Preparation method and application of nanoscale lithium iron phosphate battery positive electrode material

By using water-absorbent resin powder for high-temperature sintering in the preparation of lithium iron phosphate battery cathode materials, the problem of insufficient high-rate charge and discharge performance of lithium iron phosphate batteries was solved, and nanoscale lithium iron phosphate particles with high conductivity were prepared, which significantly Improved battery charge-discharge performance and cycle performance.

CN118754087APending Publication Date: 2024-10-11YIBIN WANPENG TIMES TECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411072043.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing lithium iron phosphate battery cathode materials have deficiencies in high-rate charge and discharge performance, mainly due to insufficient ion transport capabilities and the difficulty in preparing nanoscale particles using the commonly used solid-phase preparation method, resulting in poor charge and discharge performance.

Method used

A method for preparing nanoscale lithium iron phosphate battery cathode materials is adopted. The lithium source, carbon source, iron source, phosphorus source and water-absorbent resin powder are uniformly dispersed and then sintered at high temperature. The water-absorbent resin is used to release heat at high temperatures to release moisture. And uniformly coat lithium iron phosphate to enhance its conductivity, and prepare lithium iron phosphate particles with a particle size of less than 50nm.

Benefits of technology

It has significantly improved the high-power charge-discharge performance and cycle performance of lithium iron phosphate batteries. Compared with common lithium iron phosphate batteries on the market, the 5C current discharge performance has been improved by 30mAh/g to 50mAh/g, and the chemical activity of the material has been improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754087A_ABST
    Figure CN118754087A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a nanoscale lithium iron phosphate battery positive electrode material, and relates to the technical field of preparation of lithium battery positive electrode materials, and the preparation method comprises the following steps: dissolving acrylic acid, 2-amino-4-chloro-6-methylpyrimidine and sulfathiazole in pure water, then adding sodium hydroxide while stirring, and stirring to obtain a mixed solution; cooling to room temperature, removing oxygen in the container, sequentially adding an initiator and a cross-linking agent for polymerization, and drying and crushing gel after complete reaction to obtain water-absorbent resin powder; the preparation method comprises the following steps: adding a lithium source, a carbon source, an iron source and a phosphorus source into pure water, dispersing to obtain slurry, grinding the slurry to obtain precursor slurry, then adding water-absorbent resin powder into the precursor slurry, stirring and uniformly mixing, aging and absorbing water in a constant-temperature space, sintering after water absorption is completed and colloid is stable, and thus obtaining the lithium ion battery positive electrode material. And crushing the sintered product by air flow to obtain the nanoscale lithium iron phosphate battery positive electrode material. And the charge-discharge performance and the cycle performance of the lithium iron phosphate battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of preparation of positive electrode materials for lithium batteries, and in particular to a preparation method and application of a nano-scale positive electrode material for lithium iron phosphate batteries. Background Art

[0002] Lithium iron phosphate is the mainstream positive electrode material for power batteries at present. It has the advantages of strong energy storage capacity, low price, safety, and strong cycle capacity, and is popular in the market. Olivine lithium iron phosphate (LiFePO4) has a high theoretical specific capacity (170mAh / g), a stable charging and discharging platform, a large volume energy density, safety, non-toxicity, and low price. It is one of the most promising positive electrode materials for lithium-ion power batteries. With the advancement of technology, various new handheld mobile devices and power tools are constantly emerging in the market, and the rapid iteration of new energy vehicles has made people put forward higher requirements for the capacity, charging and discharging capacity, and safety performance of lithium iron phosphate batteries. However, with the rapid iteration of products, consumers have put forward higher requirements for the rapid energy replenishment and high-power discharge performance of electric vehicles. The type and performance of the positive active material in the battery material have a decisive influence on the electrical performance of the battery. Due to its material crystal characteristics, lithium iron phosphate itself has weaker high-rate charging and discharging performance than ternary materials.

[0003] At present, the main reason that restricts the high-rate charge and discharge performance of finished lithium iron phosphate batteries is that the lithium iron phosphate positive electrode material itself has insufficient ion transmission capacity and narrow ion transmission channels. The commonly used method to improve the ion transmission capacity of lithium iron phosphate positive electrode materials is mainly to coat the outer layer of lithium iron phosphate with amorphous and shaped carbon to improve the ion transmission capacity of the material and improve the conductivity. However, this method has limited ion transmission capacity of the material, resulting in poor charge and discharge performance when lithium iron phosphate is used as a positive electrode material for batteries.

[0004] In the prior art, the most common solid-phase method for preparing lithium iron phosphate is to first prepare a uniformly dispersed suspension of carbon source, phosphorus source, iron source, lithium source, pure water, etc. with a certain solid content, then use sand milling or ball milling to increase the uniformity of the particles and reduce the particle size, and then use spray drying to granulate, convert the suspension into powder, and then put the powder into a sagger for high-temperature sintering. However, during the sintering process, the powder will still maintain the morphology of spherical particles, and the particles are prone to agglomeration, making it difficult to produce nano-scale particles. Summary of the invention

[0005] Based on the problem that the current method for preparing lithium iron phosphate has poor charge and discharge performance, the purpose of the present invention is to provide a method for preparing a nano-scale lithium iron phosphate battery positive electrode material and its application. The nano-scale lithium iron phosphate battery positive electrode material prepared by this preparation method greatly improves the high-power charge and discharge performance of the lithium iron phosphate battery, and further improves the cycle performance.

[0006] The present invention is achieved through the following technical solutions:

[0007] In a first aspect, the present application provides a method for preparing a nanoscale lithium iron phosphate battery positive electrode material, comprising the following steps:

[0008] Dissolve acrylic acid (AA), 2-amino-4-chloro-6-methylpyrimidine (AM), and sulfathiazole (ST) in pure water, then add sodium hydroxide while stirring, remove oxygen in the container after cooling to room temperature, then add an initiator and a cross-linking agent in sequence to polymerize, and after the reaction is complete, dry and crush the gel to obtain a water-absorbent resin powder;

[0009] A lithium source, a carbon source, an iron source and a phosphorus source are added to pure water, and a slurry is obtained after dispersion. The slurry is ground to obtain a precursor slurry, and then a water-absorbent resin powder is added to the precursor slurry and stirred to mix well. The slurry is aged and water-absorbed in a constant temperature space. After the water absorption is completed and the colloid is stabilized, the sintering is performed. The sintered product is crushed by air flow to obtain a nano-scale lithium iron phosphate battery positive electrode material.

