Spherical medical tantalum alloy powder and preparation method and application thereof

Through two plasma spheroidization and planetary grinding technology, the problems of element burnout and low density in the preparation of tantalum alloy powder were solved, and high-performance spherical medical tantalum alloy powder was prepared for biomedical implantation devices, which improved the biological phase Capacitance and antibacterial properties.

CN118751922BActive Publication Date: 2024-11-29GUANGDONG INST OF NEW MATERIALS +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411227044.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-29
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

The existing tantalum metal powder preparation methods for additive manufacturing have problems such as large amount of element burnout and low density, and their performance needs to be further improved, making it difficult to meet the needs of high-performance biomedical implantable devices.

Method used

Using two plasma spheroidization technology combined with planetary grinding technology, the pure tantalum powder is first subjected to preliminary plasma spheroidization, then mixed with copper and silver particles for planetary grinding, and finally secondary plasma spheroidization is performed to reduce element burning and increase density , prepared spherical medical tantalum alloy powder.

Benefits of technology

A spherical medical tantalum alloy powder with small element burn loss, high density and high spherical shape was obtained. It has excellent cell compatibility and antibacterial properties. It is suitable for the manufacturing of high-end implantable devices, which improves the success rate of medical applications and Economic value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118751922B_ABST
    Figure CN118751922B_ABST
Patent Text Reader

Abstract

The present invention provides a spherical medical tantalum alloy powder and a preparation method and application thereof, wherein the preparation method comprises the following steps: S1. Preliminary plasma spheroidization of pure tantalum powder to obtain spherical pure tantalum powder; S2. Mixing the spherical pure tantalum powder obtained in S1 with pure copper particles and pure silver particles, and planetary ball milling to obtain a mixed metal powder; S3. Plasma spheroidization of the mixed metal powder obtained in S2, screening and filtering to obtain the spherical medical tantalum alloy powder. The present invention effectively reduces the burning loss of copper and silver through the preparation method of combining the secondary plasma spheroidization technology with the planetary ball milling technology, and further improves the spheroidization rate of the tantalum alloy powder, and coats the outside of the tantalum powder with copper and silver, thereby obtaining a spherical medical tantalum alloy powder with less element burning loss and high density, which is suitable for additive manufacturing, has high sphericity, less non-qualified spheres such as irregular particles or satellite powders, and excellent biocompatibility, and can be used in the medical field, with important economic value and promotion significance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of metal powder materials and preparation technology, and in particular to a spherical medical tantalum alloy powder and a preparation method and application thereof. Background Art

[0002] Tantalum metal has the characteristics of high strength, good plasticity and ductility, high chemical stability, corrosion resistance, high mechanical reliability, and good fatigue resistance, which makes it have a very broad application field. In the past decade, as a "biophilic" metal, tantalum has received widespread attention for its potential in the medical field. Tantalum metal can exist stably in the entire pH range, maintain very stable chemical properties in the human body fluid environment, has strong corrosion resistance, is non-cytotoxic, does not release harmful elements, and is not absorbed by the human body. It shows excellent cell compatibility and biostability. At the same time, tantalum also has excellent cell adhesion. It is an ideal high-performance biomedical metal material. It can be used to manufacture high-end implantable interventional devices through additive manufacturing and is widely used in medical fields such as orthopedics, craniomaxillofacial, oral and major surgery.

[0003] At present, the preparation methods of tantalum metal powder for additive manufacturing on the market include: radio frequency plasma spheroidization atomization method, electric explosion atomization method, and rotating electrode atomization method. The raw material of the radio frequency plasma spheroidization atomization method is irregular particle powder. The prepared tantalum powder has the advantages of high sphericity, uniform composition, and high powder yield. The disadvantage is that the oxygen content of the prepared powder is greatly affected by the raw material particles, and the raw materials are required to be high. The electric explosion atomization method is more suitable for the preparation of micron-level powders. The conventional powder particle size with a higher yield is in the range of 0-10 microns, while the particle size of the powder suitable for 3D printing is 15-53μm. When the electric explosion method is used to prepare particles of tens of microns, the relative powder yield is low. The rotating electrode atomization method uses rods as raw materials. Its advantages are that the prepared spherical tantalum powder has a higher sphericity and a higher powder yield, but the main particle size range is concentrated in 45-150μm, and the content of powder in the range of 15-53μm suitable for 3D printing is low. At the same time, there are problems of element burnout and density when preparing tantalum alloy powder by electric explosion atomization method and rotating electrode atomization method.

