0.01 mol / L, and the amount of lithium perchlorate added was 0.1 mol / L; the polymerization time was 2 min; and the polymerization voltage was 2 V.
[0090] Example 2
[0091] Conduct relevant tests on flexible self-supporting water-permeable and air-permeable mesh electrodes
[0092] (1) Observe the grid electrode under a scanning electron microscope. Figure 1 As shown, the grid electrode has a regular structure, is hollow and breathable.
[0093] (2) Hold the two ends of the grid electrode with tweezers, and then drip deionized water from 2 cm above the grid electrode. The water droplets can freely pass through the surface of the grid electrode. Figure 6 and Figure 7 As shown, it is shown that the grid electrode in the present invention is water permeable, and is less likely to cause stuffiness after being attached to the skin, and can achieve water permeability and free sweating.
[0094] (3) The grid electrode of the present invention was tested for sheet resistance using a four-probe resistance tester, and the sheet resistance was measured to be 0.268 Ω·sq -1 ; The transparency of the grid electrode tested by UV-visible-infrared spectrophotometer was 95%, indicating that the grid electrode in the present invention has low resistance, excellent conductivity, and good transmittance.
[0095] (4) The independent nickel grid, gold / nickel grid and the grid electrode finally obtained in the preparation process were subjected to mechanical tensile tests. The test results are shown in Table 1.
[0096] Table 1 Mechanical tensile test results
[0097]
[0098] It can be seen from Table 1 that the grid electrode has certain flexibility and tensile resistance, which is conducive to bending and stretching when worn.
[0099] (5) The grid electrode was repeatedly stretched for 100 cycles. During the test, the resistance at both ends of the grid electrode was detected in real time. At different stretching ratios, the resistance values at both ends of the grid electrode are shown in Table 2.
[0100] Table 2 Resistance of the grid electrodes after repeated stretching for 100 cycles
[0101]
[0102] The grid electrode was subjected to a 100-cycle bending test, during which the resistance at both ends was tested in real time. The resistance values at both ends of the grid electrode at different bending ratios are shown in Table 3.
[0103] Table 3 Resistance of the two ends of the grid electrode after repeated bending for 100 cycles
[0104] Bending ratio initial 15° 30° 45° 60° 75° 90° Resistance(Ω) 3.41 3.41 3.40 3.39 3.50 3.51 3.64
[0105] It can be seen from Tables 2 and 3 that the resistance of the grid electrode in the present invention can remain stable during the deformation process with little change, and can still maintain a low resistance after repeated stretching or bending, indicating that the grid electrode in the present invention has high conductivity, stable conductivity after deformation, and has high applicability in flexible wearable sensors.
[0106] In summary, the preparation method of the present invention uses a certain thickness of negative photoresist for patterning, uses electroplating to form an independent nickel grid of a certain thickness, and releases the independent nickel grid through a debonding agent, so that an independent nickel grid structure with independent self-supporting ability can be obtained without using a transfer flexible substrate. Then, the independent nickel grid is used as the basic skeleton, and gold and PEDOT polymers with excellent ductility and conductivity are coated on its surface, so that the grid electrode finally obtained has mechanical, flexible and conductive properties at the same time. At the same time, the hollow structure makes the grid electrode completely breathable after being attached to the skin surface, can sweat freely, and has a high degree of comfort wearability.
[0107] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0108] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A flexible self-supporting water-permeable and air-permeable mesh electrode, characterized in that: It comprises a self-supporting base layer, the self-supporting base layer is coated with an extension layer, and the extension layer is coated with a flexible polymer layer; The self-supporting base layer has micropores and is hollow.
2. A flexible self-supporting water-permeable and air-permeable mesh electrode according to claim 1, characterized in that: Each grid in the grid electrode is composed of four curved grid lines.
3. A flexible self-supporting water-permeable and air-permeable mesh electrode according to claim 2, characterized in that: Each grid line consists of two opposing semicircular arcs.
4. A flexible self-supporting water-permeable and air-permeable mesh electrode according to claim 1, characterized in that: The intersection nodes of the grid lines in the grid electrode are staggered intersections.
5. A flexible self-supporting water-permeable and air-permeable mesh electrode according to claim 4, characterized in that: When the offset crosses, the offset distance is half the line width.
6. A flexible self-supporting water-permeable and air-permeable mesh electrode according to claim 1, characterized in that: The grid line width in the grid electrode is 10-100 μm.
7. A flexible self-supporting water-permeable and air-permeable mesh electrode according to claim 1, characterized in that: The micropore size of the grid electrode is 0.1-4 mm.
8. The flexible self-supporting water-permeable and air-permeable mesh electrode according to claim 1, characterized in that: The self-supporting substrate layer is a nickel layer; and / or, the extension layer is a gold layer; and / or, the flexible polymer layer is a PEDOT polymer layer; The thickness of the nickel layer is 20-30 μm; and / or the thickness of the gold layer is 400-600 nm; and / or the thickness of the flexible polymer layer is 200-1000 nm.
9. A method for preparing a flexible self-supporting water-permeable and air-permeable mesh electrode according to any one of claims 1 to 8, characterized in that: include: depositing an extension layer on the self-supporting substrate layer; A flexible polymer layer is deposited on the ductile layer.
10. A flexible self-supporting water-permeable and air-permeable mesh electrode according to claim 9, characterized in that: The preparation of the self-supporting substrate layer comprises: Cleaning the substrate; coating a sacrificial layer of adhesion promoter and photoresist on the substrate and drying; Performing photolithography and development on the photoresist to achieve grid patterning on the photoresist; removing the sacrificial layer of the adhesion promoter remaining at the bottom of the pattern by using oxygen plasma to expose the substrate; depositing nickel metal in the photoresist pattern; The substrate is immersed in a stripping agent to remove the photoresist and obtain a self-supporting substrate layer.