Method for preparing high-purity quartz sand from feldspar granite pegmatite

Through the crushing, calcination, wet ball milling and flotation process of feldspathic granite pegmatite, combined with the acid treatment method, the problem of shortage of high-purity quartz raw materials and backward processing technology in China was solved, and a high-purity grade of 4N7 was successfully prepared. Pure quartz sand meets the demand for localized supply of high-end products.

CN118754134APending Publication Date: 2024-10-11HEFEI WANQUAN NON METALLIC MINERAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410980003.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

There are few high-purity quartz raw material deposits in China, and existing processing technology cannot meet the demand for large-scale production of high-end products. As a result, high-purity quartz relies on foreign imports and there are supply risks.

Method used

Using feldspathic granite pegmatite crushing, calcination, wet ball milling, magnetic separation and flotation processes, combined with acid treatment, WQ-39 and W40 collectors are used for deep purification to prepare high-purity grade 4N7 Quartz sand.

Benefits of technology

It effectively improves the purity and yield of high-purity quartz, reduces the content of impurity elements, and realizes the localized supply of high-end high-purity quartz products to meet the needs of semiconductor, photovoltaic and other industries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754134A_ABST
    Figure CN118754134A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of quartz sand purification, in particular to a method for preparing high-purity quartz sand from feldspar granite pegmatite. The method comprises the following steps: crushing feldspar granite pegmatite to obtain small blocks of ores containing quartz, feldspar and mica; calcining the small ore blocks, immediately carrying out water quenching, and crushing to obtain ore with the particle size of less than 3mm; carrying out wet ball milling on the ore, and carrying out desliming and magnetic separation on ore pulp of less than 70 meshes to obtain magnetic separation quartz fine sand; and mixing the magnetic separation quartz fine sand with acid, adding a collecting agent, and carrying out flotation to obtain the quartz fine sand. The SiO2 content of the purified feldspar granite pegmatite type high-purity quartz ranges from 99.9959% to 99.9981%, and the purity grade of the purified feldspar granite pegmatite type high-purity quartz reaches 4N 5-8.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of quartz sand purification, in particular to a method for preparing high-purity quartz sand by utilizing feldspar granite pegmatite. Background Art

[0002] The strategic position of high purity quartz:

[0003] The high-purity quartz industry chain is related to the development of high-tech industries in various countries, so the processing and preparation technology and export of high-purity quartz have been strictly controlled. Due to the rapid expansion of emerging industries such as semiconductors, foreign monopoly companies have been controlling the price of high-purity quartz sand by reducing production, which seriously affects the supply stability of high-purity quartz terminal semiconductors and other application fields in China. Therefore, high-purity quartz raw material mines should be given enough attention.

[0004] Application of high purity quartz in emerging industries:

[0005] High-purity quartz has excellent chemical stability, high insulation withstand voltage and extremely low volume expansion coefficient. It has a wide range of applications and a wide variety of products. With the rapid development of emerging industries, the demand for high-purity quartz continues to grow, especially in the fields of semiconductors, optical fiber communications and photovoltaics.

[0006] In the semiconductor field, the main types of quartz used in semiconductors include quartz crucibles, quartz ingots, quartz tubes, and quartz boats. Chip manufacturing mainly consists of four parts: single crystal growth, wafer processing and manufacturing, integrated circuit wafer production, and post-packaging. Single crystal growth requires quartz crucibles and quartz devices. A large amount of auxiliary quartz glass is required in the etching, diffusion, oxidation, annealing and other steps of the wafer processing part, such as quartz sheets, quartz rings, quartz boats and other high-purity quartz products. The diffusion step is to diffuse elements such as boron and phosphorus into silicon wafers in a quartz furnace tube at about 1000°C.

[0007] In the photovoltaic industry, quartz crucibles are an indispensable and important supporting material and a key component of photovoltaic single crystal furnaces. As consumable vessels, they can support solar energy and semiconductor users to continuously pull large-diameter single crystal silicon under high temperature conditions. They are used to hold molten silicon and make crystal rods required for subsequent processes. In the production of single crystal silicon, quartz crucibles are disposable key materials for molten silicon and crystal growth, which have a direct impact on the production cost and product output quality of single crystal silicon. Quartz crucibles have the advantages of high purity, strong temperature resistance, large size, high precision, good thermal insulation, energy saving, and stable quality. They are increasingly used in the fields of solar photovoltaic cell manufacturing.

