Oxygen sulfide photocatalyst as well as preparation method and application thereof

By preparing a new oxysulfide photocatalyst Sr3In4O4S5, the problem of insufficient structure of existing oxysulfide photocatalysts is solved, an efficient photocatalytic water splitting reaction is achieved, the rates of hydrogen and oxygen production are significantly increased, and the rate of hydrogen and oxygen production is improved, with stable oxygen production. capabilities and practical value.

CN118751256AActive Publication Date: 2024-10-11UNIV OF CHINESE ACAD OF SCI
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411116389.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-10-11
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The number of existing oxysulfide photocatalysts is limited, and there is a lack of materials with completely new structures to achieve efficient photocatalytic water splitting reactions.

Method used

A new type of oxysulfide photocatalyst Sr3In4O4S5 was prepared, which has an orthorhombic crystal structure and a one-dimensional chain structure. Its photocatalytic performance was optimized through high-temperature reaction method and acid treatment surface modification method.

Benefits of technology

It achieves a suitable band gap position, stabilizes the oxidation behavior of sulfide ions, significantly improves the rate of photocatalytic hydrogen and oxygen production, and has relatively stable oxygen production capacity and practical value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118751256A_ABST
    Figure CN118751256A_ABST
Patent Text Reader

Abstract

The invention provides a novel oxysulfide photocatalyst and a preparation method and application thereof, the chemical formula of the novel oxysulfide photocatalyst is Sr3In4O4S5, the novel oxysulfide photocatalyst belongs to an orthorhombic system Pmmn space group and has a one-dimensional chain structure, the coordination form of In is [InO2S3] distorted tetragonal pyramids, the tetragonal pyramids are mutually connected and extend along a c axis, and Sr ions are located among one-dimensional chains. The oxysulfide has a proper band edge position, and can simultaneously meet the condition of producing oxygen and hydrogen by photocatalytic decomposition of water, and the oxidation effect of photo-generated holes on sulfur ions can be effectively relieved by oxygen and sulfur anion orbital hybridization at the valence band top. The oxysulfide disclosed by the invention shows good photocatalytic performance, and has important significance in practical application of photocatalytic water decomposition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of photocatalysts, and in particular to a preparation method of an oxysulfide photocatalyst and application thereof. Background Art

[0002] Solar energy is an inexhaustible, clean and pollution-free green energy source that is expected to alleviate the increasingly severe energy crisis. Therefore, it has become one of the future energy sources that countries around the world are competing to develop. Photocatalytic materials are an important medium for achieving efficient utilization of solar energy. The photocatalytic process can be described as a semiconductor with a certain band gap. Under light, the electrons at the top of its valence band have a certain probability of being stimulated to transition to the conduction band, forming photogenerated electron-hole pairs. After the electron-hole pairs separate and migrate to the semiconductor surface under a specific driving force, they can undergo redox reactions with species in the environment, thereby realizing the conversion of solar energy to chemical energy. The photocatalytic process of semiconductors can be applied to the photocatalytic synthesis of various chemical substances (such as hydrogen, oxygen, high-value-added organic matter, etc.), and can also catalytically degrade pollutants in the environment. Among them, the photocatalytic complete water splitting reaction can produce another clean, pollution-free and easier to store chemical energy-hydrogen. Therefore, the exploration of photocatalysts for complete water splitting has important scientific significance and practical value.

[0003] In recent years, oxysulfide photocatalysts have attracted extensive attention from researchers. Oxysulfide refers to the presence of oxygen ions and sulfur anions (such as S 2- 、Se 2- Oxysulfide photocatalysts represented by Y2Ti2S2O5 show unique advantages different from single anion photocatalysts. Compared with oxides, oxysulfides have a higher valence band top, so they can have the ability to photocatalytically split water while ensuring a narrow band gap. Compared with sulfide compounds, the hybrid valence band components of oxysulfides enable them to alleviate the self-oxidation behavior of photogenerated holes on sulfide anions. The above characteristics make oxysulfides a very promising photocatalyst material system for the splitting of water. However, the number of known oxysulfide photocatalysts is very small, and oxysulfide photocatalysts with new structures are in urgent need of development. Summary of the invention

[0004] The invention provides a novel oxysulfide photocatalyst and a preparation method and application thereof.

