A method for preparing heterogeneous element doped carbon material
By introducing heterogeneous element-doped porous carbon materials into lithium-ion batteries, the problems of structural failure of silicon-based anode materials and insufficient diffusion capacity of lithium ion in lithium-ion batteries are solved, and the structural stability and rate performance of the material are achieved. Improved, suitable for the industrial production of lithium-ion batteries.
Patent Information
- Application Number
- CN202411237235.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-05
AI Technical Summary
The structural failure of the silicon-based anode material in lithium-ion batteries and the low diffusion coefficient of lithium ion during the embedded/deliquefaction process leads to insufficient cyclic stability and rate performance, making it difficult to achieve large-scale application.
By introducing heterogeneous element doping into the porous carbon material, the strength of the carbon framework structure and lithium ion diffusion capacity are enhanced, and combined with silicon deposition and carbon coating, a silicon-carbon composite material with stable structure and high kinetic properties is formed.
It significantly improves the structural stability and cyclic stability of silicon-carbon composite materials, improves the rate performance and lithium ion transmission capabilities, and achieves the stable and efficient electrochemical performance of the battery.
Smart Images

Figure CN118754119B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of batteries, and in particular relates to a method for preparing a heterogeneous element doped carbon material. Background Art
[0002] The energy density of traditional lithium-ion batteries with layered oxides as positive electrodes and graphite as negative electrodes has gradually approached its theoretical limit. Developing new positive and negative electrode material systems is an important means to further improve the energy density of lithium-ion batteries. For negative electrode materials, silicon has become the most powerful candidate for the next generation of lithium-ion battery negative electrode materials because of its specific capacity (4200 mAh / g) that is about an order of magnitude higher than graphite, suitable working potential (0.4 V vs. Li+ / Li), abundant reserves, and environmental friendliness. However, during the lithium insertion / extraction process, silicon will produce a volume change of more than 300%, resulting in a series of negative effects such as particle breakage, electrode stripping, electrolyte consumption, and repeated SEI formation, which seriously hinders the practical application of silicon.
[0003] The electrochemical-mechanical properties of silicon have a significant size effect. Specifically, the nano-sized silicon anode can withstand the huge mechanical stress during the lithium insertion / extraction process, thereby inhibiting the structural damage of silicon and improving the cycle stability of silicon. However, the problems of increased interface side reactions, decreased compaction density, reduced processing performance, and increased production costs caused by the reduction of particle size make it difficult to achieve large-scale application. Micron-sized materials have more advantages in volume energy density, processing performance and cost. Therefore, the practical application of silicon-based anodes needs to combine the advantages of nanoscale and microscale to construct nano-micro composite materials to achieve a comprehensive improvement in comprehensive performance. Specifically, on the one hand, it is necessary to reduce the active silicon to nanoscale to exert the size effect of silicon and improve the structural stability. On the other hand, it is necessary to combine the nano-sized silicon together to form micron-sized particles to improve its practicality in the actual battery system. Therefore, it is a solution to use a carbon material with a nanoporous structure as a substrate and fill silicon into the pores through a chemical vapor infiltration method to form a silicon-based anode. However, due to the poor mechanical properties of the carbon material itself, during the lithium insertion / extraction process, it is easy to produce structural damage due to the change in silicon volume, resulting in reduced cycle stability. In addition, the low diffusion coefficient of lithium ions in carbon materials also limits the ability of the material to insert / extract lithium at high current density. Therefore, it is necessary to improve the mechanical properties and ion transport capacity of carbon materials to further improve the electrochemical performance of silicon-carbon composites. Summary of the invention
[0004] The purpose of the present invention is to improve the mechanical properties and ion transport capacity of porous carbon materials, and to provide a porous carbon material and a corresponding silicon-carbon material doped with heterogeneous elements to improve the mechanical properties and lithium ion transport capacity. In the process of preparing a porous carbon skeleton, heterogeneous doping elements are introduced therein to enhance the overall structural strength of the carbon skeleton, increase the lithium ion diffusion coefficient, maintain the structural stability and cycle stability of the silicon-carbon composite material in the electrochemical process, and improve the rate performance of the silicon-carbon composite material. The present invention provides the following technical solutions to achieve the above purpose:
[0005] A method for preparing a heterogeneous element-doped carbon material comprises the following steps:
[0006] (S1) mixing a phenolic monomer, an aldehyde monomer and a non-metallic doping source uniformly, prepolymerizing to obtain a liquid phenolic resin oligomer, then adding a metal doping source, mixing uniformly, and curing to obtain a solid precursor;
[0007] (S2) the solid precursor is sequentially crushed, pyrolyzed and carbonized, and activated to form pores to obtain a carbon material with a porous structure;
[0008] (S3) crushing the carbon material having a porous structure, putting it into a reactor and introducing a silicon-containing gas to perform silicon deposition, and then performing a stabilization treatment to obtain a silicon-carbon composite material;
[0009] (S4) Carbon coating is performed on the surface of the silicon-carbon composite material to obtain a product heterogeneous element doped carbon material.