[0010] After the gel is dried and crushed, it can be sieved using a sieve with a mesh size of 150.

[0011] When preparing the water-absorbent resin powder, the reaction temperature for the polymerization reaction by adding an initiator and a cross-linking agent is 60°C.

[0012] The grinding process may be performed using a grinder with an operating time of 0.5 to 3 hours and an operating speed of 200 rpm to 1500 rpm until the specified particle size D50 is 0.2 μm to 1.3 μm.

[0013] The aging and water absorption time is 8 hours, the temperature in the constant temperature space is 10° C. to 40° C., and the humidity is 50% to 80%.

[0014] The sintering temperature is 650° C. to 850° C., and the sintering time is 5 h to 9 h.

[0015] The sintered product is crushed to a finished product particle size D50 of 0.5 μm to 2.5 μm.

[0016] The water-absorbent resin powder prepared in the present invention is a macromolecule containing a hydrophilic group and a cross-linked structure, which can quickly absorb water hundreds of times larger than its own weight to form a gel. The water absorption capacity, water retention capacity and water absorption speed of this gel are all very high, and it is resistant to high temperatures. The present invention adds high-temperature resistant water-absorbent resin powder to the ground precursor slurry, and after aging and stabilization for a period of time, the uniformly dispersed lithium iron phosphate precursor is placed in a sagger for high-temperature sintering. The lithium iron phosphate precursor is stably dispersed in the gel. During the sintering process, the gap size of the granules can be adjusted by adjusting the amount of pure water added. The water-absorbent resin will release heat and release water after being heated at high temperature. As the temperature continues to rise, the water-absorbent resin will crack and evenly coat the outside of the lithium iron phosphate, thereby enhancing the conductive properties of the material.

[0017] The solid obtained by sintering the nano-scale lithium iron phosphate battery positive electrode material prepared by the preparation method of the present invention is crushed by air flow, and the primary grain size of the lithium iron phosphate is partially less than 50nm, and most of the primary grains are less than 100nm, which has excellent charge and discharge performance as a positive electrode material of the battery. In addition, the nano-scale lithium iron phosphate particles will destroy the periodic boundary conditions of the material, and the magnetism, internal pressure, light absorption, thermal resistance, chemical activity, catalytic properties and melting point are greatly changed compared with ordinary particles. The nano-scale lithium iron phosphate prepared by the preparation method of the present invention has super strong chemical activity, which greatly improves the high-power charge and discharge performance of the lithium iron phosphate battery. Compared with the battery made of lithium iron phosphate commonly used in the market, the battery prepared by the lithium iron phosphate prepared by the method of the present invention has a 5C current discharge performance of 30mAh / g to 50mAh / g, and further improves the cycle performance.

[0018] Furthermore, when preparing the water-absorbent resin powder, the mass of 2-amino-4-chloro-6-methylpyrimidine accounts for 15% to 25% of the mass of acrylic acid, the mass of sulfathiazole accounts for 5% to 10% of the mass of acrylic acid, and the mass of pure water is 300% of the total mass of acrylic acid, 2-amino-4-chloro-6-methylpyrimidine and sulfathiazole.

[0019] Furthermore, when preparing the water-absorbent resin powder, the mass of the added sodium hydroxide is 35% to 45% of the mass of the acrylic acid, wherein the stirring speed after adding the sodium hydroxide is 100 rpm to 200 rpm.

[0020] Furthermore, when preparing the water-absorbent resin powder, the initiator used includes potassium persulfate (KPS) or ammonium persulfate (APS).

[0021] Furthermore, when preparing the water-absorbent resin powder, the crosslinking agent used includes any one of tetraallyl ammonium chloride (TAAC), tetraallyl ammonium bromide (TAAB), 2-mercaptobenzoic acid (MBA), epichlorohydrin (ECH), divinyl sulfone (DVS), and citric acid (CA).

[0022] Furthermore, the iron source and the phosphorus source are both ferric phosphate, and the molar ratio of the iron element to the phosphorus element in the ferric phosphate is (0.93-0.99):1.

[0023] The mass ratio of the amount of pure water added to the amount of iron phosphate is (2.5-3):1.

[0024] Furthermore, the lithium source includes any one or more combinations of lithium carbonate, lithium nitrate, lithium hydroxide, and lithium acetate, and the molar ratio of lithium ions to the sum of the iron source and the phosphorus source is (1.001-1.07):1.

[0025] The added lithium source provides lithium atoms for the prepared lithium iron phosphate battery positive electrode material.

[0026] Furthermore, the carbon source includes any one or more combinations of sucrose, glucose, starch, polyethylene glycol, graphite, and carbon nanotubes, and the mass ratio of the carbon source to the sum of the iron source and the phosphorus source is (0.03-0.3):1.

[0027] The added carbon source provides carbon elements for the prepared lithium iron phosphate battery positive electrode material. After adding the carbon source and sintering, a uniform carbon layer will be formed on the outer layer of the lithium iron phosphate material, increasing the conductivity of the lithium iron phosphate material. At the same time, the coated carbon will limit the growth of lithium iron phosphate during the sintering process, and smaller particles will also enhance the conductivity of the material.

[0028] Furthermore, the mass ratio of the added amount of the water-absorbent resin powder to the total amount of the iron source and the phosphorus source is (0.1-0.2):1.

[0029] In a second aspect, the present application provides an application of a nanoscale lithium iron phosphate battery positive electrode material prepared using any one of the above-mentioned preparation methods, including use in preparing a lithium iron phosphate battery.