[0005] In a first aspect, the present invention provides an oxysulfide having a chemical formula of Sr3In4O4S5 and belonging to an orthorhombic system. Pmm Space group, in which the coordination form of In is [InO2S3] distorted tetrahedral pyramid, the tetrahedral pyramids are interconnected and extend along the c-axis to form a one-dimensional chain structure, Sr ions are located between the one-dimensional chains, the valence state of Sr is +2, the valence state of In is +3, the valence state of O is -2, and the valence state of Se is -2.

[0006] Among the oxysulfides, Sr in Sr3In4O4S5 may be partially replaced by, but not limited to, Ca, Ba or Pb, and S in Sr3In4O4S5 may be partially replaced by, but not limited to, Se or Te.

[0007] In a second aspect, the present invention provides a method for preparing the above-mentioned novel oxysulfide, comprising placing a raw material containing Sr element, In element, O element, S element and doping element under vacuum or inert atmosphere conditions, keeping it at 650-800° C. for 24-72 hours and then cooling it.

[0008] The molar ratio of the Sr element, the In element, the O element and the S element in the raw material is (2.8-3.5):4:4:(4.8-5.5).

[0009] The high temperature reaction may include heating from room temperature to 650-800° C. within 10 hours.

[0010] The high temperature reaction may include heating to 700-800° C. and then keeping the temperature for 24-72 hours, then cooling to 500° C. within 24-72 hours, and then naturally cooling to room temperature.

[0011] In the above preparation process, a flux may be added to the reaction raw materials, and the types of flux include but are not limited to alkali metal halides such as KCl, KI, RbCl, CsI, etc., to promote crystal growth.

[0012] In a third aspect, the present invention provides a method for surface modification of the above-mentioned oxysulfide, that is, Sr3In4O4S5 is dispersed in a dilute acid solution, stirred at room temperature, filtered, washed with deionized water, and then dried.

[0013] The hydrogen ion concentration of the dilute acid solution may be 0.01 to 0.1 mol / L, and the acid may be hydrochloric acid, sulfuric acid, nitric acid, or the like.

[0014] The room temperature stirring process can last for 10 to 24 hours.

[0015] In a fourth aspect, the present invention provides a use of the above-mentioned oxysulfide for photocatalytic decomposition of water to produce hydrogen and oxygen. Before surface modification, the maximum hydrogen production rate is 257.9 μmol×g -1 ×h -1 The maximum oxygen production rate was 75.5 μmol×g -1 ×h -1 After the surface modification method of the third aspect is used, the maximum hydrogen production rate can reach 760.2 μmol×g -1 ×h -1 The maximum oxygen production rate can reach 258.4 μmol×g -1 ×h-1 .

[0016] When the above-mentioned oxysulfide photocatalyst is used for photocatalytic hydrogen production, Na2S and Na2SO3 are used as sacrificial agents.

[0017] When the above-mentioned oxysulfide photocatalyst is used for photocatalytic oxygen production, NaIO3 is used as a sacrificial agent.

[0018] In summary, the present invention provides an oxysulfide photocatalyst with a completely new crystal structure, which has the following beneficial effects:

[0019] 1. The novel oxysulfide photocatalyst obtained by the present invention has a suitable band edge position, can simultaneously meet the conditions for photocatalytic decomposition of water to produce oxygen and hydrogen, and has certain practical value and application prospects.

[0020] 2. In the oxysulfide obtained by the present invention, the orbital hybridization of the oxysulfur anion at the top of the valence band effectively stabilizes the sulfur ions, alleviates the oxidation effect of the photogenerated holes on them, and achieves a relatively stable oxygen production capacity.

[0021] 3. The present invention provides a simple and effective strategy for surface modification of oxysulfides, which significantly improves the rate of photocatalytic hydrogen and oxygen production. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a schematic diagram of the crystal structure of Sr3In4O4S5 of the present invention; Figure 2 This is the X-ray diffraction pattern of Sr3In4O4S5 powder of Example 1 of the present invention; Figure 3 The scanning electron microscope (SEM) photo and energy spectrum (EDS) analysis diagram of Example 1 of the present invention are shown; Figure 4 The UV-visible absorption spectra of Examples 1 and 4 of the present invention are shown; Figure 5 A graph showing the photocatalytic hydrogen production of Examples 1 and 4 of the present invention; Figure 6 The photocatalytic oxygen production of Examples 1 and 4 of the present invention is shown. DETAILED DESCRIPTION

[0023] The present invention is further described below by the following embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, but not to limit the present invention.