[0010] Further, in step (S1), the phenolic monomers include but are not limited to phenol, o-cresol, m-cresol, p-cresol, 2,3-dimethylphenol, 2,4-dimethylphenol, 2,5-dimethylphenol, 2,6-dimethylphenol, 3,4-dimethylphenol, 3,5-dimethylphenol, resorcinol, tert-butylphenol, tert-octylphenol, tert-amylphenol, sec-butylphenol, cyclohexylphenol, nonylphenol, benzylphenol, bisphenol A, etc.; the aldehyde monomers include but are not limited to formaldehyde, paraformaldehyde, triformaldehyde, acetaldehyde, triacetaldehyde, furfural, propionaldehyde, butyraldehyde, acrolein, benzaldehyde, cinnamaldehyde, 2-furancarboxaldehyde, glyceraldehyde, ethanolaldehyde, malondialdehyde, succinaldehyde, phthalaldehyde, etc.; the molar ratio of the phenolic and aldehyde monomers is 1:0.5-1.5, preferably 1:0.7-1.
[0011] Further, in step (S1), the non-metallic doping source contains non-metallic elements such as boron, nitrogen, phosphorus, oxygen, sulfur, selenium, fluorine, chlorine, and bromine, and is specifically selected from at least one of urea, pyridine, pyrrole, acrylamide, melamine, polyvinylpyrrolidone, phosphoric acid, methyl phosphate, dimethyl phosphate, trimethyl phosphate, phosphorous acid, hypophosphorous acid, phenylphosphoric acid, triphenylphosphine, boric acid, isopropyl borate, triphenylborate, thiourea, ethanethiol, thioanisole, methyl sulfide, thiophenol, and thiophene. The amount of the non-metallic doping source is 7-12wt% of the total mass of the phenolic monomer and the aldehyde monomer.
[0012] Furthermore, in step (S1), the process parameters for curing phenolic monomers and aldehyde monomers to prepare liquid phenolic resin are well known in the art, such as in the presence of an alkaline catalyst, keeping warm for a period of time under stirring and heating conditions, the alkaline catalyst includes but is not limited to sodium hydroxide, ammonia water, barium hydroxide, calcium hydroxide, magnesium hydroxide, sodium carbonate, etc.; the amount of alkaline catalyst is such that the pH range of the system is greater than 9. The prepolymerization is carried out by keeping warm at 40-50°C for 5-10h to obtain a liquid phenolic resin oligomer.
[0013] Further, in step (S1), the metal doping source is a salt of metal lithium, potassium, magnesium, aluminum, calcium, tin, titanium, vanadium, chromium, zirconium, molybdenum, and germanium, and the salt is selected from acetate, halogen salt (fluoride salt, chloride salt, bromide salt), and nitrate. Specifically, the metal doping source includes but is not limited to lithium acetate, sodium acetate, potassium acetate, magnesium acetate, calcium acetate, aluminum acetate, titanium acetate, vanadium acetate, chromium acetate, zirconium acetate, niobium acetate, molybdenum acetate, germanium acetate, tin acetate, lithium nitrate, sodium nitrate, potassium nitrate, magnesium nitrate, calcium nitrate, aluminum nitrate, titanium nitrate, vanadium nitrate, chromium nitrate, zirconium nitrate, niobium nitrate, molybdenum nitrate, germanium nitrate, tin nitrate, lithium chloride, sodium chloride, potassium chloride, magnesium chloride, calcium chloride, aluminum chloride, titanium chloride, vanadium chloride, chromium chloride, zirconium chloride, niobium chloride, molybdenum chloride, germanium chloride, and tin chloride. The amount of the metal doping source is 1-5wt% of the sum of the mass of phenolic and aldehyde monomers, preferably 2-4wt%. There is no particular limitation on the method for uniformly mixing the metal doping source and the liquid phenolic resin oligomer, such as stirring.
[0014] Furthermore, in step (S1), the curing is carried out at 80-110° C. for 3-6 hours to obtain a solid precursor.
