Surface wrinkled biomass charcoal as well as preparation method and application thereof

Preparing surface wrinkled biomass carbon by flame spray gun heating method solves the problems of complex and high cost preparation of biomass-based carbon electrode materials in the existing technology, improves its electrochemical performance in supercapacitors, and achieves low-cost, high-efficiency electrode material applications.

CN118754105AActive Publication Date: 2024-10-11ENERGY RESOURCES INST HEBEI ACADEMY OF SCI
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411246108.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-10-11
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

The application of existing biomass-based carbon-based electrode materials in supercapacitors is limited by complex preparation processes, high costs and low energy density, making it difficult to be widely used.

Method used

The flame spray gun moving heating method is used to mix corn starch, metal chloride salt and KOH to form surface wrinkled biomass charcoal, which simplifies the preparation process and reduces costs. KOH and metal chloride salt are used to form molten salt to generate a rich wrinkle structure to improve the electricity consumption. chemical properties.

Benefits of technology

It achieves rapid and low-cost preparation of biomass carbon, improves its electrochemical performance in supercapacitors, especially its performance under high current density, and has high practical application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754105A_ABST
    Figure CN118754105A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of carbon materials, and provides surface wrinkled biomass charcoal and a preparation method and application thereof.The preparation method comprises the steps that corn starch, metal chlorine salt and KOH are mixed according to the mass ratio of 300-320: 3-10: 40-45, a flame spray gun is adopted for movable heating, and biomass charcoal is obtained after 5-10 min; the outer flame temperature of the flame spray gun is 700-1300 DEG C, and the moving speed of the flame spray gun is 0.5-2 cm / s. The biomass charcoal is excellent in electrochemical performance, and the preparation method is simple.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of carbon materials and relates to a surface wrinkled biomass charcoal and a preparation method and application thereof. Background Art

[0002] At present, carbon materials are widely used in adsorbents, catalysts, fuel cells, electrode materials for secondary batteries, supercapacitors, composite materials, gas sensors, solar cells, and various electronic devices due to their excellent porous properties.

[0003] Among them, supercapacitors have high power density and energy density, and are a new type of energy storage structure that combines the characteristics of traditional capacitors and batteries. Carbon materials have different properties due to their different functional elements, doping elements, pore volume and pore size. Biomass is an ideal precursor for carbon materials because of its wide source, renewable and low cost. In recent years, electrode materials based on biomass-based carbon have been studied more and more widely, but they cannot be well applied to capacitors, and the preparation process is complicated, the cost is relatively high, and the energy density is low, which restricts their large-scale application. Summary of the invention

[0004] The invention provides a biomass charcoal with wrinkled surface and a preparation method and application thereof. The biomass charcoal has excellent electrochemical performance and a simple and rapid preparation method.

[0005] The technical solution of the present invention is achieved in this way: Technical Theme 1 A method for preparing surface wrinkled biochar comprises: mixing corn starch, metal chloride and KOH in a mass ratio of 300-320:3-10:40-45, and heating by moving with a flame spray gun to obtain biochar after 5-10 minutes; the outer flame temperature of the flame spray gun is 700-1300°C, and the moving speed is 0.5-2cm / s; the metal chloride is KCl and / or NaCl.

[0006] Preferably, the outer flame temperature of the flame spray gun is 1000-1300° C., and the moving speed is 1-1.5 cm / s.

[0007] Preferably, the metal chloride salt is KCl.

[0008] Preferably, the mass ratio of the corn starch, KCl and KOH is 320:3:45.

[0009] Preferably, the mixing is performed by grinding in a mortar, and the grinding is followed by passing through a 100-300 mesh sieve.

[0010] Technical Theme 2 The present invention also provides biomass charcoal obtained by the preparation method of the biomass charcoal with wrinkled surface.

[0011] Technical Theme 3 The present invention also provides the use of the biochar obtained by the preparation method of the biochar with wrinkled surface in energy storage materials.

[0012] The present invention also provides the use of the biomass charcoal obtained by the preparation method of the biomass charcoal with wrinkled surface as a supercapacitor electrode material.

[0013] The working principle and beneficial effects of the present invention are: 1. The present invention provides a biochar with a wrinkled surface, a preparation method and an application thereof. The biochar has abundant wrinkles on the surface, and its preparation method has the advantages of low cost and simple steps. The biochar is used in supercapacitors as an electrode material and has a high practical application prospect.

