Preparation method of nanoscale porous silicon with controllable size
Patent Information
- Application Number
- CN202410971107.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-19
AI Technical Summary
[0004]综上所述,现有多孔硅的制备主要存在的问题是:(1)现有方法较多使用的原料为块体硅,多为不规则或二维形貌,以此原料制得的多孔硅尺寸不可控,且颗粒为微米级,用于制备电极材料时团聚较为严重,制得的电极材料性能较差,电极的循环稳定性不好;(2)在蚀刻过程中,多使用HF溶液,环境不友好,且蚀刻得到的粉体颗粒孔径不均一、孔结构坍塌
[0028] 1. The present invention can synthesize Si of different sizes by using ethyl orthosilicate to undergo hydrolysis and polycondensation in an ethanol aqueous solution. x O y Precursor material, for Si x O y After the precursor material is dispersed and activated, mixed with inorganic salts and reducing agents, and calcined for reduction, nanoscale Si particles with dispersed particles can be obtained. x O y Precursor material; for the resulting nanoscale Si x O y The precursor material is etched in an acid solution with a dispersant added to obtain a spherical nanoporous silicon material with completely dispersed particles and uniform pore size; the preparation is convenient, simple and low-cost, and non-toxic and harmless chemical reactions are used in the preparation process material, environmentally friendly, green and environmentally friendly.
Smart Images

Figure CN118754129A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of material processing, and in particular to a method for preparing size-controllable nano-scale porous silicon. Background Art
[0002] Porous silicon is a three-dimensional nanoporous material with the characteristics of large specific surface area, photoluminescence, and excellent anti-reflection properties. The porous structure also brings abundant active sites and high connectivity. Current research on porous silicon has involved a series of energy conversion and storage devices such as biological and chemical sensors, drug delivery, lithium-ion batteries, and supercapacitors.
[0003] According to the different etching processes, the preparation of porous silicon mainly includes electrochemical etching (anodization), photochemical corrosion, chemical corrosion, de-alloying and magnesium thermal reduction. Electrochemical etching is the most commonly used preparation method for porous silicon materials. HF is used as the electrolyte, p / n type silicon material is used as the anode, Pt or graphite is used as the cathode, and an anodic oxidation reaction is carried out. However, silicon plates are generally used in the reaction process. The composition and concentration of the electrolyte, the resistivity and crystal phase of silicon, the temperature during electrolysis and the light conditions have an important influence on the film formation speed of porous silicon, and the current density is unevenly distributed on the silicon material, resulting in uneven and incomplete etching of the obtained material surface, and more impurities. Photochemical etching is to immerse the bulk silicon in an HF solution under the action of light for etching reaction. The solution concentration, the doping degree of the silicon wafer and the light intensity are the main factors affecting the corrosion rate. The chemical etching method uses precious metals such as Pt, Au, etc. on the surface of the bulk Si, and then etches the precious metals to form a porous structure. However, the correlation and mutual restriction between the intrinsic variables of etching reaction (such as, the type and morphology of precious metal, the intrinsic characteristics of etching agent, Si substrate, temperature, etc.) of photochemical etching and chemical etching are still not accurately grasped, and the repeatability is poor. The de-alloying method obtains porous silicon material by etching away the metal in Si-metal alloy, but the ratio of Si-metal greatly affects the morphology and performance of the porous silicon finally obtained. The higher the metal content, the larger the specific surface area of the porous silicon formed, and the higher the porosity. However, if the metal content in the alloy exceeds a certain amount, the porous silicon after etching will be unable to maintain the original structure, its specific surface area and porosity will be reduced, and the cyclic stability of the material will also be deteriorated. Therefore, the performance of porous silicon prepared by de-alloying method is closely related to the parameters such as the alloy type, size, and silicon content in the alloy used, so, the silicon alloy made by different manufacturers is used as a precursor to prepare porous silicon, and when the performance test is finally performed, the electrochemical performance obtained is also quite different, and for the silicon alloy produced by the same manufacturer, the different silicon content in the alloy will also affect the performance of the product. The magnesium thermal reduction method is to synthesize silicon by reducing SiO2 and Mg, and then use HF etching to remove the residual SiO2 to obtain porous silicon with good electrochemical properties. The existing magnesium thermal reduction method for producing porous silicon materials has the following problems: incomplete reaction, resulting in the formation of by-product Mg2Si, uneven surface of powder particles, collapse of pore structure, and environmental unfriendliness (using HF for etching).