[0024] Embodiment 1 The oxysulfide Sr3In4O4S5 of this embodiment belongs to the orthorhombic system. PmmSpace group, where the coordination form of In is [InO2S3] distorted tetrahedral pyramids, which are interconnected and extend along the c-axis to form a one-dimensional chain structure, with Sr ions located between the one-dimensional chains (see Figure 1 ). The valence state of Sr is +2, the valence state of In is +3, the valence state of O is -2, and the valence state of Se is -2. Sr can be replaced by elements such as Ca, Ba or Pb, and S can also be replaced by elements such as Se or Te. The unit cell parameters of Sr3In4O4S5 are a = 9.1558(8)Å, b = 17.8619(18) Å, c = 3.9038(3) Å, a = b = g = 90°, Z = 2, and its crystallographic data are shown in Table 1.

[0025] Table 1 Crystallographic data of Sr3In4O4S5 Molecular formula <![CDATA[Sr3In4O4S5]]> Molecular weight 946.44 Space group a (Å) 9.1558(8) b (Å) 17.8619(18) c (Å) 3.9038(3) <![CDATA[Volume (Å 3 )]]> 638.43(10) <![CDATA[Density (g×cm -3 )]]> 4.923

[0026] The following is an illustrative example of the preparation method of the novel oxysulfide Sr3In4O4S5 of the present invention.

[0027] The raw materials including strontium source, indium source, oxygen source, sulfur source and other doping elements can be placed under vacuum conditions and prepared by high temperature reaction. The raw materials can be fully ground and mixed in a mortar, and the molar ratio of Sr element, In element, O element and S element in the raw materials is (2.8~3.5):4:4:(4.8~5.5). The source of Sr can be single substance Sr, SrO or SrS, and the source of In can be single substance In, In2O3 or In2S3. A flux can be added to the raw materials to create a liquid phase reaction environment, and the types of flux include but are not limited to alkali metal halides KCl, KI or CsI.

[0028] The reaction vessel containing the reaction raw materials is placed in a muffle furnace, heated to 650-800°C, kept warm for 24-72 hours, and then cooled. In this high temperature reaction method, it is preferably heated to 650-800°C at a rate of 65-80°C / hour, so that high quality and purity crystal preparation can be achieved. In some embodiments, the reaction container may be a quartz tube, which is evacuated to 0.1 Pa and then melted and sealed, placed in a muffle furnace, and heated to 650-800°C at a rate of 65-80°C / hour. In addition, it is preferably heated to 650-800°C and kept warm for 24-72 hours, then cooled to 500°C at a cooling rate of 3-8°C / hour, and then naturally cooled to room temperature. For samples with flux added, the sample is fully washed with deionized water after the reaction is completed and then dried to obtain the final product.

[0029] Embodiment 2 This embodiment is a surface modification method for Sr3In4O4S5, that is, through acid treatment, Sr ions and O ions on the sample surface are selectively etched, and the light absorption properties and carrier transport properties of the material are regulated by surface reconstruction, thereby achieving a significant improvement in the photocatalytic hydrogen and oxygen production performance.

[0030] The surface modification method of the oxysulfide of the present invention is exemplified below.

[0031] A certain mass of oxysulfide is dispersed in a dilute acid solution with a hydrogen ion concentration of 0.01 to 0.1 mol / L. The acid type can be hydrochloric acid, sulfuric acid, nitric acid, etc., and placed on a magnetic stirring table. After stirring at room temperature for 10 to 24 hours, it is filtered and washed with deionized water until the pH of the washing liquid is close to neutral. It is then washed with ethanol and acetone in turn and dried.

[0032] The present invention provides a preparation method and use of a novel oxysulfide photocatalyst, whose chemical formula is Sr3In4O4S5, and belongs to a new type of crystal structure. This photocatalyst has a suitable band edge position, which can simultaneously meet the conditions for photocatalytic decomposition of water to produce oxygen and hydrogen. And because the orbital hybridization of the oxygen-sulfur anion at the top of the valence band of the material effectively stabilizes the sulfur ions, alleviates the oxidation effect of the photogenerated holes on it, and enables it to have a relatively stable oxygen production capacity. In addition, through simple room temperature acid treatment for surface modification, the light absorption properties and carrier transport properties of the material can be effectively regulated, and the photocatalytic hydrogen and oxygen production performance can be greatly improved, which has certain practical value and application prospects.