[0008] High-purity quartz raw materials are relatively scarce:

[0009] The global high-purity quartz raw material deposits are mainly distributed in the United States, Canada, Norway, Australia, Russia, China, Mauritania and Brazil. Among them, the Spruce Pine mine in the United States is a world-recognized high-quality quartz deposit with the advantages of large scale, few fluid impurities and stable ore quality. From the perspective of raw ore, although my country is rich in quartz resources, most of them can only be used as bulk siliceous raw materials, and the raw materials for the production of high-purity quartz are scarce. There are few raw material deposits that can be used to produce high-purity quartz in my country, mainly distributed in Donghai, Jiangsu, Qichun, Hubei, Jingde, Anhui and Taihu. Among them, the quartz mine in Donghai, Jiangsu is the best quality, and the SiO2 mass fractions of the Lingqiu Mountain Quartz Mine in Qichun, Hubei and the Longchuanmai Quartz Mine in Banshu Township, Jingde, Anhui are 99.35% and 99.01% respectively, both of which have the potential to become high-purity quartz raw materials. However, my country does not have detailed standards for the exploration of vein quartz ores for high-purity quartz, and vein quartz is mostly distributed in vein-like and chicken-coop-like shapes, the deposits are small in scale, and the ore quality is unstable. Only a small number of these vein quartz deposits may be able to produce high-purity quartz sand suitable for the semiconductor industry and chip manufacturing industry, which is difficult to meet the needs of large-scale production of high-end high-purity quartz products. It is urgent to find new types of resources with large ore scale and stable ore quality.

[0010] There is a gap between high-purity quartz sand processing technology and foreign countries:

[0011] In recent years, my country's high-purity quartz market has developed rapidly, and a lot of work has been done in the research of high-purity quartz processing technology. It has the capacity to mass-produce 4N high-purity quartz mid-end products. Jiangsu Pacific Quartz Co., Ltd. is in a leading position in China in terms of high-purity quartz purification technology and product quality, accounting for 70% to 80% of domestic production. But overall, the gap between the international advanced level is still large, and high-purity quartz products still cannot meet the development needs. High-purity quartz of 4N8 and above still needs to be imported from abroad. In general, high-purity quartz is an important support for emerging industries. The rise of emerging industries requires a large amount of high-value-added raw materials, high-purity quartz, but China's current high-purity quartz is far from meeting the needs. As a major consumer of quartz, my country can be self-sufficient in low-value-added mid- and low-end quartz products, but high-end quartz products and high-purity quartz raw materials mainly rely on imports from the United States and Norway, which poses a large risk factor.

[0012] China currently has no statistics on the reserves of high-purity quartz raw material ore. In the past few years, the domestic production of high-purity quartz sand mainly used crystal resources and vein quartz resources. As crystal resources are close to exhaustion (the resource volume is only 6,900 tons), vein quartz has become the main raw material for high-purity quartz processing and production. The proportion of domestic vein quartz that can be processed into high-purity quartz products is extremely low. The most famous one is the Lingqiushan Mine in Qichun County, Hubei Province. The deposit was discovered in the 1970s and has a controlled reserve of 3.874 million tons. At present, it is open-pit mining, and the designed mining scale is to mine 15,000 tons of ore per year. (2) Global important high-purity quartz production enterprises From a global perspective, the main upstream high-purity quartz production enterprises are: The development and application of high-purity quartz raw material mines of pegmatite granite in the region has been developed, and high-purity quartz series products such as IOTA-STD (standard grade), IOTA-4, IOTA-6, and IOTA-8 are available. The quartz is naturally pure, with few inclusions, low impurity elements, and low hydroxyl content. It is an ideal raw material for the production of high-purity and ultra-high-purity quartz. It has become an international standard, and its global high-purity quartz sand market share has an absolute monopoly advantage. The raw materials for the processed products of Norway TQC come from SprucePine and local quartz in Norway. The high-purity quartz products processed from quartz resources in the United States can meet the requirements of semiconductor sand and photovoltaic sand, while the Norwegian products are more suitable for the fields of optics and electric light sources. The company's output is about 15,000 tons. Jiangsu Pacific Quartz Co., Ltd., a leading enterprise in the national quartz materials industry, mainly relies on the processing and purification of imported high-purity quartz raw materials from vein quartz.