[0004] In summary, the main problems in the preparation of existing porous silicon are: (1) the raw materials mostly used in the existing methods are bulk silicon, which is mostly irregular or two-dimensional in morphology. The size of the porous silicon prepared from this raw material is uncontrollable, and the particles are in the micron level. When used to prepare electrode materials, agglomeration is more serious, the performance of the prepared electrode material is poor, and the cycle stability of the electrode is not good; (2) During the etching process, HF solution is mostly used, which is environmentally unfriendly, and the pore size of the powder particles obtained by etching is uneven and the pore structure collapses. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a method for preparing size-controllable nanoscale porous silicon.
[0006] The technical solution adopted by the present invention is as follows:
[0007] A method for preparing size-controllable nanoscale porous silicon comprises the following steps:
[0008] (1) Preparation of precursor: Ammonia water was added to the ethanol aqueous solution to adjust the pH, and tetraethyl orthosilicate was added after sufficient stirring to carry out stirring reaction. After the reaction, the precipitate was washed with deionized water and freeze-dried to obtain Si particles of different sizes. x O y Precursor material A; wherein x is 1 to 2, and y is 1 to 6;
[0009] (2) Si obtained in step (1) x O y Precursor material A was dispersed in anhydrous ethanol, a dispersant was added, and after ultrasonic dispersion, the reaction was stirred, and the precipitate was washed with deionized water to obtain Si x O y Precursor material B;
[0010] (3) Si obtained in step (2) x O y Precursor material B was added to the activation solution and stirred. The precipitate was washed with deionized water until neutral and freeze-dried to obtain Si x O y Precursor material C;
[0011] (4) Si obtained in step (3) x O y Precursor material C is mixed with a reducing agent and an inorganic salt, calcined and reduced under an inert atmosphere, and cooled to room temperature to obtain a solid mixture;
[0012] (5) The solid mixture obtained in step (4) is etched with an acid, and a dispersant is added, and then washed with deionized water until it is neutral, and freeze-dried to obtain nano-scale porous silicon.
[0013] Preferably, in step (2), the dispersant is at least one of polyethylene glycol, polyvinyl pyrrolidone and Tween@80.
[0014] As a non-ionic dispersant, polyethylene glycol has good solubility and wettability and can x O y The surface O or adsorbed H2O molecules form hydrogen bonds or van der Waals forces, and when hydrogen bonds are formed with H2O molecules, Si x O y The interaction between particles; the hydrophilic groups in the molecular structure of polyvinyl pyrrolidone and Si x O y The particle surfaces interact with each other to form an adsorption film, which generates repulsion and surface tension between the particles, changes the hydrophilicity and lipophilicity of the particle surface, and has a certain stability in the molecular structure. At the same time, it adjusts the rheological properties of the solution, and the protective film formed can improve the stability of the particles. Tween@80 is an oleate ester. As a non-ionic surfactant, it has strong hydrophilicity and emulsification, can competitively occupy the interface position, and inhibit Si x O y Adsorbed to the gas-liquid interface, thereby reducing oxidation or aggregation caused by contact with air, and effectively preventing Si x O y Expands at the interface during the reaction.
[0015] Preferably, in step (3), the surfactant is at least one of palladium chloride, copper sulfate, silver nitrate and stannous chloride.
[0016] Palladium chloride, copper sulfate, silver nitrate and stannous chloride all contain excess electrons, which can provide additional electron donors; they all have leaving properties, and after leaving the corresponding ions, they form relatively stable negative ions; they all have certain reducing properties, and can participate in the reduction reaction by donating electrons or negative charges, thereby accelerating the reaction.
[0017] Preferably, in step (4), the reducing agent is at least one of magnesium powder, magnesium diboride, magnesium carbide and magnesium oxide.
[0018] Make Si x O y Fully reduce while reducing the formation of by-products.
[0019] Preferably, in step (5), the acid is at least one of hydrochloric acid, nitric acid and acetic acid.
[0020] Although hydrochloric acid, nitric acid and acetic acid are highly acidic, compared with hydrofluoric acid, hydrofluoric acid is very corrosive, and the volatile gas is highly irritating to human skin and respiratory tract. Once it enters the blood, it will react with the human body to produce insoluble substances and block blood vessels.
[0021] Preferably, in step (5), the dispersant is at least one of polyethylene glycol, sodium oleate, polyvinyl pyrrolidone and Tween@80.