[0030] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0031] (1) The solid of the nano-scale lithium iron phosphate battery positive electrode material prepared by the preparation method of the present invention is sintered and crushed by air flow to obtain lithium iron phosphate particles with significantly reduced particle size. The nano-sized lithium iron phosphate has excellent charge and discharge performance as a battery positive electrode material;

[0032] (2) The present invention adds high temperature resistant water-absorbent resin powder to the ground precursor slurry, and after aging and stabilization for a period of time, the uniformly dispersed lithium iron phosphate precursor is placed in a sagger for high temperature sintering. The lithium iron phosphate precursor is stably dispersed in the gel, and the gap size of the granules can be adjusted by adjusting the solid content during the sintering process. The water-absorbent resin releases heat and releases water after being heated at high temperature. As the temperature continues to rise, the water-absorbent resin will crack and evenly coat the outside of the lithium iron phosphate, thereby enhancing the conductive properties of the material;

[0033] (3) The nano-scale lithium iron phosphate prepared by the preparation method of the present invention has super strong chemical activity, which greatly improves the high-power charge and discharge performance of the lithium iron phosphate battery. Compared with the batteries made of lithium iron phosphate commonly found in the market, the 1C current discharge performance of the battery prepared by the lithium iron phosphate prepared by the method of the present invention is improved by 30mAh / g to 50mAh / g, and the cycle performance is further improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions of the exemplary embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present invention and should not be regarded as limiting the scope. For those of ordinary skill in the art, other relevant drawings can be obtained based on these drawings without creative work. In the drawings:

[0035] Figure 1 The process flow chart of preparing water-absorbing resin powder of the present invention;

[0036] Figure 2 This is a process flow chart for preparing nano-scale lithium iron phosphate battery positive electrode materials according to the present invention;

[0037] Figure 3 This is a particle size distribution diagram of the nano-scale lithium iron phosphate battery positive electrode material prepared in Example 1 of the present invention;

[0038] Figure 4 This is a particle size distribution diagram of the nanoscale lithium iron phosphate battery positive electrode material prepared in Example 2 of the present invention;

[0039] Figure 5 This is a particle size distribution diagram of the nanoscale lithium iron phosphate battery positive electrode material prepared in Example 3 of the present invention;

[0040] Figure 6 This is a particle size distribution diagram of the nanoscale lithium iron phosphate battery positive electrode material prepared in Example 4 of the present invention;

[0041] Figure 7 This is a particle size distribution diagram of the nanoscale lithium iron phosphate battery positive electrode material prepared in Example 5 of the present invention;

[0042] Figure 8 This is a particle size distribution diagram of the nanoscale lithium iron phosphate battery positive electrode material prepared in Example 6 of the present invention;

[0043] Fig. 9 This is a particle size distribution diagram of the nanoscale lithium iron phosphate battery positive electrode material prepared in Example 7 of the present invention;

[0044] Fig.10This is a particle size distribution diagram of the positive electrode material of the lithium iron phosphate battery prepared in Comparative Example 1;

[0045] Fig.11 This is a scanning electron microscope image of the nanoscale lithium iron phosphate battery positive electrode material prepared in Example 1 of the present invention;

[0046] Fig.12 This is a scanning electron microscope image of the nanoscale lithium iron phosphate battery positive electrode material prepared in Example 2 of the present invention;

[0047] Fig.13 This is a scanning electron microscope image of the nanoscale lithium iron phosphate battery positive electrode material prepared in Example 3 of the present invention;

[0048] Fig.14 This is a scanning electron microscope image of the nanoscale lithium iron phosphate battery positive electrode material prepared in Example 4 of the present invention;

[0049] Fig.15 This is a scanning electron microscope image of the nanoscale lithium iron phosphate battery positive electrode material prepared in Example 5 of the present invention;

[0050] Fig.16 This is a scanning electron microscope image of the nanoscale lithium iron phosphate battery positive electrode material prepared in Example 6 of the present invention;

[0051] Fig.17 This is a scanning electron microscope image of the nanoscale lithium iron phosphate battery positive electrode material prepared in Example 7 of the present invention;

[0052] Fig.18 This is a scanning electron microscope image of the positive electrode material of the lithium iron phosphate battery prepared in Comparative Example 1 of the present invention;

[0053] Fig.19 This is a rate performance diagram of the lithium iron phosphate battery positive electrode material prepared in Examples 1 to 7 and Comparative Example. DETAILED DESCRIPTION

[0054] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.

[0055] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0056] In addition, the iron content of the anhydrous ferric phosphate used in the following examples is 36.4% by mass, and the purity of lithium carbonate is 99.7%.

[0057] Example 1

[0058] This embodiment provides a method for preparing a nano-scale lithium iron phosphate battery positive electrode material. Figure 1 The process flow chart of preparing water-absorbent resin is shown in FIG. Figure 2 The process flow chart of preparing lithium iron phosphate using the prepared water-absorbent resin is shown. The specific preparation method is:

[0059] S1. Weigh 100 g of acrylic acid (AA), 15 g of 2-amino-4-chloro-6-methylpyrimidine (AM), and 5 g of sulfathiazole (ST), and add them into a pure water container with a stirring device. The pure water container is filled with 360 g of pure water.

[0060] S2. Start stirring, add 40 g of sodium hydroxide into the pure water container, and then continue stirring for 30 minutes under a nitrogen environment.

[0061] S3, add 0.1g potassium persulfate (KPS) and 0.1g ammonium persulfate (TAAC) into a pure water container, continue stirring and reacting for 4 hours, and after completion, dry and crush, and sieve to obtain a water-absorbing resin powder for use.

[0062] S4. Add lithium carbonate, anhydrous ferric phosphate, glucose, sucrose and pure water into a stirring container, wherein the mass of anhydrous ferric phosphate is 100 g, lithium carbonate is 24.2 g, glucose is 15 g, sucrose is 5 g, and pure water is 300 g. Stir and disperse for 1 hour. The molar ratio of iron to phosphorus in anhydrous ferric phosphate is 0.93:1; the molar ratio of lithium ions to iron phosphate is 1.002:1; the molar ratio of the total mass of glucose to iron phosphate is 0.15:1; the molar ratio of the total mass of sucrose to iron phosphate is 0.05:1; and the ratio of the mass of pure water to iron phosphate is 3:1.

[0063] S5. Add 100 g of the dispersed slurry into a grinder for grinding until the particle size D50 is 0.2 μm to obtain a precursor slurry.

[0064] S6. Add the water-absorbent resin powder prepared in step S3 to the precursor slurry, wherein the amount of the water-absorbent resin powder added is 15 g, and allow to stand for aging for 8 hours at an ambient temperature of 25° C. and an ambient humidity of 60%.

[0065] S7. Put the aged material into a graphite sagger and sinter it in a box furnace with an inert gas atmosphere. The temperature is raised to 300°C at a heating rate of 3°C / min, and then raised to 700°C at a heating rate of 1°C / min. The oxygen content in the nitrogen atmosphere furnace is 65ppm. Keep warm for 8.5 hours, and then perform air flow crushing on the sintered material to obtain nano-scale lithium iron phosphate battery positive electrode material. The particle size D50 of the crushed material is 0.67μm.

