Refining method of lithium carbonate containing aluminum and fluorine

By removing aluminum and fluorine from aluminum-containing lithium fluoride carbonate through acidolysis and neutralization reaction, combined with the reaction of pure sodium carbonate, the problem of excessive aluminum and fluorine in the existing technology is solved, and the production of high-purity lithium carbonate and the extraction of active ingredients are realized. Recycle.

CN118754168APending Publication Date: 2024-10-11HOHHOT JIUYU RESOURCE RECYCLING TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411104275.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

In the hydrogenation method of the existing lithium carbonate refining method, when crude lithium carbonate contains aluminum and fluorine, aluminum enters the lithium bicarbonate solution during the hydrogenation process, and after heating and decomposition, the aluminum and fluorine in the sodium carbonate seriously exceed the standards, and qualified lithium carbonate cannot be produced. .

Method used

Aluminum-containing fluorine-containing lithium carbonate is dissolved using acidolysis method, the molar ratio of aluminum and fluorine is adjusted, aluminum and fluorine are removed through filtration and neutralization reaction, and then reacted with pure sodium carbonate to produce high-purity lithium carbonate.

Benefits of technology

Effectively remove aluminum and fluorine, improve the purity and recycling rate of lithium carbonate, solve the problem of excessive aluminum and fluorine in the existing technology, and realize the production of high-purity lithium carbonate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004990272120000011
    Figure HDA0004990272120000011
Patent Text Reader

Abstract

The invention discloses a refining method of lithium carbonate containing aluminum and fluorine. The refining method comprises the following steps: S1, dissolving; s2, adjusting the pH value; s3, filtering is carried out; s4, removing impurities; s5, pulping; and S6, separating and drying. The method has the advantages that aluminum in the aluminum-fluorine-containing crude lithium carbonate is reasonably utilized, after the crude lithium carbonate is dissolved with acid, part of fluorine is precipitated into cryolite (Na3AlF6), then the alkaline solution is added, excessive aluminum generates active aluminum hydroxide which has a very strong adsorption effect on fluorine, the fluorine removal effect is achieved, then filtering and washing are conducted, aluminum-fluorine residues are separated out, and the aluminum-fluorine-containing crude lithium carbonate is obtained. Afterwards, the aluminum and fluorine residues and a small amount of lithium carried in the aluminum and fluorine residues are recycled, lithium loss is avoided, and the recycling rate of effective components is increased. And mixing the low-sodium pure lithium solution from which the aluminum fluorine slag is separated with pure sodium carbonate to prepare lithium carbonate slurry, and sequentially filtering, washing, centrifugally dewatering and drying the lithium carbonate slurry to obtain a high-purity lithium carbonate product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The invention relates to the technical field of lithium carbonate refining, and in particular to a method for refining aluminum-fluoride-containing lithium carbonate. Background technology:

[0002] The solid waste produced by the electrolytic aluminum plant mainly includes five categories: overhaul slag, cathode carbon block, anode carbon block, shell surface block, and electrolyte. Among them, the overhaul slag is refractory bricks except for the main component Na3AlF6, the cathode carbon block and the anode carbon block are carbon powder except for the main component Na3AlF6, the shell surface block is mainly composed of Na3AlF6 and metal aluminum, and the electrolyte is mainly composed of Na3AlF6. It can be seen that the solid waste produced by the electrolytic plant contains a large amount of cryolite, which has a high utilization value. At present, our company has developed a process for alkaline calcium leaching to recover cryolite-containing solid waste from the electrolytic plant. It mainly uses alkaline calcium to leach the solid waste, and sodium, potassium, and lithium are leached into the alkaline leaching solution, while aluminum and fluorine are mainly left in the alkaline leaching slag, and a small amount of aluminum and fluorine remain in the alkaline leaching solution. Then the alkaline leaching solution and alkaline leaching slag are treated separately to recover the effective components therein. Among them, the alkaline leaching solution is mainly separated into sodium carbonate mother liquor and crude lithium carbonate through carbonization reaction and MVR evaporation concentration, wherein the crude lithium carbonate contains impurities such as aluminum hydroxide and sodium fluoride.