[0013] High-purity quartz is an indispensable and irreplaceable important functional material for industries such as semiconductors, photovoltaics, optical fibers, optics, and electric light sources. It is a strategic resource that is scarce in the world and in short supply in my country. Relevant data show that my country is the world's largest importer of high-purity quartz industrial raw materials, importing 144,500 tons of 4N grade and above high-purity quartz raw materials each year, accounting for about 70% of the world's total imports (205,400 tons). High-purity quartz raw materials mainly rely on imports from the United States. Therefore, it is urgent to accelerate the localization and independent supply of high-purity quartz resources. Summary of the invention

[0014] In order to solve the above problems, the present invention provides a method for preparing high-purity quartz sand using feldspar granite pegmatite. The method provided by the present invention can prepare high-end high-purity quartz products with a high purification grade of 4N7.

[0015] In order to achieve the above object, the present invention provides the following technical solutions:

[0016] The present invention provides a method for preparing high-purity quartz sand by using feldspar granite pegmatite, comprising the following steps:

[0017] 1) crushing the feldspar granite pegmatite to obtain small pieces of quartz, feldspar and mica ore;

[0018] 2) calcining the small pieces of quartz, feldspar and mica ore obtained in step 1), immediately quenching with water, and then crushing to obtain ore with a particle size of less than 3 mm;

[0019] 3) wet ball milling the ore obtained in step 2), desludging and magnetic separation of the ore pulp with a mesh size less than 70, and obtaining magnetically separated quartz concentrate;

[0020] 4) mixing the magnetically separated quartz concentrate obtained in step 3) with mixed acid, adding a collector and performing flotation to obtain high-purity quartz sand;

[0021] The collectors are WQ-39 collector and W40 collector;

[0022] The WQ-39 collector is composed of the following components in percentage by mass:

[0023] 0.065% octanedionitrile, 4.998% n-octadecylamine, 0.190% 3-cyclopropylaminopropionitrile, 89.074% N-(2-aminoethyl)-1,3-propylenediamine, 0.996% homopiperazine, 0.166% (3-aziridine-1-propyl)-hexylamine, 0.138% N-(3-aminopropyl)-1,4-butanediamine, 1.362% cyanuric acid, and 3.011% N-dichloroacetyltryptamine;

[0024] The W40 collector is composed of the following components in percentage by weight: 8.676% (1-methyl-nonadecyl)-benzene, 4.076% 10-phenyldecanoic acid, 1.299% (1-pentyloctyl)-benzene, 1.624% (1-butyloctyl)-benzene, 1.370% (1-propyl-heptadecyl)-benzene, 2.349% (1-ethyloctyl)-benzene, 3.745% (1-methyl-tridecyl)-benzene, 6.221% Methyl N-hydroxybenzoimidate, 3.344% 4-hydroxybutyric acid hydrazide, 1.939% tetradec-13-ene-11-yn-1-ol, 37.260% (Z)-9-octadecenoate, 15.567% (1-hexyltetradecyl)benzene, 3.210% 2-acetylamino-3-phenylpropionic acid, 3.819% (1-propyl-heptadecyl)-benzene, 5.501% oxo-p-tolyl-acetaldehyde oxime.

[0025] Preferably, in step 1), the feldspar granite pegmatite is crushed to a particle size of less than 30 mm.

[0026] Preferably, the calcination conditions in step 2) include: temperature of 950° C. and time of 1 h.

[0027] Preferably, the conditions for wet ball milling in step 3) include: the medium is steel balls with a particle size of 6 cm and a slurry concentration of 35%.

[0028] Preferably, the mixed acid in step 4) comprises hydrofluoric acid and sulfuric acid, and the mass ratio of the hydrofluoric acid to the sulfuric acid is 1:2.

[0029] Preferably, the mass ratio of the magnetically separated quartz concentrate to the mixed acid in step 4) is 30:1.

[0030] Preferably, the mass ratio of the magnetically separated quartz concentrate to the collector in step 4) is 150:4.75-5.25.

[0031] Preferably, the mass ratio of the WQ-39 collector to the W40 collector is 4.3-4.75:0.45-0.5.

[0032] Preferably, in step 4), the collector is added in 5 to 8 times with an interval of 30 minutes.

[0033] Preferably, the flotation time in step 4) is 2.5h-4h.