[0004] Chinese patent CN114540689A "An ultra-low elastic modulus antibacterial medical tantalum alloy and preparation method thereof" discloses a method for obtaining a tantalum alloy by mechanical alloying and spark plasma sintering. However, this method obtains tantalum alloy powder by ordinary ball milling and then directly forms parts by spark plasma sintering instead of preparing powder suitable for additive manufacturing. There is still the problem of element burnout, and its performance still needs to be further improved.

[0005] Therefore, it is of great significance to develop a spherical medical tantalum alloy powder with low element burnout, high density, excellent performance, and suitable for additive manufacturing, and a preparation method thereof. Summary of the invention

[0006] In view of the problems that the existing additively manufactured medical tantalum alloy powder has a large amount of element burnout and low density, and the performance still needs to be further improved, the present invention provides a spherical medical tantalum alloy powder and a preparation method thereof. The main component is tantalum, and the alloy components are copper and silver. It is prepared by a specific preparation method, has high tensile strength, yield strength, and excellent biocompatibility. It can be used in the medical field of implantable devices to prepare biomedical implantable devices or stents, and has important economic value and promotion significance.

[0007] To achieve the above object, the technical solution adopted by the present invention is:

[0008] A method for preparing spherical medical tantalum alloy powder comprises the following steps:

[0009] S1. Preliminary plasma spheroidization of pure tantalum powder to obtain spherical pure tantalum powder;

[0010] S2. The spherical pure tantalum powder obtained in S1 is mixed with pure copper particles and pure silver particles, and subjected to planetary ball milling to obtain a mixed metal powder;

[0011] S3. The mixed metal powder obtained in S2 is plasma spheroidized, sieved and filtered to obtain the spherical medical tantalum alloy powder.

[0012] The present invention selects to compound pure tantalum with copper and silver elements to obtain tantalum alloy powder, which gives the tantalum alloy excellent antibacterial function, so that the spherical medical tantalum alloy powder of the present invention not only has excellent cell compatibility and biostability, but also has significant antibacterial properties. It is expected to reduce the infection rate of surrounding tissues of tantalum alloy implant devices made of spherical medical tantalum alloy powder during clinical use, and improve medical efficacy and clinical use success rate.

[0013] The invention firstly plasma spheroidizes pure tantalum powder, then mixes it with pure copper particles and pure silver particles for planetary ball milling, fully mixes the alloy powder, and finally plasma spheroidizes the mixed metal powder to obtain spherical medical tantalum alloy powder, fully utilizing the advantages of radio frequency plasma spheroidization atomization method such as fast heating and cooling speed, short sintering time, high density, clean preparation process, etc., improves the component segregation and structural inhomogeneity of the alloy, and reduces the alloy manufacturing cost; by first plasma spheroidizing the pure tantalum powder once to obtain the pure tantalum powder with a certain spheroidization rate, it is easy to control Subsequently, the mixed metal powder is subjected to secondary plasma spheroidization to obtain the power of the formed powder, thereby reducing the burnout of copper and silver; pure tantalum is mixed with pure copper particles and pure silver particles through planetary ball milling to further improve the spheroidization rate of the tantalum alloy powder, and copper and silver are coated on the outside of the tantalum powder to increase the density of the spherical medical tantalum alloy powder; finally, a spherical medical tantalum alloy powder with less element burnout and high density suitable for additive manufacturing is obtained through secondary plasma spheroidization, with high sphericity, few non-qualified spheres such as special-shaped particles or satellite powders, and excellent biocompatibility.

[0014] Furthermore, the particle size of the pure tantalum powder in S1 is ≤200 μm.

[0015] The present invention preferably uses pure tantalum powder with a particle size range of ≤200 μm, so as to facilitate the subsequent secondary plasma spheroidization technology combined with planetary ball milling technology to obtain spherical medical tantalum alloy powder with a particle size in the range of 15-53 μm suitable for 3D printing.

[0016] Furthermore, the process parameters of the preliminary plasma spheroidization in S1 and the plasma spheroidization in S3 are independently: the powder supply rate is 10-20 g·min -1 , the carrier gas flow rate of the protective gas is 5-15L / min, the central gas flow rate is 15-25L / min, the sheath gas flow rate is 50-80 L / min, the grid current is 0.2-0.6A, the plate voltage is 5-15KV, and the plate current is 2-6A.