[0003] At present, the common method for refining crude lithium carbonate is hydrogenation, that is, first making crude lithium carbonate into a low-concentration slurry, then hydrogenating carbon dioxide in a carbonization tower, filtering at low temperature to obtain a lithium bicarbonate solution, and then heating the lithium bicarbonate solution to decarbonize to obtain lithium carbonate. This method can produce battery-grade lithium carbonate. If the above-mentioned aluminum- and fluorine-containing crude lithium carbonate is refined by hydrogenation, a small amount of aluminum enters the lithium bicarbonate solution during the hydrogenation process, and the solubility of fluorine is 0.01 mol / l. The sodium carbonate after heating and decomposition has the problem of seriously exceeding the aluminum and fluorine standards, and qualified lithium carbonate cannot be produced. Summary of the invention:

[0004] The object of the present invention is to provide a method for refining aluminum-fluoride-containing lithium carbonate.

[0005] The present invention is implemented by the following technical scheme: a method for refining lithium carbonate containing aluminum fluoride, which comprises the following steps:

[0006] S1: Dissolution

[0007] A dissolving acid is added to the aluminum-fluoride lithium carbonate for acid hydrolysis, the concentration of the dissolved solution is controlled at 10-30 g / L, the pH is controlled at 1-3, and the molar ratio of aluminum to fluorine in the crude lithium carbonate solution is adjusted to 1:6 so that the excess aluminum is 0.1-5 g / L, to obtain a crude lithium carbonate solution;

[0008] S2: Adjust pH

[0009] The crude lithium carbonate solution obtained in S1 is neutralized by adding sodium carbonate or sodium hydroxide, and the pH is adjusted to 5.0-8.0 to obtain a turbid lithium solution;

[0010] S3: Filtering

[0011] The turbid lithium solution prepared by S2 is filtered to remove the aluminum-fluorine slag to obtain a clear lithium solution;

[0012] S4: Impurity Removal

[0013] The clear lithium solution obtained in S3 is purified by impurities, and the soluble divalent and trivalent metals in the lithium solution are removed to obtain a low-sodium pure lithium solution;

[0014] S5: Pulping

[0015] The low sodium pure lithium solution obtained in S4 is mixed with the pure sodium carbonate solution, wherein the pure sodium carbonate solution and the low sodium pure lithium solution are calculated in a molar ratio of 1:1 and the sodium carbonate excess is 5-30 g / L, and the mixture is reacted at 60-100° C. for 30-300 min to obtain a lithium carbonate slurry;

[0016] S6: Separation and drying

[0017] The lithium carbonate slurry obtained in S5 is first filtered to obtain a solid phase material, and then the filtered solid phase material is washed with water to obtain a washing slurry, and then the washing slurry is subjected to solid-liquid separation, and finally the solid phase material separated by solid-liquid separation is dried to obtain a lithium carbonate product.

[0018] Furthermore, the dissolving acid in S1 is hydrochloric acid, sulfuric acid or nitric acid.

[0019] Furthermore, in S1, if the excess aluminum does not reach 0.1-5 g / L, aluminum chloride, aluminum sulfate or aluminum nitrate is added to adjust the excess aluminum content.

[0020] Furthermore, S3 uses a washing and filtering integrated machine for filtering, and the discharged washing water is sent back to S1 to mix with the solution in S1.

[0021] Furthermore, the pure sodium carbonate solution in S5 is prepared from industrial premium sodium carbonate, and the specific preparation process is: first, industrial premium sodium carbonate is added with water to prepare a sodium carbonate solution with a concentration of 300 g / l, and then the sodium carbonate solution is filtered to remove impurities, and finally, the filtrate after filtration and impurity removal is subjected to a chelating resin to remove soluble divalent and trivalent metals in the sodium carbonate solution to obtain a pure sodium carbonate solution.