[0066] The performance of the lithium iron phosphate battery positive electrode material prepared by the method of this embodiment was tested.

[0067] like Figure 3 Shown is the particle size distribution diagram of the lithium iron phosphate battery positive electrode material prepared in this embodiment.

[0068] As shown in the figure, the overall particle size of the agglomerated lithium iron phosphate particles that have been sintered and crushed is significantly reduced, and is closer to a normal distribution. The uniformity is higher than that of the control group, which can improve the electrical performance of the battery.

[0069] like Fig.11 Shown is a scanning electron microscope image of the lithium iron phosphate battery positive electrode material prepared in this embodiment.

[0070] As shown in the figure, the primary particles of lithium iron phosphate prepared by this method are significantly smaller than those of the control group. The primary size of the lithium iron phosphate particles is successfully regulated, shortening the on-off time of lithium ion transmission, thereby achieving the ability to enhance the battery rate performance.

[0071] Example 2

[0072] This embodiment provides a method for preparing a nano-scale lithium iron phosphate battery positive electrode material. Figure 1 The process flow chart of preparing water-absorbent resin is shown in FIG. Figure 2 The process flow chart of preparing lithium iron phosphate using the prepared water-absorbing resin is shown. Different from Example 1, the amount of 2-amino-4-chloro-6-methylpyrimidine (AM) used in this example is 17.5 g, and the amount of sulfathiazole (ST) used is 7.5 g. The specific preparation method is:

[0073] S1. Weigh 100 g of acrylic acid (AA), 17.5 g of 2-amino-4-chloro-6-methylpyrimidine (AM), and 7.5 g of sulfathiazole (ST), and add them into a pure water container with a stirring device. The pure water container is filled with 375 g of pure water.

[0074] S2. Start stirring, add 40 g of sodium hydroxide into the pure water container, and then continue stirring for 30 minutes under a nitrogen environment.

[0075] S3, add 0.1g potassium persulfate (KPS) and 0.1g ammonium persulfate (TAAC) into a pure water container, continue stirring and reacting for 4 hours, and after completion, dry and crush, and sieve to obtain a water-absorbing resin powder for use.

[0076] S4. Add lithium carbonate, anhydrous ferric phosphate, glucose, sucrose and pure water into a stirring container and stir and disperse for 1 hour. The mass of anhydrous ferric phosphate is 100g, lithium carbonate is 24.27g, glucose is 10g, sucrose is 5g, and pure water is 300g. The molar ratio of iron to phosphorus in anhydrous ferric phosphate is 0.93:1; the molar ratio of lithium ion to iron phosphate is 1.005:1; the molar ratio of the total mass of glucose to iron phosphate is 0.1:1; the molar ratio of the total mass of sucrose to iron phosphate is 0.05:1; and the ratio of the mass of pure water to iron phosphate is 3:1.

[0077] S5. Add 100 g of the dispersed slurry into a grinder for grinding until the particle size D50 is 0.2 μm to obtain a precursor slurry.

[0078] S6. Add the water-absorbent resin powder prepared in step S3 to the precursor slurry, wherein the amount of the water-absorbent resin powder added is 15 g, and allow to stand for aging for 8 hours at an ambient temperature of 25° C. and an ambient humidity of 60%.

[0079] S7. Put the aged material into a graphite crucible and sinter it in a box furnace with an inert gas atmosphere. The temperature is raised to 300°C at a heating rate of 3°C / min, and then raised to 700°C at a heating rate of 1°C / min. The oxygen content in the nitrogen atmosphere furnace is 65ppm. Keep warm for 8.5 hours, and then perform air flow crushing on the sintered material to obtain nano-scale lithium iron phosphate battery positive electrode material. The particle size D50 of the crushed material is 0.78μm.

[0080] like Figure 4 Shown is the particle size distribution diagram of the lithium iron phosphate battery positive electrode material prepared in this embodiment.

[0081] As shown in the figure, the overall particle size of the agglomerated lithium iron phosphate particles that have been sintered and crushed is significantly reduced, and is closer to a normal distribution. The uniformity is higher than that of the control group, which can improve the electrical performance of the battery.

[0082] like Fig.12 Shown is a scanning electron microscope image of the lithium iron phosphate battery positive electrode material prepared in this embodiment.

[0083] As shown in the figure, the primary particles of lithium iron phosphate prepared by this method are significantly smaller than those of the control group. The primary size of the lithium iron phosphate particles is successfully regulated, shortening the on-off time of lithium ion transmission, thereby achieving the ability to enhance the battery rate performance.

[0084] Example 3

[0085] This embodiment provides a method for preparing a nano-scale lithium iron phosphate battery positive electrode material. Figure 1 The process flow chart of preparing water-absorbent resin is shown in FIG. Figure 2 The process flow chart of preparing lithium iron phosphate using the prepared water-absorbent resin is shown. Different from Example 1, the molar ratio of iron to phosphorus in the anhydrous iron phosphate used in this example is 0.97:1, and the molar ratio of lithium ions to iron phosphate is also different. The specific preparation method is:

[0086] S1. Weigh 100 g of acrylic acid (AA), 15 g of 2-amino-4-chloro-6-methylpyrimidine (AM), and 5 g of sulfathiazole (ST), and add them into a pure water container with a stirring device. The pure water container is filled with 360 g of pure water.

[0087] S2. Start stirring, add 40 g of sodium hydroxide into the pure water container, and then continue stirring for 30 minutes under a nitrogen environment.

[0088] S3, add 0.1g potassium persulfate (KPS) and 0.1g ammonium persulfate (TAAC) into a pure water container, continue stirring and reacting for 4 hours, and after completion, dry and crush, and sieve to obtain a water-absorbing resin powder for use.

[0089] S4, add lithium carbonate, anhydrous iron phosphate, glucose, sucrose, carbon nanotubes, and pure water to a stirring container, and stir and disperse for 1 hour, wherein the mass of anhydrous iron phosphate is 100g, lithium carbonate is 24.39g, glucose is 2g, sucrose is 5g, carbon nanotubes are 0.5g, and pure water is 300g. The molar ratio of iron to phosphorus in anhydrous iron phosphate is 0.97:1; the molar ratio of lithium ions to iron phosphate is 1.01:1; the molar ratio of the total mass of glucose to iron phosphate is 0.02:1; the molar ratio of the total mass of sucrose to iron phosphate is 0.05:1; the ratio of the mass of pure water to iron phosphate is 3:1.