[0017] The preferred powder supply rate of the present invention is 10-20 g·min -1 The plasma spheroidization process parameters of the protective gas are 5-15L / min, the central gas flow rate is 15-25L / min, the sheath gas flow rate is 50-80 L / min, the grid current is 0.2-0.6A, the plate voltage is 5-15KV, and the plate current is 2-6A. By controlling the powder supply rate, carrier gas flow rate, grid current, plate voltage and plate current, the porosity and element burnout rate of the spherical medical tantalum alloy powder are further reduced, and the density is further improved, thereby obtaining a spherical medical tantalum alloy powder with less element burnout and higher density, which is suitable for additive manufacturing, has higher sphericity, and very few non-qualified spheres such as special-shaped particles or satellite powders.

[0018] Furthermore, the process parameters of the preliminary plasma spheroidization in S1 and the plasma spheroidization in S3 are independently: the powder feeding rate is 10 g·min -1 The carrier gas flow rate of the protective gas is 15 L / min, the central gas flow rate is 20 L / min, the sheath gas flow rate is 65 L / min, the gate current is 0.3 A, the plate voltage is 5 KV, the plate current is 2.5 A, and the protective gas, central gas and sheath gas are Ar.

[0019] Furthermore, the particle size of the pure copper particles in S2 is 10-100 nm; the particle size of the pure silver particles is 10-100 nm.

[0020] The present invention preferably uses pure copper particles and pure silver particles with a particle size range of 10-100 nm, which is convenient for coating copper and silver on the outside of tantalum powder in planetary ball milling and combining secondary plasma spheroidization technology with planetary ball milling technology to obtain spherical medical tantalum alloy powder with a particle size in the range of 15-53 μm suitable for 3D printing.

[0021] Furthermore, the rotation speed of the main turntable of the planetary ball mill in S2 is 50-200 r / min, and the rotation speed of the ball mill is 50-400 r / min.

[0022] The present invention preferably adopts planetary ball milling process parameters of main turntable speed of 50-200r / min and ball mill tank speed of 50-400r / min. By controlling the ball mill speed, pure tantalum powder is fully and evenly mixed with pure copper particles and pure silver particles. A series of plastic deformations occur during the ball milling process, so that the powder is refined after ball milling, and the flaky large particle powder is increased, which makes it easier to more evenly coat copper and silver on the outside of the tantalum powder, thereby obtaining a spherical medical tantalum alloy powder with more uniform composition and better performance.

[0023] Furthermore, the rotation speed of the main turntable of the planetary ball mill in S2 is 100r / min, and the rotation speed of the ball mill tank is 200r / min.

[0024] Another object of the present invention is to provide a spherical medical tantalum alloy powder.

[0025] A spherical medical tantalum alloy powder is prepared by any of the above-mentioned preparation methods.

[0026] Furthermore, the metal elements are included in the following weight percentages: Ta: 89-98.9%, Ag: 0.1-1%, Cu: 1-10%.

[0027] The present invention preferably adopts an element composition ratio of Ta: 89-98.9%, Ag: 0.1-1%, and Cu: 1-10%, wherein the weight of Cu is about 5-10 times that of Ag. By controlling the element composition ratio of pure tantalum, copper element, and silver element, it is ensured that trace copper ions and silver ions can be released from the surface of the spherical medical tantalum alloy powder for a long time, thereby giving the spherical medical tantalum alloy powder a continuous and excellent antibacterial function, and it is ensured that the spherical medical tantalum alloy powder does not release too many copper ions or silver ions, thereby affecting the corrosion resistance and biosafety of the spherical medical tantalum alloy powder.

[0028] Furthermore, the particle size is 15-53 μm.

[0029] Another object of the present invention is to provide an application of spherical medical tantalum alloy powder.

[0030] The spherical medical tantalum alloy powder is used for additive manufacturing.

[0031] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0032] The spherical medical tantalum alloy powder of the present invention is different from pure tantalum powder. The tantalum alloy contains silver and copper whose melting points are far different from those of tantalum. If the spherical medical tantalum alloy powder is prepared by rotating electrode atomization, on the one hand, the rotating electrode atomization needs to melt the tantalum-silver-copper alloy in advance and process it into rods, which increases the smelting step. The long smelting cycle increases the overall powder making process time and increases the preparation cost greatly. On the other hand, in the rotating electrode atomization powder making process, in order to obtain tantalum alloy powder with higher sphericity, the alloy needs to be completely melted and sprayed out. When the temperature of melting tantalum is reached, a large amount of silver and copper will inevitably be burned and accompanied by steam, which will seriously affect the composition accuracy of the powder particles and the density of the particles.