[0022] Preferably, in step (1), the volume ratio of tetraethyl orthosilicate to aqueous ammonia is 1:(1-25), and the volume ratio of ethanol to deionized water in the ethanol-water solvent is (4-20):1; the reaction temperature is 25-80°C, and the reaction time is 4-12h.
[0023] Preferably, in step (2), the dispersant and Si x O y The mass ratio of the precursor material A is (0.5-2):1, the mass volume ratio of the dispersant to anhydrous ethanol is (1.5-1500) g: (10-1000) mL; and the stirring time after ultrasound is 6-12 h.
[0024] Preferably, in step (3), the activator and Si x O y The mass ratio of the precursor material B is (0.01-0.5):1, the mass volume ratio of the activator to the ethanol aqueous solution is (0.04-2) g: (20-1000) mL; and the activation treatment time is 0.5-2 h.
[0025] Preferably, in step (4), Si x O y The molar ratio of the precursor material C to the reducing agent is 1:(1-2.5), Si x O y The molar ratio of the precursor material C to the inorganic salt is 1:(1-10); the calcination reduction temperature is 500-900° C., and the calcination reduction time is 2-10 hours.
[0026] Preferably, in step (5), the concentration of the acid is (0.1-10) mol / L; the temperature of the acid etching treatment is 25-65° C., and the time is 0.5-12 h.
[0027] The beneficial effects of the present invention are:
[0028] 1. The present invention can synthesize Si nanoparticles of different sizes by hydrolyzing and polycondensing tetraethyl orthosilicate in an ethanol aqueous solution. x O y Precursor materials, for Si x Oy After the precursor material is dispersed and activated, it is mixed with an inorganic salt and a reducing agent, and calcined and reduced to obtain nano-scale Si dispersed particles. x O y Precursor materials; the resulting nano-scale Si x O y The precursor material is etched in an acid solution with a dispersant added thereto to obtain a spherical nanoporous silicon material with completely dispersed particles and uniform pore size. The preparation method is convenient and simple, with low cost, and non-toxic and harmless chemical reactants are used in the preparation process, which is environmentally friendly and green.
[0029] 2. The present invention can effectively remove the excess heat generated in the highly exothermic reaction by introducing inorganic salts in the calcination reduction step, and prevent the collapse and cross-linking of the pore structure of the obtained porous silicon. In addition, the inorganic salt can be used as an agglomeration inhibitor to effectively prevent the generation of the byproduct Mg2Si and the agglomeration of the product porous silicon, which not only maintains the advantages of the nanostructure in terms of cycle stability, but also inhibits the generation of excess SiO x formation. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 For the SiO of Examples 1, 2, and 3 x XRD patterns of the precursor materials.
[0031] Figure 2 1 and 2 are XRD diagrams of the porous silicon materials of Examples 1, 2 and 3.
[0032] Figure 3 The SiO of Example 1 x SEM image of the precursor material.
[0033] Figure 4 The SiO of Example 2 x SEM image of the precursor material.
[0034] Figure 5 The SiO of Example 3 x SEM image of the precursor material.
[0035] Figure 6 This is the SEM image of the 50nm porous silicon material of Example 1.
[0036] Figure 7 This is the SEM image of the 200nm porous silicon material of Example 2.
[0037] Figure 8 This is the SEM image of the 500nm porous silicon material of Example 3.
[0038] Fig. 9 This is the SEM image of the 50nm porous silicon material of Example 4.
[0039] Fig.10 This is the SEM image of the 200nm porous silicon material of Example 5.
[0040] Fig.11 This is the SEM image of the 500nm porous silicon material of Example 6. Specific implementation methods
[0042] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.
[0043] Example 1
[0044] A method for preparing 50nm porous silicon, specifically:
[0045] S1: Synthesis of 50nm SiO2 precursor material: Add ammonia water to 100mL deionized water to adjust the pH to 8.5, then add 20mL tetraethyl orthosilicate and 80mL anhydrous ethanol to the solution, react at 60℃ for 12h, wash the precipitate with deionized water until neutral, freeze-dry to obtain 50nm SiO2 precursor material, XRD and SEM test of the material are as follows Figure 1 , Figure 3 shown.
[0046] from Figure 1 It can be seen that the present invention successfully synthesized SiO2 precursor material. Figure 3 It can be seen that the size of the synthesized SiO2 precursor material is 50nm.