[0022] Furthermore, the filtration in S6 is carried out in a washing and filtering integrated machine, and the washing water discharged from the washing and filtering integrated machine and the liquid phase separated by the solid-liquid separation are mixed with industrial high-grade sodium carbonate to prepare a sodium carbonate solution.

[0023] Further, in S6, an acid solution is added to the filtrate after filtering the lithium carbonate slurry to react with carbonate ions in the solution to release carbon dioxide to obtain a sodium salt solution, and then the sodium salt solution is evaporated and crystallized to obtain a sodium salt product.

[0024] Furthermore, in S6, the acid added to the filtrate after filtering the lithium carbonate slurry is hydrochloric acid, sulfuric acid or nitric acid.

[0025] The advantages of the present invention are as follows: the aluminum in the aluminum-fluoride-containing crude lithium carbonate is reasonably utilized. After the crude lithium carbonate is dissolved by acid, part of the fluorine is precipitated as cryolite (Na3AlF6). Then, an alkaline solution is added to make the excess aluminum generate active aluminum hydroxide, which has a strong adsorption effect on fluorine, thereby achieving the effect of removing fluorine. After that, the aluminum-fluoride slag is separated by filtration and washing, and then it can be sent back to the alkaline leaching process for recycling treatment to recover the aluminum-fluoride slag and a small amount of lithium carried therein, without lithium loss, thereby improving the recovery rate of effective components. After the low-sodium pure lithium solution of the separated aluminum-fluoride slag is mixed with pure sodium carbonate to obtain lithium carbonate slurry, the lithium carbonate slurry is filtered, washed, centrifuged and dehydrated, and dried in sequence to obtain a high-purity lithium carbonate product. Description of the drawings:

[0026] Figure 1 This is a schematic diagram of the overall structure of Example 4.

[0027] Dissolution tank 1, crude lithium carbonate feeding port 101, acid adding port 2, alkali adding port 3, first washing filter 4, first resin exchange column 5, pure sodium carbonate feeding pipe 6, lithium carbonate precipitation tank 7, second washing filter 8, pulping tank 9, centrifugal separator 10, dryer 11, lithium carbonate product discharge pipe 12, carbon dioxide discharge tank 13, acid liquid feeding pipe 14, MVR evaporation crystallizer 15, sodium salt product discharge pipe 16, configuration tank 17, filter 18, second resin exchange column 19. Specific implementation method:

[0028] In the description of the present invention, it should be noted that, if the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc. appear, the orientation or position relationship indicated is based on the orientation or position relationship shown in the drawings, which is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, if the terms "first", "second", "third" appear, they are only used for descriptive purposes and cannot be understood as indicating or implying relative importance.

[0029] Embodiment 1: A method for refining lithium carbonate containing aluminum fluoride, comprising the following steps:

[0030] S1: Dissolution

[0031] Aluminum-fluorinated lithium carbonate is added with a dissolving acid for acid hydrolysis, and the dissolving acid is hydrochloric acid. The concentration of the dissolved solution is controlled at 10 g / L, the pH is controlled at 1, and the molar ratio of aluminum and fluorine in the crude lithium carbonate solution is adjusted to 1:6, and there is an excess aluminum of 0.1 g / L to obtain a crude lithium carbonate solution; if the excess aluminum does not reach 0.1 g / L, aluminum chloride is added to adjust the excess aluminum content. The dissolution reaction is as follows:

[0032] Al(OH)3+HCL=AlCl3+2H2O

[0033] Li2CO3+2HCl=2LiCl+CO2↑+H2O

[0034] S2: Adjust pH

[0035] The crude lithium carbonate solution obtained in S1 is neutralized with sodium hydroxide and the pH is adjusted to 5.0 to obtain a turbid lithium solution containing aluminum hydroxide and cryolite; the reaction process is as follows:

[0036] AlCl3+6NaF=Na3AlF6↓+3NaCl

[0037] AlCl3+3NaOH=Al(OH)3↓+3NaCl

[0038] S3: Filtering

[0039] The turbid lithium solution prepared by S2 is filtered to filter out the aluminum fluoride slag mainly composed of aluminum hydroxide and cryolite to obtain a clear lithium solution;

[0040] S3 uses a washing and filtering integrated machine for filtration, and the discharged washing water is sent back to S1 to mix with the solution in S1.