[0015] In step (S1), the preparation process of the solid precursor can be divided into two stages: preliminary polymerization and curing. The preliminary polymerization stage forms a polymer with a relatively low molecular weight, and then forms a high molecular weight phenolic resin after curing. The present invention performs two-step doping, in which non-metallic elements are doped in the preliminary polymerization stage, and metal elements are doped in the curing stage. Metallic elements cannot effectively form bonds with carbon under the conditions of preliminary polymerization of the resin, and effective atomic doping cannot be achieved, but can effectively bond with non-metallic elements such as boron, nitrogen, phosphorus, sulfur, selenium, fluorine, chlorine, and bromine through coordination bonds. Therefore, it is necessary to first perform doping of non-metallic elements in the preliminary polymerization stage, and then perform doping of metal elements in the curing stage. Through the doping of non-metallic elements, the stronger bond energy between non-metallic elements and carbon elements is utilized to enhance the structural strength of the material, thereby suppressing the particle crushing and pulverization caused by the material being unable to withstand large volume deformation due to low mechanical strength during the charge and discharge process, and enhancing structural stability and cycle stability. By doping with metal elements and taking advantage of the fact that metal elements can only combine with non-metallic doping elements, "end groups" that are not combined with carbon atoms are produced in the carbon skeleton, breaking the continuous network structure of carbon-carbon bonding and constructing a diffusion path for lithium ions in silicon-carbon composite materials, thereby improving the material's kinetic properties and charge and discharge rates.
[0016] Further, in step (S2), the crushing is to crush into particles of 10-70 mesh; the pyrolysis carbonization is carried out under an inert atmosphere at 400-700°C for 4-10 hours; the activation pore-forming method is carried out in an activation furnace, including physical activation, which includes but is not limited to oxygen, water vapor, carbon dioxide, etc., the activation temperature is 700-1050°C, and the activation time is 10-20 hours. The pore size of the carbon material with a porous structure after activation pore-forming is 0.4-50 nm, and the specific surface area is 1300-2700 m 2 / g.
[0017] Further, in step (S3), the median particle size of the carbon material after crushing is 1-20 um, preferably 5-15 um; the silicon-containing gas includes but is not limited to monosilane, disilane, trisilane, monochlorosilane, dichlorosilane, trichlorosilane, and silicon tetrachloride; the stabilization process is heat treated at 350-420°C for 1-5 h in an atmosphere of oxygen, carbon dioxide, acetylene, ethylene, propylene, propyne, methane, ethane, propane, etc. The silicon content of the silicon-carbon composite material is 30-70wt%, preferably 50-60wt%. Silicon is uniformly filled in the pores of the above-mentioned carbon material, and some silicon may also exist on the surface of the carbon material.
[0018] Furthermore, in step (S4), the carbon coating is carried out at 500-700° C. after the air is excluded and the carbon source process gas and the inert gas are introduced into the reactor together, and the thickness of the carbon coating layer is 2-20 nm, preferably 5-10 nm.
[0019] The present invention achieves the synergistic effect of non-metallic element doping and metal element doping by introducing non-metallic element doping and metal element doping respectively in the prepolymerization and curing stages of phenolic resin, and the combined effect greatly improves the electrochemical performance of silicon-carbon composite materials. First, in the synthesis of phenolic resin, a non-metallic doping source is added in the mixing stage of phenolic and aldehyde monomers to achieve uniform dispersion of the non-metallic doping source, and the reaction conditions are controlled to obtain a non-metallic doped liquid phenolic resin oligomer solution. At this time, a metal doping source is added, and the previous non-metallic doping is utilized to achieve the combined effect of the metal doping element and the non-metallic element to improve the structural stability and cycle stability of the silicon-carbon composite material. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a scanning electron microscope photograph of the silicon-carbon composite material obtained in Example 1;
[0021] Figure 2 This is a transmission electron microscope photo of the silicon-carbon composite material obtained in Example 1;
[0022] Figure 3 This is the first charge and discharge curve of the silicon-carbon composite material prepared in Example 1. DETAILED DESCRIPTION
[0023] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments.
[0024] The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.
[0025] The scanning electron microscope (SEM) was Regulus 8100, and the transmission electron microscope (TEM) was JEM-2100F.