[0034] The mechanism of the present invention for preparing high-end high-purity quartz products with a high purification grade of 4N8 is:

[0035] The feldspar granite pegmatite type quartz resources are large in scale, with few impurities and stable quality. The main mineral components are quartz, potassium feldspar, plagioclase, muscovite and a small amount of biotite, and it has the advantages of low gas-liquid inclusion content.

[0036] The particle size of quartz particles is between 0.2 and 4 mm, and some quartz particles are wrapped inside feldspar. The content of impure particles containing fluid inclusions in quartz particles is relatively small. The requirements for the content of each impurity element after purification vary according to the different uses of the prepared high-purity quartz products. The overall requirement is that the content of impurity elements is as low as possible. The purification process of high-purity quartz mainly includes physical purification and chemical deep purification. Physical separation such as magnetic separation and flotation can almost remove all feldspar and mica minerals in the form of monomers, and obtain flotation quartz concentrate with a main impurity element content of 89.445 ppm, a decrease in impurity content of up to 54.66%, and SiO2: 99.9959% quartz sand. Among them, flotation is crucial, and feldspar and mica minerals must be thoroughly floated. To obtain higher purity quartz, chemical purification is required. Chemical deep purification mainly includes acid treatment, which mainly removes impurities that exist on the surface of quartz sand particles in the form of inclusions or embedded in the particles to obtain high-purity quartz sand.

[0037] The beneficial effects of the present invention are:

[0038] After comprehensive beneficiation and impurity removal, the total amount of impurities in the feldspar granite pegmatite is 29.208ppm, and the SiO2 content reaches 99.9971%. The results show that the test has basically met the main technical requirements, and the feldspar granite pegmatite type high-purity quartz has the potential to prepare high-end high-purity quartz products. The SiO2 content of the purified feldspar granite pegmatite type high-purity quartz ranges from 99.9959% to 99.9971%, and the product purity grade reaches 4N5~8. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required to be used in the embodiments are briefly introduced below.

[0040] Figure 1 Flow chart for preparing magnetically separated quartz concentrate;

[0041] Figure 2 This is a flotation process flow chart;

[0042] Figure 3 This is a microscope image of high-purity quartz sand;

[0043] Figure 4 This is a microscope image of high-purity quartz sand;

[0044] Figure 5 This is the process flow chart of high purity quartz sand production. DETAILED DESCRIPTION

[0045] The present invention provides a method for preparing high-purity quartz sand by using feldspar granite pegmatite, comprising the following steps:

[0046] 1) Crushing the feldspar granite pegmatite and selecting small pieces of quartz, feldspar and mica ores;

[0047] 2) calcining the small pieces of quartz, feldspar and mica ore obtained in step 1), immediately quenching with water, and then crushing to obtain ore with a particle size of less than 3 mm;

[0048] 3) wet ball milling the ore obtained in step 2), desludging and magnetic separation of the ore pulp with a mesh size less than 70, and obtaining magnetically separated quartz concentrate;

[0049] 4) mixing the magnetically separated quartz concentrate obtained in step 3) with mixed acid, adding a collector and performing flotation to obtain high-purity quartz sand;

[0050] The collectors are WQ-39 collector and W40 collector;

[0051] The WQ-39 collector is composed of the following components in percentage by mass:

[0052] 0.065% octanedionitrile, 4.998% n-octadecylamine, 0.190% 3-cyclopropylaminopropionitrile, 89.074% N-(2-aminoethyl)-1,3-propylenediamine, 0.996% homopiperazine, 0.166% (3-aziridine-1-propyl)-hexylamine, 0.138% N-(3-aminopropyl)-1,4-butanediamine, 1.362% cyanuric acid, and 3.011% N-dichloroacetyltryptamine;

[0053] The W40 collector is composed of the following components in percentage by mass: 8.676% (1-methyl-nonadecyl)-benzene, 4.076% 10-phenyldecanoic acid, 1.299% (1-pentyloctyl)-benzene, 1.624% (1-butyloctyl)-benzene, 1.370% (1-propyl-heptadecyl)-benzene, 2.349% (1-ethyloctyl)-benzene, 3.745% (1-methyl-tridecyl)-benzene, 6.221% Methyl N-hydroxybenzoimidate, 3.344% 4-hydroxybutyric acid hydrazide, 1.939% tetradec-13-ene-11-yn-1-ol, 37.260% (Z)-9-octadecenoate, 15.567% (1-hexyltetradecyl)benzene, 3.210% 2-acetylamino-3-phenylpropionic acid, 3.819% (1-propyl-heptadecyl)-benzene, 5.501% oxo-p-tolyl-acetaldehyde oxime.