[0041] S4: Impurity Removal

[0042] The clear lithium solution obtained in S3 is purified by chelating resin to remove soluble divalent and trivalent metals in the lithium solution to obtain a low-sodium pure lithium solution;

[0043] S5: Pulping

[0044] The low sodium pure lithium solution obtained in S4 is mixed with the pure sodium carbonate solution, and the pure sodium carbonate solution and the low sodium pure lithium solution are calculated according to a molar ratio of 1:1, and the sodium carbonate excess is 5 g / L, and the mixture is reacted at 60° C. for 30 min to obtain a lithium carbonate slurry; the reaction process is as follows:

[0045] 2LiCl+NaCO=2NaCl+LiCO↓

[0046] The pure sodium carbonate solution in S5 is prepared from industrial premium sodium carbonate. The specific preparation process is: first, industrial premium sodium carbonate is added with water to prepare a sodium carbonate solution with a concentration of 300 g / l, then the sodium carbonate solution is filtered to remove impurities, and finally, the filtrate after filtration and impurity removal is subjected to chelating resin to remove soluble divalent and trivalent metals in the sodium carbonate solution to obtain a pure sodium carbonate solution.

[0047] S6: Separation and drying

[0048] The lithium carbonate slurry obtained in S5 is first filtered to obtain a solid phase material, and then the filtered solid phase material is washed with water to obtain a washing slurry, and then the washing slurry is subjected to solid-liquid separation, and finally the solid phase material separated by solid-liquid separation is dried to obtain a lithium carbonate product.

[0049] The filtration in S6 is carried out in a washing and filtering integrated machine, and the washing water discharged from the washing and filtering integrated machine and the liquid phase separated by solid-liquid separation are mixed with industrial high-grade sodium carbonate to prepare a sodium carbonate solution.

[0050] In S6, hydrochloric acid is added to the filtrate after filtering the lithium carbonate slurry to react with carbonate ions in the solution to release carbon dioxide to obtain a sodium salt solution, and then the sodium salt solution is evaporated and crystallized to obtain a sodium salt product.

[0051] Embodiment 2: A method for refining lithium carbonate containing aluminum fluoride, comprising the following steps:

[0052] S1: Dissolution

[0053] Aluminum-fluorinated lithium carbonate is added with a dissolving acid for acid hydrolysis, wherein the dissolving acid is sulfuric acid. The concentration of the dissolved solution is controlled at 30 g / L, the pH is controlled at 3, and the molar ratio of aluminum to fluorine in the crude lithium carbonate solution is adjusted to 1:6 to obtain an excess aluminum of 5 g / L. If the excess aluminum does not reach 5 g / L, aluminum chloride, aluminum sulfate or aluminum nitrate is added to adjust the excess aluminum content, and finally a crude lithium carbonate solution is obtained; the reaction equation is as follows:

[0054] 2Al(OH)3+3H2SO4=Al2(SO4)3+6H2O

[0055] Li2CO3+H2SO4=2Li2SO4+CO2↑+H2O

[0056] S2: Adjust pH

[0057] The crude lithium carbonate solution obtained in S1 is neutralized with sodium carbonate and the pH is adjusted to 8.0 to obtain a turbid lithium solution containing aluminum hydroxide and cryolite; the reaction process is as follows:

[0058] Al2(SO4)3+6NaF=Na3AlF6↓+3Na2SO4

[0059] Al2(SO4)3+3Na2CO3+3H2O=3Na2SO4+2Al(OH)3↓+3CO2↑

[0060] S3: Filtering

[0061] The turbid lithium solution prepared by S2 is filtered to filter out the aluminum fluoride slag mainly composed of aluminum hydroxide and cryolite to obtain a clear lithium solution;

[0062] S3 uses a washing and filtering integrated machine for filtration, and the discharged washing water is sent back to S1 to mix with the solution in S1.