[0090] S5. Add 100 g of the dispersed slurry into a grinder for grinding until the particle size D50 is 0.2 μm to obtain a precursor slurry.

[0091] S6. Add the water-absorbent resin powder prepared in step S3 to the precursor slurry, wherein the amount of the water-absorbent resin powder added is 15 g, and allow to stand for aging for 8 hours at an ambient temperature of 25° C. and an ambient humidity of 60%.

[0092] S7. Put the aged material into a graphite sagger and sinter it in a box furnace with an inert gas atmosphere. The temperature is raised to 300°C at a heating rate of 3°C / min, and then raised to 700°C at a heating rate of 1°C / min. The oxygen content in the nitrogen atmosphere furnace is 65ppm. Keep warm for 8.5 hours, and then perform air flow crushing on the sintered material to obtain nano-scale lithium iron phosphate battery positive electrode material. The particle size D50 of the crushed material is 0.75μm.

[0093] like Figure 5 Shown is the particle size distribution diagram of the lithium iron phosphate battery positive electrode material prepared in this embodiment.

[0094] As shown in the figure, the overall particle size of the agglomerated lithium iron phosphate particles that have been sintered and crushed is significantly reduced, and is closer to a normal distribution. The uniformity is higher than that of the control group, which can improve the electrical performance of the battery.

[0095] like Fig.13 Shown is a scanning electron microscope image of the lithium iron phosphate battery positive electrode material prepared in this embodiment.

[0096] As shown in the figure, the primary particles of lithium iron phosphate prepared by this method are significantly smaller than those of the control group. The primary size of the lithium iron phosphate particles is successfully regulated, shortening the on-off time of lithium ion transmission, thereby achieving the ability to enhance the battery rate performance.

[0097] Example 4

[0098] This embodiment provides a method for preparing a nano-scale lithium iron phosphate battery positive electrode material. Figure 1 The process flow chart of preparing water-absorbent resin is shown in FIG. Figure 2 The process flow chart of preparing lithium iron phosphate using the prepared water-absorbing resin is shown. Different from Example 1, the amount of 2-amino-4-chloro-6-methylpyrimidine (AM) used in this example is 25g, and the amount of sulfathiazole (ST) used is 10g. The specific preparation method is:

[0099] S1. Weigh 100 g of acrylic acid (AA), 25 g of 2-amino-4-chloro-6-methylpyrimidine (AM), and 10 g of sulfathiazole (ST), and add them into a pure water container with a stirring device. The pure water container is filled with 405 g of pure water.

[0100] S2. Start stirring, add 40 g of sodium hydroxide into the pure water container, and then continue stirring for 30 minutes under a nitrogen environment.

[0101] S3, add 0.1g potassium persulfate (KPS) and 0.1g ammonium persulfate (TAAC) into a pure water container, continue stirring and reacting for 4 hours, and after completion, dry and crush, and sieve to obtain a water-absorbing resin powder for use.

[0102] S4. Add lithium carbonate, anhydrous ferric phosphate, glucose, sucrose and pure water to a stirring container and stir and disperse for 1 hour, wherein the mass of anhydrous ferric phosphate is 100g, lithium carbonate is 24.44g, glucose is 2g, sucrose is 5g and pure water is 300g. The molar ratio of iron to phosphorus in anhydrous ferric phosphate is 0.93:1; the molar ratio of lithium ion to ferric phosphate is 1.012:1; the molar ratio of the total mass of glucose to ferric phosphate is 0.02:1; the molar ratio of the total mass of sucrose to ferric phosphate is 0.05:1; the ratio of the mass of pure water to ferric phosphate is 3:1.

[0103] S5. Add 100 g of the dispersed slurry into a grinder for grinding until the particle size D50 is 0.2 μm to obtain a precursor slurry.

[0104] S6. Add the water-absorbent resin powder prepared in step S3 to the precursor slurry, wherein the amount of the water-absorbent resin powder added is 15 g, and allow to stand for aging for 8 hours at an ambient temperature of 25° C. and an ambient humidity of 60%.

[0105] S7. Put the aged material into a graphite sagger and sinter it in a box furnace with an inert gas atmosphere. The temperature is raised to 300°C at a heating rate of 3°C / min, and then raised to 685°C at a heating rate of 1°C / min. The oxygen content in the nitrogen atmosphere furnace is 65ppm. Keep warm for 8.5 hours, and then perform air flow crushing on the sintered material to obtain nano-scale lithium iron phosphate battery positive electrode material. The particle size D50 of the crushed material is 0.91μm.

[0106] like Figure 6 Shown is the particle size distribution diagram of the lithium iron phosphate battery positive electrode material prepared in this embodiment.

[0107] As shown in the figure, the overall particle size of the agglomerated lithium iron phosphate particles that have been sintered and crushed is significantly reduced, and is closer to a normal distribution. The uniformity is higher than that of the control group, which can improve the electrical performance of the battery.

[0108] like Fig.14 Shown is a scanning electron microscope image of the lithium iron phosphate battery positive electrode material prepared in this embodiment.

[0109] As shown in the figure, the primary particles of lithium iron phosphate prepared by this method are significantly smaller than those of the control group. The primary size of the lithium iron phosphate particles is successfully regulated, shortening the on-off time of lithium ion transmission, thereby achieving the ability to enhance the battery rate performance.

[0110] Example 5

[0111] This embodiment provides a method for preparing a nano-scale lithium iron phosphate battery positive electrode material. Figure 1 The process flow chart of preparing water-absorbent resin is shown in FIG. Figure 2 The process flow chart of preparing lithium iron phosphate using the prepared water-absorbent resin is shown. Different from Example 1, the molar ratio of iron to phosphorus in the anhydrous iron phosphate used in this example is 0.99:1, and the molar ratio of lithium ions to iron phosphate is also different. The specific preparation method is:

[0112] S1. Weigh 100 g of acrylic acid (AA), 15 g of 2-amino-4-chloro-6-methylpyrimidine (AM), and 5 g of sulfathiazole (ST), and add them into a pure water container with a stirring device. The pure water container is filled with 360 g of pure water.

[0113] S2. Start stirring, add 40 g of sodium hydroxide into the pure water container, and then continue stirring for 30 minutes under a nitrogen environment.

[0114] S3, add 0.1g potassium persulfate (KPS) and 0.1g ammonium persulfate (TAAC) into a pure water container, continue stirring and reacting for 4 hours, and after completion, dry and crush, and sieve to obtain a water-absorbing resin powder for use.