[0054] In the present invention, the W40 collector and the WQ-39 collector are from Hefei Wanquan Silicon Material Technology Co., Ltd.

[0055] The present invention crushes the feldspar granite pegmatite to obtain small pieces of ore containing quartz, feldspar and mica. The present invention preferably crushes the feldspar granite pegmatite to a particle size of less than 30 mm, and then color sorts the ore containing quartz, feldspar and mica. The present invention has no special limitation on the source of the feldspar granite pegmatite.

[0056] The present invention calcines the obtained small pieces of quartz, feldspar and mica ore, immediately quenches them with water, and then crushes them to obtain ore with a particle size of less than 3 mm. In the present invention, the calcination conditions preferably include: a temperature of 950° C. and a time of 1 hour. In the present invention, the immediate water quenching after calcination mainly utilizes the expansion and explosion of quartz crystal defects and gas-liquid inclusions to form a large number of cracks on the particle surface, expose interstitial impurities, and improve the impurity removal rate.

[0057] The present invention wet-ball-mills the obtained ore, deslimes and magnetically separates the slurry with a particle size less than 70 meshes, and obtains magnetically separated quartz concentrate. In the present invention, the conditions of the wet ball-milling preferably include: the medium is a steel ball with a particle size of 6 cm, and the slurry concentration is 35%. The present invention does not specifically limit the method of desliming the slurry, and those skilled in the art can use conventional methods. In the present invention, the magnetic separation preferably uses high-gradient magnetic separation, and the specific method is preferably: the magnetic field strength of the first high-gradient magnetic separation is 15000GS, and the magnetic field strength of the second high-gradient magnetic separation is 18000GS.

[0058] The invention mixes the obtained magnetically separated quartz concentrate with mixed acid, and then adds a collector to carry out flotation to obtain high-purity quartz sand; the collector is WQ-39 collector and W40 collector.

[0059] In the present invention, the mixed acid preferably includes hydrofluoric acid and sulfuric acid. In the present invention, the mass ratio of hydrofluoric acid to sulfuric acid is 1:12. In the present invention, the mass ratio of the magnetic quartz concentrate to the mixed acid is preferably 30:1, and the pickling is carried out for 20 hours at a temperature of 8°C. In the present invention, the mass ratio of the magnetic quartz concentrate to the collector is preferably 150:4.75-5.25. In the present invention, the mass ratio of the WQ-39 collector and the W40 collector is preferably 4.3-4.75:0.45-0.5. In the present invention, the collector is preferably added in 5 to 8 times, and the interval time is preferably 30 minutes. In the present invention, the flotation time is preferably 2.5-4h.

[0060] In order to further illustrate the present invention, the present invention is described in detail below in conjunction with embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0061] Example 1

[0062] 1. Mineral sample collection and preparation

[0063] 1.1 Sample collection

[0064] Feldspar granite pegmatite ore samples collected in mid-November 2023,

[0065] 1.2 Preparation of feldspar granite pegmatite samples

[0066] 1.2.1 Sample crushing

[0067] First, the large feldspar granite pegmatite ore is coarsely crushed to -30mm, and then small pieces of quartz ore with less intergrowths such as mica and feldspar and high quartz content are manually selected, accounting for about 20% of the original ore (percentage by mass), and the remaining about 80% of the small pieces of ore are mainly feldspar, mica and some fine quartz. Then the selected small pieces of quartz ore are calcined at 950℃ for 1h and quickly taken out and water quenched. The calcination and water quenching mainly use the expansion and bursting of quartz crystal defects and gas-liquid inclusions to form a large number of cracks on the particle surface, exposing interstitial impurities and improving the impurity removal rate. The small pieces of quartz ore dried at residual temperature are then medium-crushed and finely crushed to obtain -3mm ore samples.

[0068] 1.2.2 Grinding of samples

[0069] The grinding sample is -3mm finely crushed ore. The grinding equipment is a ball mill, and the medium is steel balls. The ore is wet ground under the condition of 35% mass percentage pulp concentration. The +70 mesh sample is returned for re-grinding. All the -70 mesh pulp is deslimed and then subjected to high gradient magnetic separation to obtain magnetically separated quartz concentrate, which accounts for about 16.38% of the original ore. The sample preparation process is shown in Figure 1 .