[0033] For example, if the electric explosion method is used to prepare spherical medical tantalum alloy powder, firstly, it also needs to add the step of smelting the required wire or rod in the early stage, and the raw materials are usually thin metal wires, which are difficult to process; secondly, the electric explosion method uses pre-stored electrical energy to pulse discharge the metal conductor (conductor wire or foil). The large pulse current causes the metal conductor to melt, vaporize, and expand, and an explosion occurs to obtain powder. When the temperature of molten tantalum is reached, a large amount of silver and copper will be burned and accompanied by steam, which seriously affects the accuracy of the powder particle composition and the density of the particles; finally, the metal powder generated by the electric explosion method has a small particle size, a large specific surface area, a high activity, and is difficult to collect.

[0034] After repeated research, the present invention creatively combines the secondary plasma spheroidization technology with the planetary ball milling technology to obtain pure tantalum powder with a certain spheroidization rate through preliminary plasma spheroidization, and then mixes it with pure copper particles and pure silver particles for planetary ball milling to fully mix the alloy powder. Finally, the mixed metal powder is plasma spheroidized to obtain spherical medical tantalum alloy powder. The burnout of copper and silver can be reduced by controlling the power of plasma spheroidization, and the spheroidization rate of the tantalum alloy powder can be further improved. Copper and silver are coated on the outside of the tantalum powder, thereby obtaining spherical medical tantalum alloy powder with less element burnout and high density, which is suitable for additive manufacturing. The powder has high sphericity, few non-qualified spheres such as special-shaped particles or satellite powders, and excellent biocompatibility. It can be used in the medical field and has important economic value and promotion significance. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] The invention is further described using the accompanying drawings, but the embodiments in the accompanying drawings do not constitute any limitation to the invention. A person skilled in the art can obtain other drawings based on the following drawings without creative work.

[0036] Figure 1 Schematic diagram of tantalum alloy powder prepared by the present invention.

[0037] Figure 2 This is the SEM image of Example 1 of the present invention.

[0038] Figure 3 It is the SEM picture of comparative example 1 of the present invention.

[0039] Figure 4 This is a cell staining fluorescence microscope image of the sample prepared in Example 1 of the present invention.

[0040] Figure 5 It is a cell staining fluorescence microscope picture of the sample prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0041] In order to better illustrate the purpose, technical scheme and advantages of the present invention, the present invention is further described by the following examples. Obviously, the following examples are only part of the embodiments of the present invention, rather than all the embodiments; it should be understood that the embodiments of the present invention are only used to illustrate the technical effects of the present invention, rather than to limit the scope of protection of the present invention.

[0042] The raw materials in the examples can all be obtained commercially; unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0043] Embodiment 1: A method for preparing spherical medical tantalum alloy powder, comprising the following steps:

[0044] The spherical medical tantalum alloy powder includes the following metal elements in weight percentage: 94.5% Ta, 0.5% Ag, and 5% Cu.

[0045] S1. Preliminary plasma spheroidization of pure tantalum powder with a particle size of ≤200μm, with a powder supply rate of 15g·min -1 , the carrier gas flow rate of the protective gas Ar is 15 L / min, the central gas Ar flow rate is 20 L / min, the sheath gas Ar flow rate is 65 L / min, the grid current is 0.4 A, the plate voltage is 7 KV, and the plate current is 3.5 A, and spherical pure tantalum powder is obtained;

[0046] S2. The spherical pure tantalum powder obtained in S1 is mixed with pure copper particles having a particle size of 10-100 nm and pure silver particles having a particle size of 10-100 nm, and the mixture is subjected to planetary ball milling at a main turntable speed of 100 r / min and a ball milling tank speed of 200 r / min to obtain a mixed metal powder;

[0047] S3. The mixed metal powder obtained in S2 is plasma spheroidized at a powder supply rate of 10 g min -1 The carrier gas flow rate of the protective gas Ar is 15 L / min, the central gas Ar flow rate is 20 L / min, the sheath gas Ar flow rate is 65 L / min, the gate current is 0.3 A, the plate voltage is 5 KV, the plate current is 2.5 A, and the tantalum alloy powder with a particle size of 15-53 μm is obtained by sieving and filtering to obtain the spherical medical tantalum alloy powder.

[0048] Embodiment 2: A method for preparing spherical medical tantalum alloy powder, comprising the following steps:

[0049] The spherical medical tantalum alloy powder includes the following metal elements in weight percentage: 98.9% Ta, 0.1% Ag, and 1% Cu.

