Compression-resistant tempered glass ceramic, cover plate glass, electronic equipment and glass device
By introducing zinc-aluminum spinel-magnesia-aluminum spinel solid solution and specific oxides into glass ceramics and performing chemical strengthening treatment, the problem of insufficient pressure resistance of existing glass ceramics in deep sea environments has been solved, and efficient anti-pressure properties have been achieved. Improved extrusion performance for deep sea applications.
Patent Information
- Application Number
- CN202410740146.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-07
AI Technical Summary
Existing glass ceramics have insufficient pressure resistance in water environments, especially deep sea environments, and are difficult to meet the high requirements of smart wearable devices and deep-sea manned detection devices.
Using zinc-aluminum spinel-magnesium-aluminum spinel solid solution as the main crystal phase, through chemical strengthening treatment, strengthened glass ceramics with a thickness greater than 0.7mm are prepared, and specific contents of Li2O and Na2O are added to form a surface compressive stress layer and internal tensile stress. , optimizing the oxide composition to improve extrusion resistance.
The extrusion resistance of reinforced glass-ceramics is significantly improved, allowing it to be more stably applied in deep-sea environments, and is suitable for transparent glass windows in smart wearable devices and deep-sea manned detection devices.
Smart Images

Figure CN118754440A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of microcrystalline glass, and in particular to a pressure-resistant strengthened glass ceramic, cover glass, electronic equipment and glass device. Background Art
[0002] With the popularization of smart electronic devices, people have higher and higher requirements for the performance of electronic devices. For example, more and more smart wearable devices are required to be used in water environments, such as swimming, diving, etc. When used in water environments, they need to meet certain pressure resistance requirements, because when used in water environments, in addition to dealing with possible destructive impacts, smart wearable devices are also subject to pressure from water. Only with sufficient compressive strength can it be ensured that the water pressure in deep water will not be too high to damage the structure of smart wearable devices.
[0003] As we all know, the deeper the depth, the greater the water pressure. In an underwater environment, the water pressure increases by 1 atmosphere for every 10 meters of depth. Therefore, the diving environment, especially the deep diving environment, will exert great pressure on smart wearable devices. Similarly, some devices used for deep-sea manned exploration have very high requirements for the pressure resistance of their transparent glass windows. At present, although the performance of glass ceramics on the market is generally better than that of ordinary glass, its pressure resistance still needs to be further improved. Summary of the invention
[0004] Spinel crystals have excellent properties such as high hardness and high modulus. Compared with the use of ordinary glass, chemical strengthening of glass ceramics with spinel crystal phase as the main crystal phase to prepare strengthened glass ceramics is more conducive to obtaining strengthened glass ceramic materials with excellent anti-extrusion properties.
[0005] The purpose of this application is to provide a reinforced glass ceramic with excellent anti-extrusion performance and spinel crystal phase as the main crystal phase. In order to achieve the above purpose, this application provides the following technical solutions:
[0006] In a first aspect, a reinforced glass ceramic is provided, wherein the reinforced glass ceramic is in a plate shape, and the thickness t of the reinforced glass ceramic is greater than 0.7 mm, preferably, the thickness t is not less than 0.8 mm, and more preferably, the thickness t is not less than 0.9 mm;
[0007] The reinforced glass ceramic comprises a main crystal phase of zinc aluminum spinel-magnesium aluminum spinel solid solution and a secondary crystal phase of zirconium oxide; the reinforced glass ceramic has a compressive stress layer on the surface and tensile stress inside;
[0008] In terms of the mass percentage of oxides, the composition at the center of the reinforced glass-ceramic includes Li2O and Na2O, and the mass percentage of Li2O is greater than 1.00%, preferably, the mass percentage of Li2O is greater than 1.30%, more preferably, the mass percentage of Li2O is greater than or equal to 1.50%, and the mass percentage of Na2O is greater than 1.00%, preferably, the mass percentage of Na2O is greater than 2.00%, more preferably, the mass percentage of Na2O is greater than 2.70%;
[0009] Calculated by mass percentage of oxides, the surface K2O mass percentage of the reinforced glass ceramic is 2.00% to 7.50%, preferably, the surface K2O mass percentage of the reinforced glass ceramic is 2.50% to 6.50%, and more preferably, the surface K2O mass percentage of the reinforced glass ceramic is 3.00% to 6.00%;
[0010] Calculated as a percentage by mass of oxides, the surface Na2O mass percentage of the reinforced glass-ceramic is less than or equal to 0.010%, preferably, the surface Na2O mass percentage of the reinforced glass-ceramic is less than or equal to 0.005%, and more preferably, the surface Na2O mass percentage of the reinforced glass-ceramic is less than or equal to 0.002%;
[0011] The strengthened glass ceramic satisfies: 5.00 μm ≤ DOL_K ≤ 20.00 μm, preferably, 5.50 μm ≤ DOL_K ≤ 18.00 μm, more preferably, 6.00 μm ≤ DOL_K ≤ 16.00 μm, wherein DOL_K is K measured from the main surface of the strengthened glass ceramic. + Diffusion depth.