[0014] 2. In the process of calcining the raw materials using a high-temperature spray gun, the KOH and metal chloride salt in the mixed raw materials will form a molten salt, isolating the raw materials from oxygen in the air, so no inert gas protection is required. It usually takes more than four or five hours to prepare carbon materials with inert gas, but the present invention only takes 5-10 minutes to prepare; In the present invention, KOH and metal chloride salt form a molten salt, so that the surface of the prepared biochar forms abundant wrinkles. Due to the presence of surface wrinkles, electrolyte ions are more likely to gather on the surface of the biochar, thereby improving the electrochemical performance of the biochar at high current density. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0016] Figure 1 is a SEM image of the biochar obtained in Example 1; Figure 2 is a SEM image of the biochar obtained in Example 3; Figure 3 This is the SEM image of the biochar obtained in Comparative Example 1; Figure 4 This is the SEM image of the biochar obtained in Comparative Example 2; Figure 5 This is the SEM image of the biochar obtained in Comparative Example 3. DETAILED DESCRIPTION

[0017] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. The combustion gas in the flame spray gun used in the following embodiments is butane.

[0018] Example 1 A method for preparing surface wrinkled biochar comprises: mixing 32g corn starch, 0.3g KCl and 4.5g KOH, grinding and mixing in a mortar, passing through a 200-mesh sieve after grinding, and heating by a flame spray gun to obtain biochar after 5 minutes, wherein the outer flame temperature of the flame spray gun is 1000°C and the moving speed is 1cm / s.

[0019] Example 2 A method for preparing surface wrinkled biochar comprises: mixing 30g corn starch, 1g KCl and 4g KOH, grinding and mixing in a mortar, passing through a 200-mesh sieve after grinding, and heating by a flame spray gun to obtain biochar after 6 minutes, wherein the outer flame temperature of the flame spray gun is 1000°C and the moving speed is 1.5cm / s.

[0020] Example 3 A method for preparing surface wrinkled biochar comprises: mixing 32g corn starch, 0.3g NaCl and 4.5g KOH, grinding and mixing in a mortar, passing through a 200-mesh sieve after grinding, and heating by a flame spray gun to obtain biochar after 5 minutes, wherein the outer flame temperature of the flame spray gun is 1000°C and the moving speed is 1cm / s.

[0021] Example 4 A method for preparing surface wrinkled biochar comprises: mixing 31g corn starch, 0.5g KCl and 4.2g KOH, grinding and mixing in a mortar, passing through a 100-mesh sieve after grinding, and heating by a flame spray gun to obtain biochar after 10 minutes, wherein the outer flame temperature of the flame spray gun is 700°C and the moving speed is 0.5cm / s.

[0022] Example 5 A method for preparing surface wrinkled biochar comprises: mixing 32g corn starch, 0.6g KCl and 4.3g KOH, grinding and mixing in a mortar, passing through a 300-mesh sieve after grinding, and heating by a flame spray gun to obtain biochar after 5 minutes, wherein the outer flame temperature of the flame spray gun is 1300°C and the moving speed is 2cm / s.

[0023] Example 6 A method for preparing surface wrinkled biochar comprises: mixing 30g corn starch, 1g NaCl and 4.0g KOH, grinding and mixing in a mortar, passing through a 100-mesh sieve after grinding, and heating by a flame spray gun to obtain biochar after 5 minutes, wherein the outer flame temperature of the flame spray gun is 1300°C and the moving speed is 2cm / s.

[0024] Example 7 A method for preparing surface wrinkled biochar comprises: mixing 31g corn starch, 0.5g NaCl and 4.2g KOH, grinding and mixing in a mortar, passing through a 300-mesh sieve after grinding, and heating by a flame spray gun to obtain biochar after 10 minutes, wherein the outer flame temperature of the flame spray gun is 700°C and the moving speed is 0.5cm / s.

[0025] Comparative Example 1 A method for preparing biochar, comprising: mixing 32g corn starch, 0.3g Na2CO3, and 4.5g KOH, grinding and mixing in a mortar, passing through a 200-mesh sieve after grinding, and heating by a flame spray gun to obtain biochar after 5 minutes, wherein the outer flame temperature of the flame spray gun is 1000°C and the moving speed is 1cm / s.

[0026] Comparative Example 2 A method for preparing biochar, comprising: mixing 32g corn starch, 0.3g K2CO3, and 4.5g KOH, grinding and mixing in a mortar, passing through a 200-mesh sieve after grinding, and heating by a flame spray gun to obtain biochar after 5 minutes, wherein the outer flame temperature of the flame spray gun is 1000°C and the moving speed is 1cm / s.