[0050] S1. Preliminary plasma spheroidization of pure tantalum powder with a particle size of ≤200μm, with a powder supply rate of 18g·min -1 , the carrier gas flow rate of the protective gas Ar is 15 L / min, the central gas Ar flow rate is 20 L / min, the sheath gas Ar flow rate is 65 L / min, the grid current is 0.4 A, the plate voltage is 7 KV, and the plate current is 3.5 A, and spherical pure tantalum powder is obtained;

[0051] S2. The spherical pure tantalum powder obtained in S1 is mixed with pure copper particles having a particle size of 10-100 nm and pure silver particles having a particle size of 10-100 nm, and the mixture is subjected to planetary ball milling at a main turntable speed of 100 r / min and a ball milling tank speed of 200 r / min to obtain a mixed metal powder;

[0052] S3. The mixed metal powder obtained in S2 is plasma spheroidized at a powder supply rate of 10 g min-1 The carrier gas flow rate of the protective gas Ar is 15 L / min, the central gas Ar flow rate is 20 L / min, the sheath gas Ar flow rate is 65 L / min, the gate current is 0.3 A, the plate voltage is 5 KV, the plate current is 2.5 A, and the tantalum alloy powder with a particle size of 15-53 μm is obtained by sieving and filtering to obtain the spherical medical tantalum alloy powder.

[0053] Embodiment 3: A method for preparing spherical medical tantalum alloy powder, comprising the following steps:

[0054] The spherical medical tantalum alloy powder includes the following weight percentages of metal elements: 89% Ta, 1% Ag, and 10% Cu.

[0055] S1. Preliminary plasma spheroidization of pure tantalum powder with a particle size of ≤200μm, with a powder supply rate of 20g·min -1 , the carrier gas flow rate of the protective gas Ar is 15 L / min, the central gas Ar flow rate is 20 L / min, the sheath gas Ar flow rate is 65 L / min, the grid current is 0.4 A, the plate voltage is 7 KV, and the plate current is 3.5 A, and spherical pure tantalum powder is obtained;

[0056] S2. The spherical pure tantalum powder obtained in S1 is mixed with pure copper particles having a particle size of 10-100 nm and pure silver particles having a particle size of 10-100 nm, and the mixture is subjected to planetary ball milling at a main turntable speed of 100 r / min and a ball milling tank speed of 200 r / min to obtain a mixed metal powder;

[0057] S3. The mixed metal powder obtained in S2 is plasma spheroidized at a powder supply rate of 10 g min -1 The carrier gas flow rate of the protective gas Ar is 15 L / min, the central gas Ar flow rate is 20 L / min, the sheath gas Ar flow rate is 65 L / min, the gate current is 0.3 A, the plate voltage is 5 KV, the plate current is 2.5 A, and the tantalum alloy powder with a particle size of 15-53 μm is obtained by sieving and filtering to obtain the spherical medical tantalum alloy powder.

[0058] Embodiment 4: A method for preparing spherical medical tantalum alloy powder, comprising the following steps:

[0059] The spherical medical tantalum alloy powder includes the following metal elements in weight percentage: 94.5% Ta, 0.5% Ag, and 5% Cu.

[0060] S1. Preliminary plasma spheroidization of pure tantalum powder with a particle size of ≤200μm, with a powder supply rate of 10g·min -1, the carrier gas flow rate of the protective gas Ar is 5 L / min, the central gas Ar flow rate is 15 L / min, the sheath gas Ar flow rate is 50 L / min, the grid current is 0.2 A, the plate voltage is 5 KV, and the plate current is 2 A, and spherical pure tantalum powder is obtained;

[0061] S2. The spherical pure tantalum powder obtained in S1 is mixed with pure copper particles having a particle size of 10-100 nm and pure silver particles having a particle size of 10-100 nm, and the mixture is subjected to planetary ball milling at a main turntable speed of 50 r / min and a ball milling tank speed of 50 r / min to obtain a mixed metal powder;

[0062] S3. The mixed metal powder obtained in S2 is plasma spheroidized at a powder supply rate of 10 g min -1 The carrier gas flow rate of the protective gas Ar is 5 L / min, the central gas Ar flow rate is 15 L / min, the sheath gas Ar flow rate is 50 L / min, the gate current is 0.2 A, the plate voltage is 5 KV, the plate current is 2 A, and the tantalum alloy powder with a particle size of 15-53 μm is obtained by sieving and filtering to obtain the spherical medical tantalum alloy powder.