[0026] Example 1
[0027] (S1). Preparation of carbon material precursor: First, 7.1 kg of m-diphenol was added to the reactor, followed by 7.2 kg of 37% formaldehyde solution and 1 kg of melamine. After stirring evenly, the mixture was heated to 50 °C and reacted at a constant temperature for 12 h to obtain a liquid phenolic resin oligomer. Then, 0.20 kg of molybdenum acetate was added, and the mixture was heated to 110 °C and reacted at a constant temperature for 6 h to obtain a solid nitrogen-doped phenolic resin, i.e., a solid precursor.
[0028] (S2) Preparation of carbon materials: The solid precursor obtained in step (S1) was crushed into 10 mesh particles, heated to 700 ° C for 4 hours under nitrogen protection to obtain a carbonized doped carbon material; the carbonized material was placed in an activation furnace and kept at 900 ° C for 6 hours under a carbon dioxide atmosphere to obtain a porous doped carbon material; the pore size was between 0.4-5 nm and the specific surface area was 1800 m 2 / g;
[0029] (S3) Preparation of silicon-carbon composite material: 10 kg of porous doped carbon material was crushed to a median particle size of about 10 μm, and put into a vertical fluidized bed reactor. After excluding the air, 15 L / min of silane gas was introduced at 420 °C and kept warm for 6 h. Subsequently, 10 L / min of acetylene gas was introduced and kept warm for 1 h, and then cooled to room temperature and discharged to obtain a doped silicon-carbon composite negative electrode material with a silicon content of 48.2 wt%;
[0030] (S4). Coating of silicon-carbon composite materials: 20 kg of doped silicon-carbon composite negative electrode material was put into a coating furnace. After the air was removed, 13 L / min of methane gas and 13 L / min of nitrogen were introduced as protective gas at 530 °C. The temperature was kept for 4 hours to obtain a doped silicon-carbon composite negative electrode material coated with a surface carbon shell, i.e., the product heterogeneous element doped carbon material.
[0031] Figure 1 This is a scanning electron microscope photograph of the silicon-carbon composite material prepared in Example 1. The particle size is about 6.5 μm. Figure 2 This is a projection electron microscope photograph of the silicon-carbon composite material prepared in Example 1. It can be seen that the thickness of the coating layer is about 6 nm.
[0032] Figure 3 This is the first charge and discharge curve of the silicon-carbon composite material prepared in Example 1.
[0033] Example 2
[0034] Other conditions and operations are the same as those in Example 1, except that in step (S1), 1 kg of melamine is replaced by 0.7 kg of urea, and 0.20 kg of molybdenum acetate is replaced by 0.28 kg of tin acetate.
[0035] Example 3
[0036] Other conditions and operations were the same as those in Example 1, except that in step (S1), 1 kg of melamine was replaced by 1.4 kg of polyvinyl pyrrolidone, and 0.20 kg of molybdenum acetate was replaced by 0.39 kg of zirconium chloride.
[0037] Example 4
[0038] Other conditions and operations were the same as those in Example 1, except that in step (S1), 1 kg of melamine was replaced by 0.8 kg of thiourea.
[0039] Example 5
[0040] Other conditions and operations were the same as those in Example 1, except that in step (S1), 1 kg of melamine was replaced by 0.7 kg of phosphoric acid.
[0041] Example 6
[0042] Other conditions and operations were the same as those in Example 1, except that in step (S1), 1 kg of melamine was replaced by 0.6 kg of isopropyl borate.
[0043] Comparative Example 1
[0044] The other operations are the same as those in Example 1, except that step (S1) is changed to: 7.1 kg of m-diphenol is added to the reactor, and then 7.2 kg of 37% formaldehyde solution, 1 kg of melamine and 0.20 kg of molybdenum acetate are added, and the mixture is stirred evenly and heated to 50° C. and reacted at a constant temperature for 12 h to initially obtain a liquid phenolic resin oligomer, and then heated to 110° C. and reacted at a constant temperature for 6 h to obtain a solid doped phenolic resin, i.e., a solid precursor.
[0045] Comparative Example 2
[0046] The other operations are the same as those in Example 1, except that step (S1) is changed to: 7.1 kg of m-diphenol is added to the reactor, and then 7.2 kg of 37% formaldehyde solution is added, and the mixture is stirred evenly and heated to 50°C for constant temperature reaction for 12 h to initially obtain a liquid phenolic resin oligomer, 1 kg of melamine and 0.20 kg of molybdenum acetate are added, mixed evenly, and then heated to 110°C for constant temperature reaction for 6 h to obtain a solid doped phenolic resin, i.e., a solid precursor.