[0063] S4: Impurity Removal

[0064] The clear lithium solution obtained in S3 is purified by chelating resin to remove soluble divalent and trivalent metals in the lithium solution to obtain a low-sodium pure lithium solution;

[0065] S5: Pulping

[0066] The low sodium pure lithium solution obtained in S4 is mixed with the pure sodium carbonate solution, and the pure sodium carbonate solution and the low sodium pure lithium solution are calculated according to a molar ratio of 1:1, and the sodium carbonate excess is 30 g / L, and the mixture is reacted at 100° C. for 300 min to obtain a lithium carbonate slurry; the reaction process is as follows:

[0067] Li2SO4+Na2CO3=Na2SO4+Li2CO3↓

[0068] The pure sodium carbonate solution in S5 is prepared from industrial premium sodium carbonate. The specific preparation process is: first, industrial premium sodium carbonate is added with water to prepare a sodium carbonate solution with a concentration of 300 g / l, then the sodium carbonate solution is filtered to remove impurities, and finally, the filtrate after filtration and impurity removal is subjected to chelating resin to remove soluble divalent and trivalent metals in the sodium carbonate solution to obtain a pure sodium carbonate solution.

[0069] S6: Separation and drying

[0070] The lithium carbonate slurry obtained in S5 is first filtered to obtain a solid phase material, and then the filtered solid phase material is washed with water to obtain a washing slurry, and then the washing slurry is subjected to solid-liquid separation, and finally the solid phase material separated by solid-liquid separation is dried to obtain a lithium carbonate product.

[0071] The filtration in S6 is carried out in a washing and filtering integrated machine, and the washing water discharged from the washing and filtering integrated machine and the liquid phase separated by solid-liquid separation are mixed with industrial high-grade sodium carbonate to prepare a sodium carbonate solution.

[0072] In S6, sulfuric acid is added to the filtrate after filtering the lithium carbonate slurry to react with carbonate ions in the solution to release carbon dioxide to obtain a sodium salt solution, and then the sodium salt solution is evaporated and crystallized to obtain a sodium salt product.

[0073] Embodiment 3: A method for refining lithium carbonate containing aluminum fluoride, comprising the following steps:

[0074] S1: Dissolution

[0075] Aluminum-fluorinated lithium carbonate is added with a dissolving acid for acid hydrolysis, wherein the dissolving acid is nitric acid. The concentration of the dissolved solution is controlled at 20 g / L, the pH is controlled at 2, and the molar ratio of aluminum to fluorine in the crude lithium carbonate solution is adjusted to 1:6 to obtain an excess aluminum of 3 g / L. If the excess aluminum does not reach 3 g / L, aluminum chloride, aluminum sulfate or aluminum nitrate is added to adjust the excess aluminum content. Finally, a crude lithium carbonate solution is obtained, and the reaction equation is as follows:

[0076] Al(OH)3+3HNO3=Al(NO3)3+3H2O

[0077] Li2CO3+2HNO3=2LiNO3+CO2↑+H2O

[0078] S2: Adjust pH

[0079] The crude lithium carbonate solution obtained in S1 is neutralized with sodium hydroxide and the pH is adjusted to 6 to obtain a turbid lithium solution containing aluminum hydroxide and sodium fluoride; the reaction process is as follows:

[0080] Al(NO3)3+3NaOH=Al(OH)3↓+3NaNO3

[0081] S3: Filtering

[0082] The turbid lithium solution prepared by S2 is filtered to filter out the aluminum fluoride slag mainly composed of aluminum hydroxide and sodium fluoride to obtain a clear lithium solution;

[0083] S3 uses a washing and filtering integrated machine for filtration, and the discharged washing water is sent back to S1 to mix with the solution in S1.