[0012] It should be understood that the reinforced glass ceramic of the present application is made of glass ceramics through chemical strengthening treatment, and the composition of the center of the reinforced glass ceramics is the same or substantially the same as the composition of the glass ceramics. That is, in the present application, the composition of the glass ceramics used to prepare the reinforced glass ceramics also contains a certain amount of Li2O and Na2O.
[0013] In the present application, by making the glass ceramic contain a certain amount of Li2O and Na2O at the same time, not only can the fracture toughness of the glass ceramic be increased, making it less likely to break when squeezed or impacted, but it can also help improve the chemical strengthening effect of the glass ceramic.
[0014] The present application uses zinc-aluminum spinel-magnesium-aluminum spinel solid solution as the main crystal phase of glass ceramics, so that the glass ceramics obtain high intrinsic strength, and by chemically strengthening the glass ceramics with a thickness greater than 0.7 mm and containing a specific content of Li ions and Na ions, and making the surface composition of the obtained strengthened glass ceramics meet specific requirements, the compressive strength of the strengthened glass ceramics is significantly improved, and the strengthened glass ceramics obtain excellent anti-extrusion performance. In the present application, (Zn,Mg)Al2O4 is used to represent zinc-aluminum spinel-magnesium-aluminum spinel solid solution (or also called zinc-magnesium spinel solid solution, zinc spinel-magnesium spinel solid solution, zinc-magnesium-aluminum spinel solid solution).
[0015] As an optional embodiment, the surface K2O mass percentage of the strengthened glass-ceramic is 3.91%, 4.16%, 3.96%, 4.12%, 4.53%, 3.24%, 4.55%, 4.51%, 4.68%, 5.75%, 3.85%, 4.48%, 5.69%, 5.45%, 5.57% or 5.54%; and / or,
[0016] The DOL_K of the reinforced glass ceramic is 7.70 μm, 9.60 μm, 10.30 μm, 8.40 μm, 10.40 μm, 8.60 μm, 14.10 μm, 12.50 μm, 6.20μm, 9.80μm, 12.80μm, 9.10μm, 8.30μm, 8.80μm, 11.40μm, 10.60μm, 11.80μm or 11.70μm.
[0017] As an optional embodiment, the reinforced glass-ceramic satisfies: along the thickness direction of the reinforced glass-ceramic, the concentration of the K element decreases nonlinearly from the main surface of the reinforced glass-ceramic to the center of the reinforced glass-ceramic.
[0018] As an optional embodiment, the composition at the center of the reinforced glass-ceramic contains Al2O3 in an amount greater than or equal to 30.00% by mass, calculated as a percentage of oxide by mass.
[0019] In the present application, by controlling the mass percentage of Al2O3 in the glass ceramic to be greater than or equal to 30%, on the one hand, it is possible to ensure the precipitation of the desired content of the main crystal phase, so that the glass ceramic obtains a high intrinsic strength (or also called, inherent strength), and on the other hand, it is possible to make the glass phase also contain a certain amount of aluminum oxide, and the aluminum oxide present in the glass phase can enter the glass network structure as [AlO4] tetrahedrons, and form a unified grid with [SiO4], so that the degree of network connection is enhanced, and the strength and stability of the glass network structure are improved, thereby further improving the intrinsic strength of the glass ceramic. At the same time, the [AlO4] tetrahedron in the glass phase can appropriately expand the ion exchange channel, improve the chemical strengthening effect of the glass ceramic, and is more conducive to the preparation of strengthened glass ceramics with excellent mechanical strength properties.
[0020] As an optional embodiment, the composition at the center of the reinforced glass-ceramic includes ZrO2 in an amount greater than or equal to 3.00% by mass, calculated as a percentage of oxide by mass.
[0021] In the present application, by controlling the mass percentage of zirconium oxide in the glass ceramic to be greater than or equal to 3.00%, it is beneficial to improve the intrinsic strength of the glass ceramic and improve the surface stress level of the reinforced glass ceramic obtained therefrom. On the one hand, zirconium oxide, as a nucleating agent, will be dispersed in the glass phase in the form of nano-scale grains after heat treatment, which can increase the hardness of the glass ceramic, thereby effectively improving the crushing resistance of the glass ceramic. On the other hand, zirconium oxide exists in the glass phase in the form of cubes [ZrO8], which can enhance the inter-ionic force and make the glass structure more compact, thereby helping to improve the mechanical strength of the glass phase. At the same time, zirconium oxide can significantly increase the surface compressive stress formed by ion exchange, thereby improving the surface stress level of the reinforced glass ceramic obtained.