[0070] 2 Preparation of high purity quartz sand

[0071] 2.1 Flotation purification of high purity quartz process

[0072] In the flotation test, under the condition of acidic medium, the prepared magnetic quartz concentrate was put into the single tank flotation machine, and the two collectors "WQ-39" and "W40" were used for flotation test. The flotation was performed by adding collectors in stages, that is, after a single flotation scraping, the above method of adding collectors for flotation was repeated until no impurities floated out of the flotation agent, and the flotation was completed. See the flotation process for details. Figure 2 .

[0073] WQ-39 collector is composed of the following components in percentage by mass:

[0074] 0.065% octanedionitrile, 4.998% n-octadecylamine, 0.190% 3-cyclopropylaminopropionitrile, 89.074% N-(2-aminoethyl)-1,3-propylenediamine, 0.996% homopiperazine, 0.166% (3-aziridine-1-propyl)-hexylamine, 0.138% N-(3-aminopropyl)-1,4-butanediamine, 1.362% cyanuric acid, and 3.011% N-dichloroacetyltryptamine;

[0075] The W40 collector is composed of the following components in percentage by mass: 8.676% (1-methyl-nonadecyl)-benzene, 4.076% 10-phenyldecanoic acid, 1.299% (1-pentyloctyl)-benzene, 1.624% (1-butyloctyl)-benzene, 1.370% (1-propyl-heptadecyl)-benzene, 2.349% (1-ethyloctyl)-benzene, 3.745% (1-methyl-tridecyl)-benzene, 6.221% Methyl N-hydroxybenzoimidate, 3.344% 4-hydroxybutyric acid hydrazide, 1.939% tetradec-13-ene-11-yn-1-ol, 37.260% (Z)-9-octadecenoate, 15.567% (1-hexyltetradecyl)benzene, 3.210% 2-acetylamino-3-phenylpropionic acid, 3.819% (1-propyl-heptadecyl)-benzene, 5.501% oxo-p-tolyl-acetaldehyde oxime.

[0076] 3. Flotation test of feldspar granite pegmatite

[0077] 3.1 Flotation test of feldspar granite pegmatite

[0078] 3.1.1 Flotation test No. QCM-3218

[0079] The test used a 0.75L single-tank flotation machine, weighed 150g of magnetically separated quartz concentrate and put it into the tank, added 5g of mixed acid (HF+H2SO4, mass ratio of 1:2) to make the pH value reach 2.5, and then the flotation was divided into 5 times of average dosing flotation, a total of 4.3g of 100% concentration WQ-39 collector was added, a total of 0.45g of 100% concentration W40 frother was added, the cumulative flotation time was 4h, and the flotation quartz concentrate yield was 81.27%.

[0080] 3.1.2 Flotation test No. QCM-3228

[0081] The test used a 0.75L single tank flotation machine, weighed 150g of magnetic concentrated sand and put it into the tank, added 5g of mixed acid (HF+H2SO4, mass ratio of 1:2) to make the pH value reach 2.5, and then the flotation was divided into 8 times of average dosing flotation, 4.49g of 100% concentration WQ-39 collector was added cumulatively, 0.47g of 100% concentration W40 frother was added cumulatively, and the cumulative flotation time was about 2.5h. The yield of flotation quartz concentrated sand was 83.13%.

[0082] 3.1.3 Flotation test No. QCM-3229

[0083] The test used a 0.75L single tank flotation machine, weighed 150g of magnetic concentrated sand and put it into the tank, added 5g of mixed acid (HF+H2SO4, mass ratio of 1:2) to make the pH value reach 2.5, and then the flotation was divided into 8 times of average dosing flotation, 4.49g of 100% concentration WQ-39 collector was added cumulatively, 0.47g of 100% concentration W40 frother was added cumulatively, and the cumulative flotation time was about 4h. The yield of flotation quartz concentrated sand was 80.85%.

[0084] 3.1.4 Flotation test No. QCM-3231

[0085] The test used a 0.75L single tank flotation machine, weighed 150g of magnetic concentrated sand and put it into the tank, added 5g of mixed acid (HF+H2SO4, mass ratio of 1:2) to make the pH value reach 2.5, and then the flotation was divided into 8 times of average dosing flotation, 4.75g of 100% concentration WQ-39 collector was added cumulatively, 0.50g of 100% concentration W40 frother was added cumulatively, and the cumulative flotation time was about 4h. The yield of flotation quartz concentrated sand was 80.00%.