[0047] S2: Pre-treat the SiO2 precursor material prepared in step S1: disperse 0.2g SiO2 in 20mL anhydrous ethanol, add 0.9g polyethylene glycol solution, ultrasonically disperse for 0.5h, stir for 6h, wash with deionized water and add it to 20mL, 10g / L SnCl2 solution, stir for 0.5h, then add it to 5g / L PdCl2 solution for activation for 0.5h, wash with deionized water until neutral, freeze-dry for later use;
[0048] S3: uniformly mixing the pretreated SiO2 precursor material, Mg2C3 and NaCl obtained in step S2, wherein the molar ratio of the mixture is 1:1:0.005;
[0049] S4: heating the mixture obtained in step S3 to 500° C. in a nitrogen atmosphere, maintaining the temperature for 4 hours, and then naturally cooling to room temperature in an inert gas atmosphere to obtain a corresponding solid powder;
[0050] S5: The solid powder obtained in step S4 was added to 20 mL of 0.5 M HNO3 solution, and 1.5 mL of Tween@80 was added, stirred for 1 h, then washed with deionized water until neutral, and freeze-dried to obtain a 50 nm porous silicon material.
[0051] The XRD and SEM tests of the 50 nm porous silicon material obtained in Example 1 are as follows: Figure 2 , Figure 6 As shown. Figure 2 It can be seen that porous silicon was successfully synthesized in this embodiment. Figure 6 It can be seen that the synthesized 50 nm porous silicon forms a rich porous structure with uniform pore size and no pore collapse and cross-linking.
[0052] Example 2
[0053] A method for preparing 200nm porous silicon, specifically:
[0054] S1: Synthesis of 200nm SiO2 precursor material: Add ammonia water to 150mL ethanol aqueous solution (the volume ratio of anhydrous ethanol to deionized water is 2:1) to adjust the pH to 8, add 15mL tetraethyl orthosilicate to the solution after sufficient stirring, react at 40℃ for 6h, wash with deionized water to neutrality, freeze-dry to obtain 200nm SiO2 precursor material, XRD and SEM test of the material are as follows Figure 1 , Figure 4 As shown. Figure 1 We can see that we have successfully synthesized SiO2. Figure 4 It can be seen that the synthesized SiO2 is 50nm;
[0055] S2: Pre-treat the SiO2 precursor material obtained in step S1: disperse 0.2g SiO2 in 20mL anhydrous ethanol, add 0.9g polyethylene glycol solution, ultrasonically disperse for 0.5h, stir for 6h, and wash with deionized water. Then add it to 20mL 10g / L CuSO4 solution for activation for 2h, wash with deionized water until neutral, and freeze-dry for later use;
[0056] S3-S5: Same as Example 1.
[0057] The XRD and SEM tests of the 200 nm porous silicon material obtained in Example 2 are as follows: Figure 2 , Figure 7 shown. Figure 2 It can be seen that the present invention successfully synthesizes Si; Figure 7 It can be seen that the synthesized 200 nm porous silicon has no agglomeration and the particles are dispersed.
[0058] Example 3
[0059] A method for preparing 500nm porous silicon, specifically:
[0060] S1: Synthesis of 500nm SiO2 precursor material: Add ammonia water to 50mL ethanol aqueous solution (the volume ratio of anhydrous ethanol to deionized water is 19:1) to adjust the pH to 9, then add 2mL tetraethyl orthosilicate to the solution, react at room temperature for 12h, wash with deionized water to neutrality, and freeze-dry to obtain 500nm SiO2 precursor material. The XRD and SEM tests of the material are as follows: Figure 1 , Figure 5 As shown. Figure 1 We can see that we have successfully synthesized SiO2. Figure 5 It can be seen that the synthesized SiO2 is 50nm;
[0061] S2: Pre-treat the SiO2 precursor material obtained in step S1: disperse 0.2g SiO2 in 20mL anhydrous ethanol, add 0.9g polyethylene glycol solution, ultrasonically disperse for 0.5h, stir for 6h, and wash with deionized water. Then add it to 30mL 8g / L AgNO3 solution for activation for 0.5h, wash with deionized water until neutral, and freeze-dry for later use;
[0062] S3-S5: Same as Example 1.
[0063] The XRD and SEM tests of the 500nm porous silicon material obtained in Example 3 are as follows: Figure 2 , Figure 8 shown. Figure 2 We can see that we have successfully synthesized Si. Figure 8 It can be seen that the synthesized 500nm porous silicon is arranged neatly and orderly, and the porous structure is dense and uniform.