[0084] S4: Impurity Removal

[0085] The clear lithium solution obtained in S3 is purified by chelating resin to remove soluble divalent and trivalent metals in the lithium solution to obtain a low-sodium pure lithium solution;

[0086] S5: Pulping

[0087] The low sodium pure lithium solution obtained in S4 is mixed with the pure sodium carbonate solution, and the pure sodium carbonate solution and the low sodium pure lithium solution are calculated according to a molar ratio of 1:1, and the sodium carbonate excess is 18 g / L, and the reaction is carried out at 80° C. for 150 min to obtain lithium carbonate slurry; the reaction process is as follows:

[0088] 2LiNO3+NaCO=2NaNO3+LiCO↓

[0089] The pure sodium carbonate solution in S5 is prepared from industrial premium sodium carbonate. The specific preparation process is: first, industrial premium sodium carbonate is added with water to prepare a sodium carbonate solution with a concentration of 300 g / l, then the sodium carbonate solution is filtered to remove impurities, and finally, the filtrate after filtration and impurity removal is subjected to chelating resin to remove soluble divalent and trivalent metals in the sodium carbonate solution to obtain a pure sodium carbonate solution.

[0090] S6: Separation and drying

[0091] The lithium carbonate slurry obtained in S5 is first filtered to obtain a solid phase material, and then the filtered solid phase material is washed with water to obtain a washing slurry, and then the washing slurry is subjected to solid-liquid separation, and finally the solid phase material separated by solid-liquid separation is dried to obtain a lithium carbonate product.

[0092] The filtration in S6 is carried out in a washing and filtering integrated machine, and the washing water discharged from the washing and filtering integrated machine and the liquid phase separated by solid-liquid separation are mixed with industrial high-grade sodium carbonate to prepare a sodium carbonate solution.

[0093] In S6, nitric acid is added to the filtrate after the lithium carbonate slurry is filtered to react with carbonate ions in the solution to release carbon dioxide to obtain a sodium salt solution, and then the sodium salt solution is evaporated and crystallized to obtain a sodium salt product.

[0094] Embodiment 4: The purification method of embodiment 1 to 3 adopts Figure 1 The refining system of aluminum fluoride lithium carbonate shown is completed, which includes a dissolution tank 1, an acid addition port 3, an alkali addition port 3, a first washing filter 4, a first resin exchange column 5, a pure sodium carbonate feed pipe 6, a lithium carbonate precipitation tank 7, a second washing filter 8, a pulping tank 9, a centrifuge 10, and a dryer 11.

[0095] The upper part of the dissolving tank 1 is connected with a crude lithium carbonate feeding port 101, an acid adding port 2, and an alkali adding port 3;

[0096] The outlet of the dissolving tank 1 is connected to the inlet of the first washing filter 4, and the filtrate outlet of the first washing filter 4 is connected to the inlet of the first resin exchange column 5;

[0097] The outlet of the first resin exchange column 5 and the pure sodium carbonate feeding pipe 6 are both connected to the inlet of the lithium carbonate precipitation tank 7, the outlet of the lithium carbonate precipitation tank 7 is connected to the inlet of the second washing filter 8, the slag discharge port of the second washing filter 8 is connected to the inlet of the pulping tank 9, the outlet of the pulping tank 9 is connected to the inlet of the centrifuge 10, the solid phase outlet of the centrifuge 10 is connected to the inlet of the dryer 11, and the outlet of the dryer 11 is connected to the lithium carbonate product discharge pipe 12.

[0098] The washing water outlet of the first washing filter 4 is communicated with the inlet of the dissolving tank 1 .

[0099] The filtrate outlet of the second washing filter 8 is connected to the inlet of the carbon dioxide exhaust tank 13, and the side of the carbon dioxide exhaust tank 13 is connected to the acid liquid feeding pipe 14; the outlet of the carbon dioxide exhaust tank 13 is connected to the inlet of the MVR evaporation crystallizer 15, and the crystal phase outlet of the MVR evaporation crystallizer 15 is connected to the sodium salt product discharge pipe 16.