[0027] Comparative Example 3 A method for preparing biochar comprises: mixing 32g corn starch and 4.5g KOH, grinding and mixing in a mortar, passing through a 200-mesh sieve after grinding, and heating by a flame spray gun to obtain biochar after 5 minutes, wherein the outer flame temperature of the flame spray gun is 1000°C and the moving speed is 1cm / s.

[0028] Comparative Example 4 Compared with Example 1, the only difference is that the carbonization is carried out under an inert gas atmosphere. Specifically, 15 g of distilled water, 4.5 g of KOH and 0.3 g of KCl are mixed to form a solution; 32 g of corn starch is added to 4 times the mass of distilled water, stirred to form a starch suspension; the KOH / KCl solution is mixed with the starch suspension to obtain a hydrogel.

[0029] The hydrogel was freeze-dried to obtain aerogel, which was then carbonized at 800 °C for 3 h in a nitrogen atmosphere to obtain biochar.

[0030] The determination method of the biochar in the above examples and comparative examples is as follows: 1. Specific capacitance measurement Weigh a certain mass of biochar, add a polytetrafluoroethylene solution with a mass fraction of 5wt%, the mass ratio of biochar to polytetrafluoroethylene is 95:5, add a magnetic stirrer for 4 hours, dry it in an oven at 105℃, apply it on a circular nickel foam with a diameter of 1.0cm, and then dry it in a vacuum drying oven at 105℃ for 8h to obtain an electrode sheet. In a 6.0M potassium hydroxide solution, the counter electrode is a mercury / mercuric oxide electrode, the reference electrode is a platinum electrode, and the charge and discharge curve is tested in a three-electrode system. The test voltage range is -1.0V to 0V, and the material specific capacitance is calculated by the charge and discharge curve. The results are shown in Table 1.

[0031] Table 1

[0032] like Figure 1 , is a SEM image of the biochar obtained in Example 1; Figure 2 is a SEM image of the biochar obtained in Example 3; Figure 3 This is the SEM image of the biochar obtained in Comparative Example 1; Figure 4 This is the SEM image of the biochar obtained in Comparative Example 2; Figure 5 This is the SEM image of the biochar obtained in Comparative Example 3. Figure 1-5 It can be seen that during the carbonization process of the present invention, KOH and metal chloride salts form molten salts, so that abundant wrinkles are formed on the surface of the prepared biochar. The presence of the wrinkled structure enables the biochar to have good electrochemical properties under high current density, especially the biochar prepared by KCl / KOH, which has obvious wrinkled structure and better electrochemical performance under high current density; while the biochar obtained by using Na2CO3 or K2CO3 has poor electrochemical performance under both low current and high current density. Comparative Example 4 uses inert atmosphere carbonization, and the electrochemical performance is basically equivalent to that of the biochar obtained in Example 1, and the preparation time of the biochar in Example 1 is much shorter than that of Comparative Example 4.

[0033] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing biochar with wrinkled surface, It is characterized in that include: Corn starch, metal chloride and KOH in a mass ratio of 300-320:3-10:40-45 are mixed, and heated by a flame spray gun to obtain biochar after 5-10 minutes; the outer flame temperature of the flame spray gun is 700-1300°C, and the moving speed is 0.5-2cm / s; the metal chloride is KCl and / or NaCl.

2. A method for preparing a surface wrinkled biochar according to claim 1, It is characterized in that The outer flame temperature of the flame spray gun is 1000-1300° C., and the moving speed is 1-1.5 cm / s.

3. The method for preparing a surface wrinkled biochar according to claim 1, It is characterized in that The metal chloride salt is KCl.

4. The method for preparing a biochar with wrinkled surface according to claim 3, It is characterized in that The mass ratio of the corn starch, KCl and KOH is 320:3:

45.

5. The method for preparing a biochar with wrinkled surface according to claim 1, It is characterized in that The mixture is ground and mixed in a mortar, and then passed through a 100-300 mesh sieve after grinding.

6. A biochar obtained by the method for preparing the surface wrinkled biochar according to any one of claims 1 to 5.

7. Use of the biochar as claimed in claim 6 in energy storage materials.

8. Use of the biochar as claimed in claim 6 as a supercapacitor electrode material.

Citation Information

Patent Citations

  • Method for producing biomass charcoal and device for producing biomass charcoal to be used therefor

    CN102388119A

  • Method for quickly preparing activated carbon

    CN106744951A

  • Method for preparing biomass-based porous carbon material from fuse salt

    CN108622895A

  • KOH activated magnetic rice husk biomass charcoal as well as preparation method and application thereof

    CN117138754A

  • Activated carbon with ultra-high specific surface area from corn and production method of thereof

    KR1020080085605A