[0064] Example 4
[0065] A method for preparing 50nm porous silicon, specifically:
[0066] S1: Same as Example 1;
[0067] S2: Pre-treat the 50nm SiO2 precursor prepared in step S1: disperse 0.2g SiO2 in 20mL anhydrous ethanol, add 1.2g polyvinyl pyrrolidone, ultrasonically disperse for 0.5h, stir for 6h, and wash with deionized water. Then add it to 20mL of 10g / L SnCl2 solution, stir for 0.5h, then add it to 5g / L PdCl2 solution for activation for 0.5h, wash with deionized water until neutral, and freeze-dry for use;
[0068] S3: uniformly mixing the pretreated SiO2 precursor material, Mg and NaCl prepared in step S2, wherein the molar ratio of the mixture is 1:1.2:0.005;
[0069] S4: heating the mixture obtained in step S3 to 600° C. in a nitrogen atmosphere, maintaining the temperature for 5 hours, and then naturally cooling to room temperature in an inert gas atmosphere to obtain a corresponding solid powder;
[0070] S5: The solid powder calcined in step S4 was added to 20 mL of 1.2 M HCl solution, and 1.2 g of polyethylene glycol was added, stirred for 1 h, then washed with deionized water until neutral, and freeze-dried to obtain a 50 nm porous silicon material.
[0071] Example 4 The SEM of the 50nm porous silicon material obtained is as follows Fig. 9 shown. Fig. 9 It can be seen that the 50 nm porous silicon synthesized in the present invention forms a rich porous structure with uniform pore size and no pore collapse and cross-linking.
[0072] Example 5
[0073] A method for preparing 200nm porous silicon, specifically:
[0074] S1: Same as Example 2;
[0075] S2: Pre-treat the 200nm SiO2 precursor prepared in step S1: disperse 0.2g SiO2 in 20mL anhydrous ethanol, add 2.5mL Tween@80 solution, ultrasonically disperse for 0.5h, stir for 6h, and wash with deionized water. Then add it to 20mL of 10g / L SnCl2 solution, stir for 0.5h, and then add it to 5g / L PdCl2 solution for activation for 0.5h, wash with deionized water until neutral, and freeze-dry for use;
[0076] S3: uniformly mix the pretreated SiO2 precursor material, MgB2, and NaCl prepared in step S2, wherein the molar ratio of the mixture is 1:1.5:0.008;
[0077] S4: heating the mixture obtained in step S3 to 650° C. in a nitrogen atmosphere, maintaining the temperature for 6 hours, and then naturally cooling to room temperature in an inert gas atmosphere to obtain a corresponding solid powder;
[0078] S5: The solid powder obtained in step S4 was added to 20 mL of 1.5 M CH3COOH solution, 0.5 g of polyvinyl pyrrolidone and 0.5 g of sodium oleate were added, stirred for 1 h, then washed with deionized water until neutral, and freeze-dried to obtain a 200 nm porous silicon material.
[0079] Example 5 The SEM of the 200nm porous silicon material obtained is as follows Fig.10 shown. Fig.10 It can be seen that the 200 nm porous silicon synthesized in the present invention has no agglomeration of particles and a dense and uniform pore structure.
[0080] Example 6
[0081] A method for preparing 500nm porous silicon, specifically:
[0082] S1: Same as Example 3;
[0083] S2: Pre-treat the 500nm SiO2 precursor material prepared in step S1: disperse 0.2g SiO2 in 20mL anhydrous ethanol, add 1.5g polyethylene glycol solution, ultrasonically disperse for 0.5h, stir for 6h, and wash with deionized water. Then add it to 20mL of 10g / L SnCl2 solution, stir for 0.5h, and then add it to 2g / L Ag(NO3)2 solution for activation for 0.5h, wash with deionized water until neutral, and freeze-dry for use;
[0084] S3: uniformly mixing the pretreated SiO2 precursor material obtained in step S2 with Mg, MgO and NaCl, wherein the molar ratio of the mixture is 1:1:0.005;
[0085] S4: heating the mixture obtained in step S3 to 800° C. in a nitrogen atmosphere, maintaining the temperature for 8 hours, and then naturally cooling to room temperature in an inert gas atmosphere to obtain a corresponding solid powder;
[0086] S5: The solid powder obtained in step S4 was added into 20 mL of 5M HCl solution, and 1.5 mL of Tween@80 was added and stirred for 6 h, then washed with deionized water until neutral, and freeze-dried to obtain a 500 nm porous silicon material.
[0087] The SEM test of the 500nm porous silicon material obtained in Example 6 is as follows Fig.11 shown. Fig.11 It can be seen that the synthesized 500 nm porous silicon particles have no agglomeration and the porous structure is dense and uniform.