[0086] 3.2 Test results of quartz concentrate from feldspar granite pegmatite flotation

[0087] The contents of main impurity elements are shown in Table 1.

[0088] Table 1 Main impurity element content / (ppm)

[0089]

[0090] By comparing the main impurity content of each group of quartz concentrate in Table 1, it can be seen that:

[0091] (1) The main impurity element content of QCM-3218 flotation quartz concentrate is 89.445 ppm, which is significantly higher than the impurity content of the other three groups.

[0092] (2) The flotation schemes of QCM-3229 and QCM-3228 are the same, so only one group of QCM-3228 flotation quartz concentrate was tested. Theoretically, the indicators of the two groups of quartz concentrate can be considered consistent.

[0093] (3) Based on the above analysis, the impurity flotation of QCM-3218 is not thorough enough, and there is still room for improvement in flotation impurity removal. In the other three groups of flotation tests, the impurity flotation in quartz concentrate was relatively thorough, the total impurity content was basically close, and the flotation index was relatively stable.

[0094] (4) After various levels of physical impurity removal, the SiO2 content of QCM-3218 flotation quartz concentrate increased to 99.9911%; the SiO2 content of QCM-3228 flotation quartz concentrate increased to 99.9923%; the SiO2 content of QCM-3231 flotation quartz concentrate increased to 99.9920%; the above flotation quartz concentrate indicators all reached the high purification level 4N+. Therefore, by adopting the above physical impurity removal processes, the pegmatite can be used to produce high-end high-purity quartz products.

[0095] 3.3 Deep chemical treatment of quartz concentrate purified by flotation of feldspar granite pegmatite

[0096] In the flotation quartz sand concentrate obtained by various physical solutions for impurity removal in the previous series, the impurity content is mainly Al, K, Na, Ti, Ca, P, six impurity elements, which account for more than 97.62% of the total impurities and are the main targets of chemical purification. Deep chemical purification mainly adopts mixed acid leaching, using the mixed acid system to remove the impurities on the mineral surface and the impurities between the quartz crystals to the maximum extent.

[0097] The deep chemical purification process is as follows: after the flotation quartz concentrate is dehydrated, it is acid-leached in a reactor at 80°C for 20 hours using mixed acid, and the sample is taken out and the reagent is removed with pure water to obtain high-purity quartz concentrate with deep chemical purification. The contents of the main impurity elements in deep chemical purification are shown in Table 2.

[0098] Table 2 Main impurity element content / (ppm)

[0099]

[0100] By comparing the main impurity contents of each group of high-purity quartz concentrate in Table 2, it can be seen that:

[0101] (1) The main impurity element content of QCM-3218-1 flotation quartz concentrate after acid washing is 40.558ppm, which is 54.66% lower than the main impurity element content of QCM-3218 flotation quartz concentrate before deep chemical purification, 89.445ppm, and SiO2: 99.9959%.

[0102] (2) QCM-3230 high-purity quartz concentrate is obtained by deep chemical purification of QCM-3229 flotation quartz concentrate. The main impurity element content is 29.208ppm, which is 61.83% lower than the main impurity element content of QCM-3228 flotation quartz concentrate before deep chemical purification (76.528ppm). SiO2: 99.9971%.

[0103] (3) QCM-3334 high-purity quartz concentrate is further chemically purified from QCM-3230, with the impurity content reduced by up to 70.18%. The main impurity element content of QCM-3334 is 8.714ppm, and SiO2: 99.9981%.

[0104] (4) Based on the above comparative analysis, it can be seen that the flotation quartz concentrate is further purified by deep chemical purification to significantly remove impurities on the mineral surface and impurities between quartz crystals.

[0105] (5) After deep chemical purification and impurity removal, the impurity content of QCM-3334 high-purity quartz concentrate decreased by as much as 70.18%, the content of major impurity elements was 8.714ppm, SiO2: 99.9981%, and the high-purity quartz concentrate index reached high-purity grades 4N6-8. Therefore, on the basis of various levels of physical impurity removal combined with deep chemical purification and impurity removal technology, the pegmatite can be used to produce high-end high-purity quartz products with a high purification grade of 4N8.