[0033] The following further examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values ​​​​exemplified below.

[0034] In the following examples, the reagents, materials and instruments used are conventional reagents, conventional materials and conventional instruments unless otherwise specified, and are all commercially available. The reagents involved can also be synthesized by conventional synthesis methods.

[0035] Example 1 Preparation of Sr3In4O4S5 by high temperature solid phase method Weigh 0.7000 g SrO, 0.1850 g In2O3 and 1.086 g In2S3, grind them thoroughly in a mortar and mix them evenly, transfer them to a quartz tube with an inner diameter of 1 cm and vacuum seal them. Evacuate to 0.1 Pa. The sealed quartz tube was placed in a muffle furnace and the insulation program was set as follows: heating to 700 °C in 10 hours, keeping at 700 °C for 48 hours, then cooling to 500 °C at a cooling rate of 3 °C per hour, and then naturally cooling to room temperature. The product was taken out of the quartz tube to obtain Sr3In4O4S5 polycrystalline powder.

[0036] Example 2 Preparation of Sr3In4O4S5 by flux method: 0.7000 g SrO, 0.1850 g In2O3, 1.086 g In2S3 and 7.5 g KI were weighed and thoroughly ground and mixed in a mortar. Then, they were transferred to a quartz tube with an inner diameter of 1 cm and vacuum sealed. The vacuum was evacuated to 0.1 Pa. The sealed quartz tube was placed in a muffle furnace, and the insulation program was set as follows: heating to 700 °C in 10 hours, keeping at 700 °C for 48 hours, then cooling to 500 °C at a cooling rate of 3 °C per hour, and then naturally cooling to room temperature. The product was taken out of the quartz tube, washed with deionized water to remove the flux, washed with ethanol and acetone in turn, and then dried to obtain Sr3In4O4S5 polycrystalline powder.

[0037] Example 3 Preparation of Se-doped Sr3In4O4S5: Weigh 0.7000 g SrO, 0.1850 g In2O3, 0.825 g In2S3, 0.372 g In2Se3 and 7.5 g KI, grind and mix them thoroughly in a mortar, transfer them to a quartz tube with an inner diameter of 1 cm, vacuum seal them, and evacuate them to 0.1 Pa. Put the sealed quartz tube into a muffle furnace, and set the insulation program as follows: heat to 700 °C in 10 hours, keep it at 700 °C for 48 hours, then cool it to 500 °C at a cooling rate of 3 °C per hour, and then cool it naturally to room temperature. Take the product out of the quartz tube, wash it with deionized water to remove the flux, wash it with ethanol and acetone in turn, and dry it to obtain Se-doped Sr3In4O4S5 polycrystalline powder.

[0038] Example 4 Surface modification of Sr3In4O4S5: Weigh 1 g of Sr3In4O4S5 sample and disperse it in 100 ml of 0.06 mol / L dilute hydrochloric acid solution. Place the mixed system on a magnetic stirring table and stir at room temperature for 24 hours. Then filter and wash with deionized water until the pH of the washing solution is close to neutral. Then wash with ethanol and acetone in turn and dry.

[0039] Example 5 Physical properties: 1) The obtained Sr3In4O4S5 crystals were ground and then subjected to powder X-ray diffraction test. The results are as follows Figure 2 The obtained powder X-ray diffraction pattern is consistent with the theoretical X-ray diffraction pattern of the crystal obtained by single crystal structure analysis, proving that the obtained crystal has a high purity; 2) Observe the obtained Sr3In4O4S5 crystals using a scanning electron microscope. Figure 3 As shown, the crystal was found to be rod-shaped, and the energy spectrum analysis showed that the four elements were evenly distributed in the crystal, and the element ratio was consistent with the results obtained from the single crystal structure analysis; 3) The obtained Sr3In4O4S5 crystals and the surface-modified samples were subjected to UV-visible diffuse reflectance spectroscopy test, and the test results were converted into UV-visible absorption spectra. The results are as follows: Figure 4 As shown in Figure 2, the optical band gap of Sr3In4O4S5 before modification is 3.2 eV, and after modification, the optical band gap becomes 2.47 eV.