[0063] Embodiment 5: A method for preparing spherical medical tantalum alloy powder, comprising the following steps:

[0064] The spherical medical tantalum alloy powder includes the following metal elements in weight percentage: 94.5% Ta, 0.5% Ag, and 5% Cu.

[0065] S1. Preliminary plasma spheroidization of pure tantalum powder with a particle size of ≤200μm, with a powder supply rate of 20g·min -1 , the carrier gas flow rate of the protective gas Ar is 15L / min, the central gas Ar flow rate is 25L / min, the sheath gas Ar flow rate is 80L / min, the grid current is 0.6A, the plate voltage is 15KV, and the plate current is 6A, and spherical pure tantalum powder is obtained;

[0066] S2. The spherical pure tantalum powder obtained in S1 is mixed with pure copper particles having a particle size of 10-100 nm and pure silver particles having a particle size of 10-100 nm, and the mixture is subjected to planetary ball milling at a main turntable speed of 200 r / min and a ball milling tank speed of 400 r / min to obtain a mixed metal powder;

[0067] S3. The mixed metal powder obtained in S2 is plasma spheroidized at a powder supply rate of 20 g min -1 The carrier gas flow rate of the protective gas Ar is 15 L / min, the central gas Ar flow rate is 25 L / min, the sheath gas Ar flow rate is 80 L / min, the gate current is 0.6 A, the plate voltage is 15 KV, the plate current is 6 A, and the tantalum alloy powder with a particle size of 15-53 μm is obtained by sieving and filtering to obtain the spherical medical tantalum alloy powder.

[0068] Embodiment 6: A method for preparing spherical medical tantalum alloy powder, comprising the following steps:

[0069] The spherical medical tantalum alloy powder includes the following metal elements in weight percentage: 94.5% Ta, 0.5% Ag, and 5% Cu.

[0070] S1. Preliminary plasma spheroidization of pure tantalum powder with a particle size of ≤200μm, with a powder supply rate of 10g·min -1 , the carrier gas flow rate of the protective gas Ar is 5 L / min, the central gas Ar flow rate is 15 L / min, the sheath gas Ar flow rate is 50 L / min, the grid current is 0.2 A, the plate voltage is 5 KV, and the plate current is 2 A, and spherical pure tantalum powder is obtained;

[0071] S2. The spherical pure tantalum powder obtained in S1 is mixed with pure copper particles having a particle size of 10-100 nm and pure silver particles having a particle size of 10-100 nm, and the mixture is subjected to planetary ball milling at a main turntable speed of 100 r / min and a ball milling tank speed of 200 r / min to obtain a mixed metal powder;

[0072] S3. The mixed metal powder obtained in S2 is plasma spheroidized at a powder supply rate of 20 g min -1 The carrier gas flow rate of the protective gas Ar is 15 L / min, the central gas Ar flow rate is 25 L / min, the sheath gas Ar flow rate is 80 L / min, the gate current is 0.6 A, the plate voltage is 15 KV, the plate current is 6 A, and the tantalum alloy powder with a particle size of 15-53 μm is obtained by sieving and filtering to obtain the spherical medical tantalum alloy powder.

[0073] Embodiment 7: A method for preparing spherical medical tantalum alloy powder, comprising the following steps:

[0074] The spherical medical tantalum alloy powder includes the following metal elements in weight percentage: 94.5% Ta, 0.5% Ag, and 5% Cu.

[0075] S1. Preliminary plasma spheroidization of pure tantalum powder with a particle size of ≤200μm, with a powder supply rate of 20g·min -1 , the carrier gas flow rate of the protective gas Ar is 15L / min, the central gas Ar flow rate is 25L / min, the sheath gas Ar flow rate is 80L / min, the grid current is 0.6A, the plate voltage is 15KV, and the plate current is 2A, and spherical pure tantalum powder is obtained;

[0076] S2. The spherical pure tantalum powder obtained in S1 is mixed with pure copper particles having a particle size of 10-100 nm and pure silver particles having a particle size of 10-100 nm, and the mixture is subjected to planetary ball milling at a main turntable speed of 100 r / min and a ball milling tank speed of 200 r / min to obtain a mixed metal powder;

[0077] S3. The mixed metal powder obtained in S2 is plasma spheroidized at a powder supply rate of 10 g min -1 The carrier gas flow rate of the protective gas Ar is 5 L / min, the central gas Ar flow rate is 15 L / min, the sheath gas Ar flow rate is 50 L / min, the gate current is 0.2 A, the plate voltage is 5 KV, the plate current is 2 A, and the tantalum alloy powder with a particle size of 15-53 μm is obtained by sieving and filtering to obtain the spherical medical tantalum alloy powder.