[0115] S4, lithium carbonate, anhydrous ferric phosphate, glucose, sucrose, and pure water are added to a stirring container, and stirred and dispersed for 1 hour, wherein the mass of anhydrous ferric phosphate is 100g, lithium carbonate is 24.35g, glucose is 4g, sucrose is 8g, graphite is 0.5g, and pure water is 300g. The molar ratio of iron to phosphorus in anhydrous ferric phosphate is 0.99:1; the molar ratio of lithium ion to ferric phosphate is 1.008:1; the molar ratio of the total mass of glucose to ferric phosphate is 0.04:1; the molar ratio of the total mass of sucrose to ferric phosphate is 0.08:1; the ratio of the mass of pure water to ferric phosphate is 3:1.

[0116] S5. Add 100 g of the dispersed slurry into a grinder for grinding until the particle size D50 is 0.2 μm to obtain a precursor slurry.

[0117] S6. Add the water-absorbent resin powder prepared in step S3 to the precursor slurry, wherein the amount of the water-absorbent resin powder added is 15 g, and allow to stand for aging for 8 hours at an ambient temperature of 25° C. and an ambient humidity of 60%.

[0118] S7. Put the aged material into a graphite sagger and sinter it in a box furnace with an inert gas atmosphere. The temperature is raised to 300°C at a heating rate of 3°C / min, and then raised to 702°C at a heating rate of 1°C / min. The oxygen content in the nitrogen atmosphere furnace is 65ppm. Keep warm for 8.5 hours, and then air flow crush the sintered material to obtain nano-scale lithium iron phosphate battery positive electrode material. The particle size D50 of the crushed material is 0.78μm.

[0119] like Figure 7Shown is the particle size distribution diagram of the lithium iron phosphate battery positive electrode material prepared in this embodiment.

[0120] As shown in the figure, the overall particle size of the agglomerated lithium iron phosphate particles that have been sintered and crushed is significantly reduced, and is closer to a normal distribution. The uniformity is higher than that of the control group, which can improve the electrical performance of the battery.

[0121] like Fig.15 Shown is a scanning electron microscope image of the lithium iron phosphate battery positive electrode material prepared in this embodiment.

[0122] As shown in the figure, the primary particles of lithium iron phosphate prepared by this method are significantly smaller than those of the control group. The primary size of the lithium iron phosphate particles is successfully regulated, shortening the on-off time of lithium ion transmission, thereby achieving the ability to enhance the battery rate performance.

[0123] Example 6

[0124] This embodiment provides a method for preparing a nano-scale lithium iron phosphate battery positive electrode material. Figure 1 The process flow chart of preparing water-absorbent resin is shown in FIG. Figure 2 The process flow chart of preparing lithium iron phosphate using the prepared water-absorbing resin is shown. Different from Example 1, the molar ratio of the total mass of glucose and sucrose used in this example to iron phosphate is 0.03:1. The specific preparation method is:

[0125] S1. Weigh 100 g of acrylic acid (AA), 15 g of 2-amino-4-chloro-6-methylpyrimidine (AM), and 5 g of sulfathiazole (ST), and add them into a pure water container with a stirring device. The pure water container is filled with 360 g of pure water.

[0126] S2. Start stirring, add 40 g of sodium hydroxide into the pure water container, and then continue stirring for 30 minutes under a nitrogen environment.

[0127] S3, add 0.1g potassium persulfate (KPS) and 0.1g ammonium persulfate (TAAC) into a pure water container, continue stirring and reacting for 4 hours, and after completion, dry and crush, and sieve to obtain a water-absorbing resin powder for use.

[0128] S4. Add lithium carbonate, anhydrous ferric phosphate, glucose, sucrose and pure water to a stirring container and stir and disperse for 1 hour, wherein the mass of anhydrous ferric phosphate is 100g, lithium carbonate is 24.51g, glucose is 2g, sucrose is 10g, graphite is 0.5g and pure water is 300g. The molar ratio of iron to phosphorus in anhydrous ferric phosphate is 0.93:1; the molar ratio of lithium ion to ferric phosphate is 1.015:1; the molar ratio of the total mass of glucose to ferric phosphate is 0.02:1; the molar ratio of the total mass of sucrose to ferric phosphate is 0.1:1; the ratio of the mass of pure water to ferric phosphate is 3:1.

[0129] S5. Add 100 g of the dispersed slurry into a grinder for grinding until the particle size D50 is 0.2 μm to obtain a precursor slurry.

[0130] S6. Add the water-absorbent resin powder prepared in step S3 to the precursor slurry, wherein the amount of the water-absorbent resin powder added is 15 g, and allow to stand for aging for 8 hours at an ambient temperature of 25° C. and an ambient humidity of 60%.

[0131] S7. Put the aged material into a graphite crucible and sinter it in a box furnace with an inert gas atmosphere. The temperature is raised to 300°C at a heating rate of 3°C / min, and then raised to 700°C at a heating rate of 1°C / min. The oxygen content in the nitrogen atmosphere furnace is 65ppm. Keep warm for 8.5 hours, and then perform air flow crushing on the sintered material to obtain nano-scale lithium iron phosphate battery positive electrode material. The particle size D50 of the crushed material is 0.92μm.

[0132] like Figure 8 Shown is the particle size distribution diagram of the lithium iron phosphate battery positive electrode material prepared in this embodiment.

[0133] As shown in the figure, the overall particle size of the agglomerated lithium iron phosphate particles that have been sintered and crushed is significantly reduced, and is closer to a normal distribution. The uniformity is higher than that of the control group, which can improve the electrical performance of the battery.

[0134] like Fig.16 Shown is a scanning electron microscope image of the lithium iron phosphate battery positive electrode material prepared in this embodiment.

[0135] As shown in the figure, the primary particles of lithium iron phosphate prepared by this method are significantly smaller than those of the control group. The primary size of the lithium iron phosphate particles is successfully regulated, shortening the on-off time of lithium ion transmission, thereby achieving the ability to enhance the battery rate performance.