[0106] 3.4 Characteristics of feldspar granite pegmatite under microscope after deep chemical purification of high-purity quartz sand

[0107] According to statistics, transparent quartz particles account for about 92% of the total quartz particles, and the particles with poor permeability are relatively few (less than 8%). The quartz purity is very high when observed under a microscope, which means that the content of gas-liquid inclusions is low. The characteristics of high-purity quartz sand under a microscope are shown in the figure below.

[0108] It can be concluded from the above embodiments that the high-purity quartz sand prepared by the present invention has SiO2≥99.995% and a total content of impurity elements≤25ug / g (25ppm).

[0109] After comprehensive beneficiation and impurity removal, the impurity element content of feldspar granite pegmatite is 8.714ppm, SiO2: 99.9981%. The results show that the test has basically met the main technical requirements, and the feldspar granite pegmatite type high-purity quartz is capable of preparing high-end high-purity quartz products. The SiO2 content of the purified feldspar granite pegmatite type high-purity quartz ranges from 99.9959% to 99.999%, and the product purity grade reaches 4N5~8.

[0110] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for preparing high-purity quartz sand using feldspar granite pegmatite, characterized in that: The following steps are involved: 1) crushing the feldspar granite pegmatite to obtain small pieces of quartz, feldspar and mica ore; 2) calcining the small pieces of quartz, feldspar and mica ore obtained in step 1), immediately quenching with water, and then crushing to obtain ore with a particle size of less than 3 mm; 3) wet ball milling the ore obtained in step 2), desludging and magnetic separation of the ore pulp with a mesh size less than 70, and obtaining magnetically separated quartz concentrate; 4) mixing the magnetically separated quartz concentrate obtained in step 3) with mixed acid, adding a collector and performing flotation to obtain high-purity quartz sand; The collectors are WQ-39 collector and W40 collector; The WQ-39 collector is composed of the following components in percentage by mass: 0.065% octanedionitrile, 4.998% n-octadecylamine, 0.190% 3-cyclopropylaminopropionitrile, 89.074% N-(2-aminoethyl)-1,3-propylenediamine, 0.996% homopiperazine, 0.166% (3-aziridine-1-propyl)-hexylamine, 0.138% N-(3-aminopropyl)-1,4-butanediamine, 1.362% cyanuric acid, and 3.011% N-dichloroacetyltryptamine; The W40 collector is composed of the following components in percentage by weight: 8.676% (1-methyl-nonadecyl)-benzene, 4.076% 10-phenyldecanoic acid, 1.299% (1-pentyloctyl)-benzene, 1.624% (1-butyloctyl)-benzene, 1.370% (1-propyl-heptadecyl)-benzene, 2.349% (1-ethyloctyl)-benzene, 3.745% (1-methyl-tridecyl)-benzene, 6.221% Methyl N-hydroxybenzoimidate, 3.344% 4-hydroxybutyric acid hydrazide, 1.939% tetradec-13-ene-11-yn-1-ol, 37.260% (Z)-9-octadecenoate, 15.567% (1-hexyltetradecyl)benzene, 3.210% 2-acetylamino-3-phenylpropionic acid, 3.819% (1-propyl-heptadecyl)-benzene, 5.501% oxo-p-tolyl-acetaldehyde oxime.

2. The method according to claim 1, characterized in that In the step 1), the feldspar granite pegmatite is crushed to a particle size of less than 30 mm.

3. The method according to claim 1, characterized in that The calcination conditions in step 2) include: temperature of 950° C. and time of 1 hour.

4. The method according to claim 1, characterized in that: The conditions of the wet ball milling in step 3) include: the medium is steel balls with a particle size of 6 cm and a slurry concentration of 35%.

5. The method according to claim 1, characterized in that The mixed acid in step 4) includes hydrofluoric acid and sulfuric acid, and the mass ratio of the hydrofluoric acid to the sulfuric acid is 1:

2.

6. The method according to claim 1, characterized in that In the step 4), the mass ratio of the magnetically separated quartz concentrate to the mixed acid is 30:

1.

7. The method according to claim 1, characterized in that In the step 4), the mass ratio of the magnetically separated quartz concentrate to the collector is 150:4.75-5.

25.

8. The method according to claim 1 or 7, characterized in that: The mass ratio of the WQ-39 collector to the W40 collector is 4.3-4.75:0.45-0.

5.

9. The method according to claim 1, characterized in that: In the step 4), the collector is added in 5 to 8 times with an interval of 30 minutes.

10. The method according to claim 1, characterized in that The flotation time in step 4) is 2.5-4 hours.