[0100] The mother liquor outlet of the MVR evaporation crystallizer 15 is communicated with the inlet of the dissolving tank 1 .

[0101] It also includes a sodium carbonate solution preparation tank 17, a filter 18 and a second resin exchange column 19 which are connected in sequence. The outlet of the second resin exchange column 19 is connected to the inlet end of the pure sodium carbonate feeding pipe 6.

[0102] The washing water outlet of the second washing filter 8 and the washing water outlet of the centrifugal separator 10 are both connected to the inlet of the sodium carbonate solution preparation tank 17.

[0103] The refining method is:

[0104] S1: Dissolution

[0105] Adding a dissolving acid to the aluminum-fluoride lithium carbonate in a dissolving tank 1 for acid hydrolysis, controlling the concentration of the dissolved solution to 10-30 g / L, the pH to 1-3, and adjusting the molar ratio of aluminum to fluorine in the crude lithium carbonate solution to 1:6 so that there is an excess of aluminum of 0.1-5 g / L, thereby obtaining a crude lithium carbonate solution;

[0106] The dissolving acid in S1 is hydrochloric acid, sulfuric acid or nitric acid; if the excess aluminum does not reach 0.1-5 g / L, aluminum chloride, aluminum sulfate or aluminum nitrate is added to adjust the excess aluminum content.

[0107] S2: Adjust pH

[0108] The crude lithium carbonate solution obtained in S1 is neutralized by adding sodium carbonate or sodium hydroxide, and the pH is adjusted to 5.0-8.0 to obtain a turbid lithium solution;

[0109] S3: Filtering

[0110] The turbid lithium solution obtained in S2 is filtered in the first washing filter 4 to filter out the aluminum-fluorine slag and obtain a clear lithium solution; the discharged washing water is sent back to the dissolving tank to mix with the solution in S1.

[0111] S4: Impurity Removal

[0112] The clear lithium solution obtained in S3 is passed through a first resin exchange column 5 to remove impurities, thereby removing soluble divalent and trivalent metals in the lithium solution to obtain a low-sodium pure lithium solution;

[0113] S5: Pulping

[0114] The low sodium pure lithium solution obtained in S4 and the pure sodium carbonate solution are mixed in a lithium carbonate precipitation tank 7, the pure sodium carbonate solution and the low sodium pure lithium solution are calculated according to a molar ratio of 1:1, and the sodium carbonate excess is 5-30 g / L, and the reaction is carried out at 60-100° C. for 30-300 min to obtain a lithium carbonate slurry;

[0115] The pure sodium carbonate solution in S5 is prepared from industrial high-grade sodium carbonate. The specific preparation process is: first, water is added to industrial high-grade sodium carbonate in the preparation tank 17 to prepare a sodium carbonate solution with a concentration of 300g / l, and then the sodium carbonate solution is filtered through a filter 18 to remove impurities. Finally, the filtrate after filtering and removing impurities is passed through a second resin exchange column 19 to remove soluble divalent and trivalent metals in the sodium carbonate solution using a chelating resin to obtain a pure sodium carbonate solution.

[0116] S6: Separation and drying

[0117] The lithium carbonate slurry obtained in S5 is first filtered through a second washing filter 8 to obtain a solid phase material, and then the filtered solid phase material is washed with water in a slurry tank 9 to obtain a washing slurry, and then the washing slurry is separated into solid and liquid in a centrifuge 10, and finally the solid phase material separated from the solid and liquid is sent to a dryer 11 for drying to obtain a lithium carbonate product.

[0118] The wash water discharged from the second washing filter 8 and the liquid phase separated by the centrifugal separator 10 are sent back to the preparation tank 17 for mixing with industrial high-grade sodium carbonate to prepare a sodium carbonate solution.

[0119] In S6, an acid solution is added to the filtrate after the lithium carbonate slurry is filtered through the second washing filter 8 to react with carbonate ions in the solution to release carbon dioxide to obtain a sodium salt solution, and then the sodium salt solution is evaporated and crystallized in an MVR evaporation crystallizer 15 to obtain a sodium salt product.