[0136] Example 7

[0137] This embodiment provides a method for preparing a nano-scale lithium iron phosphate battery positive electrode material. Figure 1 The process flow chart of preparing water-absorbent resin is shown in FIG. Figure 2 The process flow chart of preparing lithium iron phosphate using the prepared water-absorbing resin is shown. Different from Example 1, the molar ratio of the total mass of glucose and sucrose used in this example to iron phosphate is 0.2:1. The specific preparation method is:

[0138] S1. Weigh 100 g of acrylic acid (AA), 15 g of 2-amino-4-chloro-6-methylpyrimidine (AM), and 5 g of sulfathiazole (ST), and add them into a pure water container with a stirring device. The pure water container is filled with 360 g of pure water.

[0139] S2. Start stirring, add 40 g of sodium hydroxide into the pure water container, and then continue stirring for 30 minutes under a nitrogen environment.

[0140] S3, add 0.1g potassium persulfate (KPS) and 0.1g ammonium persulfate (TAAC) into a pure water container, continue stirring and reacting for 4 hours, and after completion, dry and crush, and sieve to obtain a water-absorbing resin powder for use.

[0141] S4. Add lithium carbonate, anhydrous ferric phosphate, glucose, sucrose, and pure water to a stirring container and stir and disperse for 1 hour, wherein the mass of anhydrous ferric phosphate is 100g, lithium carbonate is 24.39g, glucose is 10g, sucrose is 10g, and pure water is 300g. The molar ratio of iron to phosphorus in anhydrous ferric phosphate is 0.93:1; the molar ratio of lithium ion to ferric phosphate is 1.011:1; the molar ratio of the total mass of glucose to ferric phosphate is 0.1:1; the molar ratio of the total mass of sucrose to ferric phosphate is 0.1:1; the ratio of the mass of pure water to ferric phosphate is 3:1.

[0142] S5. Add 100 g of the dispersed slurry into a grinder for grinding until the particle size D50 is 0.2 μm to obtain a precursor slurry.

[0143] S6. Add the water-absorbent resin powder prepared in step S3 to the precursor slurry, wherein the amount of the water-absorbent resin powder added is 15 g, and allow to stand for aging for 8 hours at an ambient temperature of 25° C. and an ambient humidity of 60%.

[0144] S7. Put the aged material into a graphite crucible and sinter it in a box furnace with an inert gas atmosphere. The temperature is raised to 300°C at a heating rate of 3°C / min, and then raised to 705°C at a heating rate of 1°C / min. The oxygen content in the nitrogen atmosphere furnace is 65ppm. The temperature is kept warm for 8.5 hours. The sintered material is then air flow crushed to obtain a nano-scale lithium iron phosphate battery positive electrode material. The particle size D50 of the crushed material is 0.88μm.

[0145] like Fig. 9 Shown is the particle size distribution diagram of the lithium iron phosphate battery positive electrode material prepared in this embodiment.

[0146] As shown in the figure, the overall particle size of the agglomerated lithium iron phosphate particles that have been sintered and crushed is significantly reduced, and is closer to a normal distribution. The uniformity is higher than that of the control group, which can improve the electrical performance of the battery.

[0147] like Fig.17 Shown is a scanning electron microscope image of the lithium iron phosphate battery positive electrode material prepared in this embodiment.

[0148] As shown in the figure, the primary particles of lithium iron phosphate prepared by this method are significantly smaller than those of the control group. The primary size of the lithium iron phosphate particles is successfully regulated, shortening the on-off time of lithium ion transmission, thereby achieving the ability to enhance the battery rate performance.

[0149] Comparative Example

[0150] S1. Add lithium carbonate, anhydrous ferric phosphate, glucose, sucrose and pure water to a stirring container and stir and disperse for 1 hour, wherein the mass of anhydrous ferric phosphate is 100g, lithium carbonate is 24.39g, glucose is 5g, sucrose is 10g and pure water is 300g. The molar ratio of iron to phosphorus in anhydrous ferric phosphate is 0.93:1; the molar ratio of lithium ion to ferric phosphate is 1.01:1; the molar ratio of the total mass of glucose to ferric phosphate is 0.05:1; the molar ratio of the total mass of sucrose to ferric phosphate is 0.1:1; the ratio of the mass of pure water to ferric phosphate is 3:1.

[0151] S2. Add 100 g of the dispersed slurry into a grinder and grind until the particle size D50 is 0.5 μm to obtain a precursor slurry.

[0152] S3. Dry the precursor slurry into powder by spray drying.

[0153] S4. The dried precursor is placed in a graphite crucible and sintered in a box furnace with an inert gas atmosphere. The temperature is raised to 300°C at a heating rate of 3°C / min, and then raised to 700°C at a heating rate of 1°C / min. The oxygen content in the nitrogen atmosphere furnace is 65ppm. The temperature is kept warm for 8.5 hours, and then the sintered material is air flow crushed to obtain a nano-scale lithium iron phosphate battery positive electrode material. The particle size D50 of the crushed material is 1.3μm.

[0154] like Fig.10 Shown is the particle size distribution diagram of the lithium iron phosphate battery positive electrode material prepared in this embodiment.

[0155] Lithium iron phosphate prepared by spray drying and then crushing tends to agglomerate to form agglomerates of several microns.

[0156] like Fig.18 Shown is a scanning electron microscope image of the lithium iron phosphate battery positive electrode material prepared in this embodiment.

[0157] The primary particles of lithium iron phosphate formed are large in size and severely agglomerated, which is not conducive to the electrical properties of lithium iron phosphate.

[0158] Button batteries were prepared using the lithium iron phosphate prepared in Examples 1 to 7 and the comparative example, and their electrochemical properties were tested.

[0159] The production process of the electrode sheet is as follows:

[0160] The raw materials were evenly ground in a mass ratio of m(LiFePO4):m(conductive carbon black):m(PVDF)=8:1:1, mixed and stirred in a certain amount of N-methylpyrrolidone (NMP) solvent to form a uniform paste slurry, evenly coated on aluminum foil, dried in a vacuum drying oven at 80°C overnight, and compacted and sliced ​​to obtain a positive electrode sheet.

[0161] Battery assembly:

[0162] The assembly of the laboratory half-cell needs to be carried out in a glove box that is isolated from the air and filled with Ar gas to prevent the electrolyte from absorbing moisture and deteriorating and the negative electrode material lithium sheet from reacting with water and oxygen in the air. Subsequent electrochemical tests are carried out in the air, so the sealing of the battery is required to be high. The pressure of the tablet press is adjusted to 50MPa to seal the upper and lower shells of the battery tightly. The electrode sheet prepared by stamping is used as the positive electrode, the lithium sheet is used as the negative electrode, the electrolyte is 1M LiPF6 (EC+DEC, volume ratio is 1:1), and the diaphragm is selected as Celgard2400. The CR2016 button cell is assembled in the glove box. After assembly, the battery is aged overnight for 12 hours for testing.