[0040] Example 6 Performance Test: 1) Weigh 10 mg of Sr3In4O4S5 samples before and after modification, respectively, disperse them in 10 ml of aqueous solution containing 0.06 mol / L Na2S and Na2SO3, irradiate the solution with a 300 W xenon lamp, and analyze the amount of hydrogen obtained by gas chromatography. Figure 5 It can be seen that the hydrogen production rate of the modified oxysulfide is significantly higher than that before modification, and the maximum hydrogen production rate can reach 760.2 μmol×g -1 ×h -1 , which is three times the hydrogen production rate before modification (257.9 μmol×g -1 ×h -1 ); 2) Weigh 10 mg of Sr3In4O4S5 samples before and after modification, respectively, disperse them in 10 ml of aqueous solution containing 0.01 mol / L NaIO3, irradiate the solution with a 300 W xenon lamp, and analyze the amount of oxygen obtained by gas chromatography. Figure 6 It can be seen that the oxygen production rate of the modified oxysulfide is significantly higher than that before modification, and the maximum oxygen production rate can reach 258.4 μmol×g-1 ×h -1 , which is three times the oxygen production rate before modification (75.5 μmol×g -1 ×h -1 ).

Claims

1. An oxysulfide, characterized in that: (1) The chemical formula is Sr3In4O4S5, which belongs to the orthorhombic crystal system. Pmm Space group; (2) The coordination form of In is [InO2S3] distorted tetrahedral pyramids, which are interconnected and extend along the c-axis to form a one-dimensional chain structure, with Sr ions located between the one-dimensional chains; (3) The valence state of Sr is +2, the valence state of In is +3, the valence state of O is -2, and the valence state of S is -2.

2. An oxysulfide, characterized in that: Sr in Sr3In4O4S5 may be partially replaced by, including but not limited to, Ca, Ba or Pb.

3. An oxysulfide, characterized in that: The S in Sr3In4O4S5 may be partially replaced by, including but not limited to, Se or Te.

4. A method for preparing the oxysulfide according to claims 1 to 3, characterized in that: The synthesis is carried out by high temperature solid phase reaction, comprising the following steps: (1) Mix raw materials containing Sr element, In element, O element, S element and doping element and grind them evenly, wherein the molar ratio of Sr / In / O / S elements is (2.8~3.5):4:4:(4.8~5.5); (2) In a vacuum or inert atmosphere, heat the sample obtained in step (1) from room temperature to 650-800°C, keep the temperature for 24-72 hours, then cool it to 500°C within 24-72 hours, and then naturally cool it to room temperature.

5. A method for preparing oxysulfide according to claims 1 to 3, characterized in that: Adding a flux to the reaction raw materials comprises the following steps: (1) Mixing raw materials containing Sr, In, O, S, and doping elements with flux and grinding them evenly, wherein the molar ratio of Sr / In / O / S elements is (2.8-3.5):4:4:(4.8-5.5), and the flux types include but are not limited to alkali metal halides KCl, KI or CsI; (2) Heat the reactants from room temperature to 700~800℃ in a vacuum or inert atmosphere, keep them at this temperature for 24~72 hours, then cool them to 500℃ within 24~72 hours, and then naturally cool them to room temperature. Wash away the flux with deionized water and dry them.

6. A surface modification method for oxysulfide according to claims 1 to 3, characterized in that: Disperse it in a dilute acid solution with a hydrogen ion concentration of 0.01 to 0.1 mol / L, stir at room temperature for 10 to 24 hours, filter, wash with deionized water, and dry.

7. Use of the oxysulfide according to any one of claims 1 to 3 in photocatalytic decomposition of water to produce hydrogen and oxygen.

8. Use of the oxysulfide prepared by the preparation or modification method according to any one of claims 4 to 6 in photocatalytic decomposition of water to produce hydrogen and oxygen.

Citation Information

Patent Citations

  • Mixed oxides and sulphides of bismuth and copper for photovoltaic use

    CN106660821A

  • Activation-free ion mechanoluminescence metal sulfur oxide as well as preparation method and application thereof

    CN114316954A

  • Oxo-sulfide nonlinear optical crystal and preparation method and application thereof

    CN114808132A

  • Novel oxysulfide photocatalyst as well as preparation method and application thereof

    CN117205944A

  • Thin film photovoltaic cell, especially a copper-indium selenide based solar cell, has beta-indium oxysulfide buffer layer between absorbent photoconductive layer and transparent conductive layer

    FR2782574A1