[0120] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for refining aluminum-fluorinated lithium carbonate, characterized in that: It includes the following steps: S1: Dissolution A dissolving acid is added to the aluminum-fluoride lithium carbonate for acid hydrolysis, the concentration of the dissolved solution is controlled at 10-30 g / L, the pH is controlled at 1-3, and the molar ratio of aluminum to fluorine in the crude lithium carbonate solution is adjusted to 1:6 so that the excess aluminum is 0.1-5 g / L, to obtain a crude lithium carbonate solution; S2: Adjust pH The crude lithium carbonate solution obtained in S1 is neutralized by adding sodium carbonate or sodium hydroxide, and the pH is adjusted to 5.0-8.0 to obtain a turbid lithium solution; S3: Filtering The turbid lithium solution prepared by S2 is filtered to remove the aluminum-fluorine slag to obtain a clear lithium solution; S4: Impurity Removal The clear lithium solution obtained in S3 is purified by impurities, and the soluble divalent and trivalent metals in the lithium solution are removed to obtain a low-sodium pure lithium solution; S5: Pulping The low sodium pure lithium solution obtained in S4 is mixed with the pure sodium carbonate solution, wherein the pure sodium carbonate solution and the low sodium pure lithium solution are calculated in a molar ratio of 1:1 and the sodium carbonate excess is 5-30 g / L, and the mixture is reacted at 60-100° C. for 30-300 min to obtain a lithium carbonate slurry; S6: Separation and drying The lithium carbonate slurry obtained in S5 is first filtered to obtain a solid phase material, and then the filtered solid phase material is washed with water to obtain a washing slurry, and then the washing slurry is subjected to solid-liquid separation, and finally the solid phase material separated by solid-liquid separation is dried to obtain a lithium carbonate product.

2. A method for refining aluminum-fluorinated lithium carbonate according to claim 1, characterized in that: The dissolving acid in S1 is hydrochloric acid, sulfuric acid or nitric acid.

3. A method for refining aluminum-fluorinated lithium carbonate according to claim 1, characterized in that: In S1, if the excess aluminum does not reach 0.1-5 g / L, aluminum chloride, aluminum sulfate or aluminum nitrate is added to adjust the excess aluminum content.

4. A method for refining aluminum-fluorinated lithium carbonate according to claim 1, characterized in that: S3 uses a washing and filtering integrated machine for filtration, and the discharged washing water is sent back to S1 to mix with the solution in S1.

5. The method for refining aluminum-fluorinated lithium carbonate according to claim 1, characterized in that: The pure sodium carbonate solution in S5 is prepared from industrial premium sodium carbonate. The specific preparation process is: first, industrial premium sodium carbonate is added with water to prepare a sodium carbonate solution with a concentration of 300 g / l, then the sodium carbonate solution is filtered to remove impurities, and finally, the filtrate after filtration and impurity removal is subjected to chelating resin to remove soluble divalent and trivalent metals in the sodium carbonate solution to obtain a pure sodium carbonate solution.

6. A method for refining aluminum-fluorinated lithium carbonate according to claim 5, characterized in that: The filtration in S6 is carried out in a washing and filtering integrated machine, and the washing water discharged from the washing and filtering integrated machine and the liquid phase separated by solid-liquid separation are mixed with industrial high-grade sodium carbonate to prepare a sodium carbonate solution.

7. The method for refining aluminum-fluoride-containing lithium carbonate according to claim 1, characterized in that: In S6, an acid solution is added to the filtrate after filtering the lithium carbonate slurry to react with carbonate ions in the solution to release carbon dioxide to obtain a sodium salt solution, and then the sodium salt solution is evaporated and crystallized to obtain a sodium salt product.

8. A method for refining aluminum-fluoride-containing lithium carbonate according to claim 7, characterized in that: In S6, the acid added to the filtrate after filtering the lithium carbonate slurry is hydrochloric acid, sulfuric acid or nitric acid.