[0163] Battery charge and discharge performance test:

[0164] The battery charge and discharge performance test is an important means to detect the quality of electrode materials and whether the battery assembly process is scientific and reasonable. The battery charge and discharge performance test mainly includes: constant current charge and discharge test, cycle charge and discharge test and rate performance test. Constant current charge and discharge is to charge and discharge the assembled battery at a constant current density, and the charge and discharge voltage range is 2.0~4.2V. The specific charge and discharge procedure is: (1) stand for 1 minute; (2) constant current charge to a cut-off voltage of 3.8V; (3) charge at a constant voltage of 3.8V until the current is lower than a certain value; (4) continue to stand for 1 minute; (5) constant current discharge to a cut-off voltage of 2.0V, the cycle ends, and enters the next cycle. The size of the charge and discharge current is calculated based on the test rate, 1C=170mA. The cycle charge and discharge attenuation spectrum is drawn by constant current charge and discharge and cycle charge and discharge data, and the specific capacity, cycle life and other electrochemical properties of the electrode material can be accurately known. The rate performance test is to use different current densities to charge and discharge the battery to test the stability of the electrode material structure under different current density charging and discharging conditions and the deintercalation of the material at different rates. + The present invention uses the buckle 3000-1 battery testing system produced by Wuhan Landian Testing Equipment Co., Ltd. to measure the charge and discharge specific capacity, cycle performance, coulomb efficiency, rate performance, etc. of the electrode material.

[0165] The rate performance test results of Examples 1 to 7 of the present application and the comparative example are as follows Fig.19The discharge performance is shown in Table 1. It can be seen that the lithium iron phosphate prepared by the present invention has significantly improved several test results of the first discharge electrical performance compared with the control example, among which the 0.1C first discharge is increased by about 11mAh / g, the first charge and discharge efficiency is increased by about 2%, 1C is increased by 23mAh / g compared with the control example, and 5C is increased by about 40mAh / g. In summary, the invention significantly improves the electrical performance of lithium iron phosphate prepared by combining innovative regulation and coating.

[0166] Table 1

[0167]

[0168] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a nanoscale lithium iron phosphate battery positive electrode material, characterized in that: The following steps are involved: Dissolve acrylic acid, 2-amino-4-chloro-6-methylpyrimidine and sulfathiazole in pure water, then add sodium hydroxide while stirring, remove oxygen in the container after cooling to room temperature, then add initiator and cross-linking agent in sequence to polymerize, and after the reaction is complete, dry and crush the gel to obtain water-absorbent resin powder; A lithium source, a carbon source, an iron source and a phosphorus source are added to pure water, and a slurry is obtained after dispersion. The slurry is ground to obtain a precursor slurry, and then a water-absorbent resin powder is added to the precursor slurry and stirred to mix well. The slurry is aged and water-absorbed in a constant temperature space. After the water absorption is completed and the colloid is stabilized, the sintering is performed. The sintered product is crushed by air flow to obtain a nano-scale lithium iron phosphate battery positive electrode material.

2. The method for preparing a nano-scale lithium iron phosphate battery positive electrode material according to claim 1, characterized in that: When preparing the water-absorbent resin powder, the mass of 2-amino-4-chloro-6-methylpyrimidine accounts for 15% to 25% of acrylic acid, the mass of sulfathiazole accounts for 5% to 10% of acrylic acid, and the mass of pure water is 300% of the total mass of acrylic acid, 2-amino-4-chloro-6-methylpyrimidine and sulfathiazole.

3. The method for preparing a nano-scale lithium iron phosphate battery positive electrode material according to claim 1, characterized in that: When preparing the water-absorbent resin powder, the mass of the added sodium hydroxide is 35% to 45% of the mass of the acrylic acid.

4. The method for preparing a nano-scale lithium iron phosphate battery positive electrode material according to claim 1, characterized in that: When preparing the water-absorbent resin powder, the initiator used includes potassium persulfate or ammonium persulfate.

5. The method for preparing a nano-scale lithium iron phosphate battery positive electrode material according to claim 1, characterized in that: When preparing the water-absorbent resin powder, the crosslinking agent used includes any one of tetraallylammonium chloride, tetraallylammonium bromide, 2-mercaptobenzoic acid, epichlorohydrin, divinyl sulfone and citric acid.

6. The method for preparing a nano-scale lithium iron phosphate battery positive electrode material according to claim 1, characterized in that: The iron source and the phosphorus source are both ferric phosphate, and the molar ratio of the iron element to the phosphorus element in the ferric phosphate is (0.93-0.99):

1.

7. The method for preparing a nano-scale lithium iron phosphate battery positive electrode material according to claim 1, characterized in that: The lithium source includes any one or more combinations of lithium carbonate, lithium nitrate, lithium hydroxide, and lithium acetate, and the molar ratio of lithium ions to the sum of the iron source and the phosphorus source is (1.001-1.07):

1.

8. The method for preparing a nano-scale lithium iron phosphate battery positive electrode material according to claim 1, characterized in that: The carbon source includes any one or more combinations of sucrose, glucose, starch, polyethylene glycol, graphite, and carbon nanotubes, and the mass ratio of the carbon source to the sum of the iron source and the phosphorus source is (0.03-0.3):

1.

9. The method for preparing a nano-scale lithium iron phosphate battery positive electrode material according to claim 1, characterized in that: The mass ratio of the added amount of the water-absorbent resin powder to the total amount of the iron source and the phosphorus source is (0.1 to 0.2):

1.

10. An application of a nano-scale lithium iron phosphate battery positive electrode material prepared by the preparation method according to any one of claims 1 to 9, characterized in that: Including for the preparation of lithium iron phosphate batteries.

Citation Information

Patent Citations

  • Preparation method of hydrophilic sulfa drug molecularly imprinted solid-phase extraction column

    CN104001486A

  • Nano single crystal type lithium-rich manganese-based positive electrode material as well as preparation method and application thereof

    CN115411261A

  • Method for improving electrical property of lithium iron phosphate positive electrode material through coating

    CN118387850A

  • NANO single-crystal type lithium-rich manganese-based positive electrode material, and preparation method therefor and use thereof

    WO2024036695A1