[0047] Comparative Example 3
[0048] The other operations are the same as those in Example 1, except that step (S1) is changed to: 7.1 kg of m-diphenol is added to the reactor, and then 7.2 kg of 37% formaldehyde solution and 1 kg of melamine are added, and the mixture is stirred evenly and heated to 50°C for constant temperature reaction for 12 h to initially obtain a liquid phenolic resin oligomer, and then heated to 110°C for constant temperature reaction for 6 h to obtain a solid doped phenolic resin, i.e., a solid precursor.
[0049] Comparative Example 4
[0050] The other operations are the same as those in Example 1, except that step (S1) is changed to: 7.1 kg of m-diphenol is added to the reactor, and then 7.2 kg of 37% formaldehyde solution is added, and the mixture is stirred evenly and heated to 50 °C for constant temperature reaction for 12 h to initially obtain a liquid phenolic resin oligomer, and then 0.20 kg of molybdenum acetate is added, and the mixture is subsequently heated to 110 °C for constant temperature reaction for 6 h to obtain a solid doped phenolic resin, i.e., a solid precursor.
[0051] Application Examples
[0052] The electrochemical properties of the silicon-based negative electrode materials prepared in the above examples and comparative examples were tested according to the following method: the prepared silicon-carbon composite material, carbon black and carboxymethyl cellulose (CMC) were mixed with styrene-butadiene rubber (SBR) composite binder in a mass ratio of 80:10:10 to form a slurry (wherein the mass ratio of CMC to SBR was 1:1), the slurry was uniformly coated on a copper foil current collector, and vacuum dried for 12 h to form a working electrode; a lithium sheet was used as a counter electrode, a glass fiber membrane (purchased from Whatman, UK) was used as a diaphragm, 1 mol / L LiPF6 (the solvent was a mixture of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1) was used as an electrolyte, 1% VC and 5% FEC were added to the electrolyte, and button cells were assembled in an argon atmosphere in a Braun inert gas glove box in Germany.
[0053] The silicon-carbon composite material prepared in Example 1 was subjected to electrochemical analysis test, and the results are as follows: Figure 3 The charge and discharge range is 0-1.5 V. When charged and discharged at a current density of 0.2C, the material capacity can reach 1925.4 mAh / g, and the first cycle coulombic efficiency is 91.5%. When charged and discharged at 1C, the specific capacity is 88.7% under 0.2C conditions, that is, the 1C capacity retention rate; the capacity of the battery is maintained at 97.2% after 100 cycles at 1C, proving that the silicon-carbon composite material obtained by the present invention has good cycle stability and rate performance.
[0054] The negative electrode materials of other embodiments and comparative examples were subjected to charge and discharge tests according to the above method, and the results are shown in Table 1 below:
[0055] Table 1 Electrochemical performance test
[0056] .
[0057] In summary, the silicon-carbon composite material prepared by element-doped porous carbon provided by the present invention has good structural stability and kinetic performance, so that the battery has stable cycle and excellent rate performance, and the preparation method provided by the present invention is simple and easy to implement, and is suitable for industrial-scale production. Comparative Examples 1-4 cannot effectively form co-doping of metal elements and non-metals, so the electrochemical performance is poor.
Claims
1. A method for preparing a heterogeneous element doped carbon material, It is characterized in that The following steps are involved: (S1) mixing a phenolic monomer, an aldehyde monomer and a non-metallic doping source uniformly, prepolymerizing to obtain a liquid phenolic resin oligomer, then adding a metal doping source, mixing uniformly, and curing to obtain a solid precursor; The prepolymerization is carried out by heat preservation at 40-50°C for 5-10 hours to obtain a liquid phenolic resin oligomer; the curing is carried out by heat preservation at 80-110°C for 3-6 hours to obtain a solid precursor; (S2) the solid precursor is sequentially crushed, pyrolyzed and carbonized, and activated to form pores to obtain a carbon material with a porous structure; (S3) crushing the carbon material having a porous structure, putting it into a reactor and introducing a silicon-containing gas to perform silicon deposition, and then performing a stabilization treatment to obtain a silicon-carbon composite material; (S4) Carbon coating is performed on the surface of the silicon-carbon composite material to obtain a product heterogeneous element doped carbon material.