[0022] As an optional embodiment, the thickness t of the reinforced glass-ceramic is 0.85mm to 2.00mm, preferably, the thickness t is 0.90mm to 1.50mm; and / or, the reinforced glass-ceramic is 2D, 2.5D, 3D or special-shaped; and / or, the reinforced glass-ceramic is of equal thickness or unequal thickness. In the present application, when the thickness of the reinforced glass-ceramic is small, its compressive performance will be significantly reduced, and when the thickness is too large, on the one hand, it will lead to an increase in weight, which is not conducive to the realization of lightweight electronic equipment. On the other hand, too large a thickness will cause the transmittance of the glass-ceramic to decrease, making its transmittance performance worse. "Unequal thickness" means that the reinforced glass-ceramic includes at least two parts with different thicknesses.
[0023] As an optional embodiment, the composition at the center of the reinforced glass-ceramic, measured in percentage by mass of oxides, comprises:
[0024] SiO2: 25.00%~55.00%, Al2O3: 30.00%~55.00%, ZrO2: 3.00%~8.00%, MgO: 2.00%~5.00%, ZnO: 5.00%~15.00%, Na2O: 1.00%~10.0 0%, K2O: 0% to 5.00%, Li2O: 1.00% to 6.00%, CaO: 0% to 6.00%, B2O3: 0% to 10.00%, BaO: 0% to 10.00%, Y2O3: 0% to 6.00%, La2O3: 0% to 12.00%.
[0025] By adjusting and controlling the content range of each oxide component, it is helpful to ensure that the reinforced glass-ceramics satisfying the desired crystal phase structure is obtained, and it is also helpful to ensure that the reinforced glass-ceramics obtain excellent optical properties and high intrinsic strength.
[0026] As an optional embodiment, the composition at the center of the reinforced glass-ceramic, measured in percentage by mass of oxides, comprises:
[0027] The mass percentage of SiO2 is 30.00% to 42.00%, preferably, the mass percentage of SiO2 is 35.00% to 40.00%; and / or, the mass percentage of Al2O3 is 32.00% to 42.00%, preferably, the mass percentage of Al2O3 is 34.00% to 42.00%; and / or, the mass percentage of ZrO2 is 4.00% to 7.00%, preferably, the mass percentage of ZrO2 is 5.00% to 6.00% %; and / or, the mass percentage of MgO is 2.50% to 4.00%, preferably, the mass percentage of MgO is 2.50% to 3.50%; and / or, the mass percentage of ZnO is 9.00% to 13.00%, preferably, the mass percentage of ZnO is 9.00% to 11.00%; and / or, the mass percentage of Na2O is 1.00% to 8.00%, preferably, the mass percentage of Na2O is 2.00% to 6.00%; and / or, K The mass percentage of K2O is 0% to 3.00%, preferably, the mass percentage of K2O is 0% to 1.00%; and / or the mass percentage of Li2O is 1.00% to 4.00%, preferably, the mass percentage of Li2O is 2.00% to 3.00%; and / or the mass percentage of CaO is 0% to 3.00%, preferably, the mass percentage of CaO is 0% to 1.50%; and / or the mass percentage of B2O3 is 0% to 8.00%, preferably Select that the mass percentage of B2O3 is 0% to 4.00%; and / or the mass percentage of BaO is 0% to 7.00%, preferably, the mass percentage of BaO is 0% to 4.00%; and / or the mass percentage of Y2O3 is 0% to 4.00%, preferably, the mass percentage of Y2O3 is 0% to 2.00%; and / or the mass percentage of La2O3 is 0% to 5.00%, preferably, the mass percentage of La2O3 is 0% to 3.00%.