[0078] Comparative Example 1: A method for preparing spherical medical tantalum alloy powder, comprising the following steps:

[0079] The spherical medical tantalum alloy powder includes the following metal elements in weight percentage: 94.5% Ta, 0.5% Ag, and 5% Cu.

[0080] S1. Preliminary plasma spheroidization of pure tantalum powder with a particle size of ≤200μm, with a powder supply rate of 15g·min -1 , the carrier gas flow rate of the protective gas Ar is 15 L / min, the central gas Ar flow rate is 20 L / min, the sheath gas Ar flow rate is 65 L / min, the grid current is 0.4 A, the plate voltage is 7 KV, and the plate current is 3.5 A, and spherical pure tantalum powder is obtained;

[0081] S2. The spherical pure tantalum powder obtained in S1 is mixed with pure copper particles having a particle size of 10-100 nm and pure silver particles having a particle size of 10-100 nm, and the mixture is subjected to planetary ball milling at a main turntable speed of 100 r / min and a ball milling tank speed of 200 r / min to obtain a mixed metal powder;

[0082] S3. The mixed metal powder obtained in S2 is plasma spheroidized at a powder supply rate of 25 g min -1 The carrier gas flow rate of the protective gas Ar is 15 L / min, the central gas Ar flow rate is 20 L / min, the sheath gas Ar flow rate is 65 L / min, the gate current is 0.3 A, the plate voltage is 5 KV, the plate current is 2.5 A, and the tantalum alloy powder with a particle size of 15-53 μm is obtained by sieving and filtering to obtain the spherical medical tantalum alloy powder.

[0083] Compared with Example 1, the powder feeding rate in step S3 of this comparative example is 25 g·min -1 .

[0084] Comparative Example 2: A method for preparing spherical medical tantalum alloy powder, comprising the following steps:

[0085] The spherical medical tantalum alloy powder includes the following weight percentages of metal elements: 90% Ta, 10% Cu.

[0086] S1. Preliminary plasma spheroidization of pure tantalum powder with a particle size of ≤200μm, with a powder supply rate of 15g·min -1 , the carrier gas flow rate of the protective gas Ar is 15 L / min, the central gas Ar flow rate is 20 L / min, the sheath gas Ar flow rate is 65 L / min, the grid current is 0.4 A, the plate voltage is 7 KV, and the plate current is 3.5 A, and spherical pure tantalum powder is obtained;

[0087] S2. The spherical pure tantalum powder obtained in S1 is mixed with pure copper particles having a particle size of 10-100 nm, and the mixture is subjected to planetary ball milling at a main turntable speed of 100 r / min and a ball milling tank speed of 200 r / min to obtain a mixed metal powder;

[0088] S3. The mixed metal powder obtained in S2 is plasma spheroidized at a powder supply rate of 10 g min -1 The carrier gas flow rate of the protective gas Ar is 15 L / min, the central gas Ar flow rate is 20 L / min, the sheath gas Ar flow rate is 65 L / min, the gate current is 0.3 A, the plate voltage is 5 KV, the plate current is 2.5 A, and the tantalum alloy powder with a particle size of 15-53 μm is obtained by sieving and filtering to obtain the spherical medical tantalum alloy powder.

[0089] Compared with Example 1, the alloy element content of this comparative example is: 90% Ta, 10% Cu.

[0090] The microscopic morphology of Example 1 and Comparative Example 1 was analyzed, and the SEM images thereof are as follows: Figure 2 , Figure 3 As shown in the figure, it can be seen that the spherical medical tantalum alloy powder prepared by the preparation method of the present invention has a high sphericity, and basically has no irregular particles or satellite powders and other unqualified spheres. The test results of the other embodiments are basically consistent. However, in Comparative Example 1, due to the excessive supply rate of the powder, some particles cannot be fully spheroidized in time, the powder is sprayed too densely, and some molten metal droplets adhere to the surrounding particles or solidify directly in an irregular state, resulting in a low sphericity and affecting the yield rate.