2. The preparation method according to claim 1, It is characterized in that In step (S1), the phenol monomer includes phenol, o-cresol, m-cresol, p-cresol, 2,3-dimethylphenol, 2,4-dimethylphenol, 2,5-dimethylphenol, 2,6-dimethylphenol, 3,4-dimethylphenol, 3,5-dimethylphenol, resorcinol, tert-butylphenol, tert-octylphenol, tert-amylphenol, sec-butylphenol, cyclohexylphenol, nonylphenol, benzylphenol or bisphenol A; the aldehyde monomer includes formaldehyde, paraformaldehyde, triformaldehyde, acetaldehyde, triacetaldehyde, furfural, propionaldehyde, butyraldehyde, acrolein, benzaldehyde, cinnamaldehyde, 2-furancarboxaldehyde, glyceraldehyde, ethanolaldehyde, malondialdehyde, succinaldehyde or phthalaldehyde; the molar ratio of the phenol and aldehyde monomers is 1:0.5-1.
5.
3. The preparation method according to claim 1, It is characterized in that In step (S1), the non-metallic doping source contains boron, nitrogen, phosphorus, oxygen, sulfur, selenium, fluorine, chlorine or bromine; the metal doping source is a salt of metal lithium, potassium, magnesium, aluminum, calcium, tin, titanium, vanadium, chromium, zirconium, molybdenum, or germanium, and the salt is selected from acetates, halides, and nitrates.
4. The preparation method according to claim 3, It is characterized in that In step (S1), the non-metallic doping source is selected from at least one of urea, pyridine, pyrrole, acrylamide, melamine, polyvinylpyrrolidone, phosphoric acid, methyl phosphate, dimethyl phosphate, trimethyl phosphate, phosphorous acid, hypophosphorous acid, phenylphosphoric acid, triphenylphosphine, boric acid, isopropyl borate, triphenylborate, thiourea, ethanethiol, anisyl thioether, methyl sulfide, thiophenol, and thiophene; the amount of the non-metallic doping source is 7-12wt% of the total mass of the phenolic monomer and the aldehyde monomer.
5. The preparation method according to claim 3, It is characterized in that In step (S1), the metal doping source is selected from at least one of lithium acetate, sodium acetate, potassium acetate, magnesium acetate, calcium acetate, aluminum acetate, titanium acetate, vanadium acetate, chromium acetate, zirconium acetate, niobium acetate, molybdenum acetate, germanium acetate, tin acetate, lithium nitrate, sodium nitrate, potassium nitrate, magnesium nitrate, calcium nitrate, aluminum nitrate, titanium nitrate, vanadium nitrate, chromium nitrate, zirconium nitrate, niobium nitrate, molybdenum nitrate, germanium nitrate, tin nitrate, lithium chloride, sodium chloride, potassium chloride, magnesium chloride, calcium chloride, aluminum chloride, titanium chloride, vanadium chloride, chromium chloride, zirconium chloride, niobium chloride, molybdenum chloride, germanium chloride, and tin chloride; the amount of the metal doping source is 2-4wt% of the sum of the mass of the phenolic and aldehyde monomers.
6. The preparation method according to claim 1, It is characterized in that In step (S1), phenol monomers and aldehyde monomers are cured to prepare liquid phenolic resin in the presence of an alkaline catalyst, and the temperature is kept for a period of time under stirring and heating conditions. The alkaline catalyst includes sodium hydroxide, ammonia water, barium hydroxide, calcium hydroxide, magnesium hydroxide or sodium carbonate; the amount of the alkaline catalyst is such that the pH range of the system is greater than 9.
7. The preparation method according to claim 1, It is characterized in that In step (S2), the crushing is to crush into particles of 10-70 mesh; the pyrolysis carbonization is carried out under an inert atmosphere at 400-700°C for 4-10 hours; the pore size of the carbon material with a porous structure after activation and pore formation is 0.4-50 nm, and the specific surface area is 1300-2700 m 2 / g.
8. The preparation method according to claim 1, It is characterized in that In step (S3), the median particle size of the carbon material after crushing is 5-15μm; the silicon-containing gas includes but is not limited to monosilane, disilane, trisilane, monochlorosilane, dichlorosilane, trichlorosilane, and silicon tetrachloride; the stabilization treatment process is a heat treatment at 300-420°C for 1-5 h in an atmosphere of oxygen, carbon dioxide, acetylene, ethylene, propylene, propyne, methane, ethane, and propane; the silicon content of the silicon-carbon composite material is 50-60wt%; and / or in step (S4), the carbon coating is carried out by excluding air, and then introducing the carbon source process gas and the inert gas into the reactor at 500-700°C, and the thickness of the carbon coating layer is 5-10nm.
9. A heterogeneous element doped carbon material, It is characterized in that It is prepared by the preparation method according to any one of claims 1 to 8.