[0088] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification or equivalent changes made to the above embodiments based on the technical essence of the present invention fall within the protection scope of the present invention.
Claims
1. A method for preparing size-controllable nanoscale porous silicon, characterized in that: The following steps are involved: (1) Preparation of precursor: Ammonia water was added to the ethanol aqueous solution to adjust the pH, and tetraethyl orthosilicate was added after sufficient stirring to carry out stirring reaction. After the reaction, the precipitate was washed with deionized water and freeze-dried to obtain Si particles of different sizes. x O y Precursor material A; (2) Si obtained in step (1) x O y Precursor material A was dispersed in anhydrous ethanol, a dispersant was added, and after ultrasonic dispersion, the reaction was stirred, and the precipitate was washed with deionized water to obtain Si x O y Precursor material B; (3) Si obtained in step (2) x O y Precursor material B was added to the activation solution and stirred. The precipitate was washed with deionized water until neutral and freeze-dried to obtain Si x O y Precursor material C; (4) Si obtained in step (3) x O y Precursor material C is mixed with a reducing agent and an inorganic salt, calcined and reduced under an inert atmosphere, and cooled to room temperature to obtain a solid mixture; (5) The solid mixture obtained in step (4) is etched with an acid, and a dispersant is added, and then washed with deionized water until it is neutral, and freeze-dried to obtain nano-scale porous silicon.
2. The method for preparing size-controllable nanoscale porous silicon according to claim 1, characterized in that: In step (2), the dispersant is at least one of polyethylene glycol, polyvinyl pyrrolidone and Tween@80.
3. The method for preparing size-controllable nanoscale porous silicon according to claim 1, characterized in that: In step (3), the surfactant is at least one of palladium chloride, copper sulfate, silver nitrate and stannous chloride.
4. The method for preparing size-controllable nanoscale porous silicon according to claim 1, characterized in that: In step (4), the reducing agent is at least one of magnesium powder, magnesium diboride, magnesium carbide and magnesium oxide.
5. The method for preparing size-controllable nanoscale porous silicon according to claim 1, characterized in that: In step (5), the acid is at least one of hydrochloric acid, nitric acid and acetic acid.
6. The method for preparing size-controllable nanoscale porous silicon according to claim 1, characterized in that: In step (5), the dispersant is at least one of polyethylene glycol, polyvinyl pyrrolidone and Tween@80.
7. The method for preparing size-controllable nanoscale porous silicon according to claim 1, characterized in that: In step (1), the volume ratio of tetraethyl orthosilicate to ammonia water is 1:(1-25), the volume ratio of ethanol to deionized water in the ethanol-water solvent is (4-20):1; the reaction temperature is 25-80°C, and the reaction time is 4-12h.
8. The method for preparing size-controllable nanoscale porous silicon according to claim 1, characterized in that: In step (2), the dispersant and Si x O y The mass ratio of the precursor material A is (0.5-2):1, the mass volume ratio of the dispersant to anhydrous ethanol is (1.5-1500) g: (10-1000) mL; and the stirring time after ultrasound is 6-12 h.
9. The method for preparing size-controllable nanoscale porous silicon according to claim 1, characterized in that: In step (3), the activator and Si x O y The mass ratio of the precursor material B is (0.01-0.5):1, the mass volume ratio of the activator to the ethanol aqueous solution is (0.04-2) g: (20-1000) mL; and the activation treatment time is 0.5-2 h.
10. The method for preparing size-controllable nanoscale porous silicon according to claim 1, characterized in that: In step (4), Si x O y The molar ratio of the precursor material C to the reducing agent is 1:(1-2.5), Si x O y The molar ratio of the precursor material C to the inorganic salt is 1:(1-10); the calcination reduction temperature is 500-900° C., and the calcination reduction time is 2-10 hours.
11. The method for preparing size-controllable nanoscale porous silicon according to claim 1, characterized in that: In step (5), the concentration of the acid is (0.1-10) mol / L; the temperature of the acid etching treatment is 25-65° C., and the time is 0.5-12 h.
Citation Information
Patent Citations
Preparation method of electrode material of lithium-sulfur battery
CN106602032A
Controllable preparation method of porous silicon material by using reducing agent
CN114044519A
Preparation method of nano silicon-carbon negative electrode material
CN114400327A
Preparation method of high-reactivity silicon nanoparticles with mesoporous structure
CN116177551A
Lithium ion batteries based on nanoporous silicon
WO2011156419A2