[0091] Laser 3D printing was performed on Example 1 and Comparative Example 2, and the prepared samples were subjected to cytotoxicity experiments. The cell staining fluorescence microscope images are shown in FIG. Figure 4 , Figure 5 As shown in the figure, Figure 4In the microscope field of view, it can be clearly observed that the cell tissue is stained, and the distribution of cells is relatively uniform and dense, which indicates that the sample prepared by using the spherical medical tantalum alloy powder of the present invention has good biological activity. Figure 5 It was found after staining that there were almost no living cells in the microscope field of view, which indicated that the tantalum alloy powder simply added with copper in Comparative Example 2 had certain cytotoxicity and affected the normal culture of cells.

[0092] In summary, the present invention adopts a preparation method combining secondary plasma spheroidization technology with planetary ball milling technology, obtains pure tantalum powder with a certain spheroidization rate through preliminary plasma spheroidization, and then mixes it with pure copper particles and pure silver particles for planetary ball milling to fully mix the alloy powder, and finally plasma spheroidizes the mixed metal powder, reduces the burnout of copper and silver by controlling the power of spheroidization, and further improves the spheroidization rate of tantalum alloy powder, and coats copper and silver on the outside of tantalum powder to obtain spherical medical tantalum alloy powder with less element burnout and high density, which is suitable for additive manufacturing, has high sphericity, less non-qualified spheres such as irregular particles or satellite powder, and excellent biocompatibility, can be used in the medical field, and has important economic value and promotion significance.

[0093] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing spherical medical tantalum alloy powder, characterized in that: The following steps are involved: S1. Preliminary plasma spheroidization of pure tantalum powder to obtain spherical pure tantalum powder; S2. The spherical pure tantalum powder obtained in S1 is mixed with pure copper particles and pure silver particles, and subjected to planetary ball milling to obtain a mixed metal powder; S3. The mixed metal powder obtained in S2 is plasma spheroidized, sieved and filtered to obtain the spherical medical tantalum alloy powder; The process parameters of the preliminary plasma spheroidization in S1 and the plasma spheroidization in S3 are independently: the powder feeding rate is 10-20 g·min -1 , the carrier gas flow rate of the protective gas is 5-15L / min, the central gas flow rate is 15-25L / min, the sheath gas flow rate is 50-80 L / min, the grid current is 0.2-0.6A, the plate voltage is 5-15KV, and the plate current is 2-6A.

2. A method for preparing spherical medical tantalum alloy powder according to claim 1, characterized in that: The particle size of the pure tantalum powder described in S1 is ≤200 μm.

3. A method for preparing spherical medical tantalum alloy powder according to claim 1, characterized in that: The process parameters of the preliminary plasma spheroidization in S1 and the plasma spheroidization in S3 are independently: the powder feeding rate is 10 g·min -1 The carrier gas flow rate of the protective gas is 15 L / min, the central gas flow rate is 20 L / min, the sheath gas flow rate is 65 L / min, the gate current is 0.3 A, the plate voltage is 5 KV, the plate current is 2.5 A, and the protective gas, central gas and sheath gas are Ar.

4. A method for preparing spherical medical tantalum alloy powder according to claim 1, characterized in that: The particle size of the pure copper particles in S2 is 10-100 nm; the particle size of the pure silver particles is 10-100 nm.

5. A method for preparing spherical medical tantalum alloy powder according to claim 1, characterized in that: S2 The main rotating disk speed of the planetary ball mill is 50-200r / min, and the rotating speed of the ball mill is 50-400r / min.

6. A spherical medical tantalum alloy powder, characterized in that: Prepared by the preparation method according to any one of claims 1 to 5.

7. A spherical medical tantalum alloy powder according to claim 6, characterized in that: The metal elements are included in the following weight percentages: Ta: 89-98.9%, Ag: 0.1-1%, Cu: 1-10%.

8. A spherical medical tantalum alloy powder according to claim 6, characterized in that: The particle size is 15-53μm.

9. A spherical medical tantalum alloy powder according to any one of claims 6 to 8, used for additive manufacturing.

Citation Information

Patent Citations

  • Ultralow elastic modulus antibacterial medical tantalum alloy and preparation method thereof

    CN114540689A

  • 3D printing manufacturing method for metal tantalum and application

    CN109014181A

  • Spherical tantalum powder, preparation thereof and application of spherical tantalum powder in 3D printing

    CN114653959A

  • Porous tantalum medical implant material and preparation method and application thereof

    CN114855024A

  • Antibacterial osteogenesis-promoting medical nano-porous tantalum-copper alloy and preparation method thereof