[0028] As an optional embodiment, the composition at the center of the reinforced glass-ceramic, measured in percentage by mass of oxides, comprises:
[0029] The mass percentage of SiO2 is 37.08%, 36.87%, 33.23%, 37.43%, 37.40%, 38.33%, 36.05%, 35.67%, 32.39%, 37.50%, 35.64%, 37.32% or 36.31%; and / or,
[0030] The mass percentage of Al2O3 is 35.83%, 36.98%, 36.27%, 37.52%, 36.60%, 37.07%, 34.84%, 34.55%, 35.88%, 38.63%, 36.23% or 35.10%; and / or,
[0031] The mass percentage of ZrO2 is 5.69%, 5.65%, 5.61%, 5.74%, 5.81%, 5.89%, 5.54%, 5.48%, 5.76%, 5.72%, 5.99% or 5.58%; and / or,
[0032] The mass percentage of MgO is 3.00%, 2.98%, 3.04%, 3.03%, 3.06%, 3.10%, 2.92%, 2.89%, 3.01%, 3.27% or 2.94%; and / or,
[0033] The mass percentage of ZnO is 10.77%, 10.71%, 10.55%, 10.87%, 11.01%, 11.15%, 10.46%, 10.37%, 12.50%, 10.82%, 11.33% or 10.54%; and / or,
[0034] The mass percentage of Na2O is 2.86%, 2.85%, 2.89%, 3.00%, 1.69%, 2.79%, 2.76%, 3.31%, 4.61%, 3.01% or 8.00%; and / or,
[0035] Preferably contains no K2O; and / or,
[0036] The mass percentage of Li2O is 2.35%, 1.55%, 1.50%, 1.77%, 1.60%, 1.62%, 2.28%, 2.27%, 2.24%, 1.60%, 1.57%, 2.85% or 1.53%; and / or,
[0037] The mass percentage of CaO is 0%, 0.75%, 1.15% or 0.92%; and / or,
[0038] The mass percentage of B2O3 is 0% or 7.07%; and / or,
[0039] The mass percentage of BaO is 2.42%, 2.41%, 6.94%, 0%, 2.35% or 2.32%; and / or,
[0040] The mass percentage of Y2O3 is 0%, 1.52% or 0.60%; and / or,
[0041] The mass percentage of La2O3 is 0%, 2.17% or 3.69%.
[0042] As an optional embodiment, in the composition at the center of the reinforced glass-ceramic, the mass percentage of Na2O [Na2O] and the mass percentage of Li2O [Li2O], calculated as the mass percentage of oxides, satisfy the following relationship: [Na2O] / [Li2O]=0.60-6.00, preferably 0.90-5.00, more preferably 1.00-3.00; and / or
[0043] In the composition at the center of the reinforced glass-ceramic, the mass percentage of Li2O [Li2O] and the mass percentage of SiO2 [SiO2] satisfy the following relationship: [Li2O] / [SiO2]=0.03~0.20, preferably 0.04~0.15, and more preferably 0.04~0.10.
[0044] On the basis of adjusting and controlling the content range of each oxide component, by adjusting and controlling the ratio between the oxide components, especially the mass percentage relationship between Na2O and Li2O and Li2O and SiO2, it is beneficial to improve the intrinsic strength and chemical strengthening effect of glass ceramics, and thus to obtain strengthened glass ceramics with excellent mechanical strength properties.
[0045] As an optional embodiment, in the reinforced glass-ceramic, the average crystal size does not exceed 20.0 nm, preferably 1.0 nm to 10.0 nm, more preferably 4.0 nm to 9.0 nm, more preferably 4.0 nm to 8.0 nm; and / or
[0046] In terms of mass percentage, the total content of the crystalline phase in the reinforced glass-ceramic is 25% to 60%, preferably 30% to 55%, and more preferably 40% to 50%.
[0047] By making the glass-ceramics satisfy the desired total crystalline content / crystallinity and appropriate average crystal size, it is beneficial for the glass-ceramics to maintain excellent optical properties while satisfying excellent mechanical strength properties and high intrinsic strength.
[0048] As an optional embodiment, in the reinforced glass-ceramic, the average crystal size is 5.0nm, 6.8nm, 6.4nm, 6.5nm, 8.1nm, 7.0nm, 6.1nm, 5.1nm or 6.2nm; and / or
[0049] In terms of mass percentage, the total crystalline content of the reinforced glass-ceramic is 48.69%, 45.11%, 49.52%, 47.85%, 54.07%, 51.56%, 45.49%, 44.77%, 52.28%, 35.52%, 48.75% or 44.33%.
[0050] As an optional embodiment, the reinforced glass ceramic is transparent in the visible light wavelength range. Preferably, at a thickness of 0.90 mm, for light of 550 nm wavelength, the transmittance of the reinforced glass ceramic is ≥ 85.00%, preferably ≥ 87.00%.
[0051] Strengthened glass ceramics that meet this transmittance can ensure good light transmittance and transparency, and are suitable for use in electronic device displays that have requirements for display effects.
[0052] As an optional embodiment, the Vickers hardness of the reinforced glass-ceramic is greater than or equal to 750 kgf / mm 2 Preferably, the Vickers hardness of the reinforced glass ceramic is greater than or equal to 790 kgf / mm 2 and / or,
[0053] The fracture toughness value of the reinforced glass ceramic is greater than or equal to 1.00 MPa·m 0.5 Preferably, the fracture toughness value of the reinforced glass ceramic is greater than or equal to 1.20 MPa·m 0.5 More preferably, the fracture toughness value of the reinforced glass ceramic is greater than or equal to 1.50 MPa·m 0.5 and / or,
[0054] The reinforced glass-ceramic has a |CT_AV| not exceeding 60.00 MPa, preferably a |CT_AV| of 4.00 MPa to 55.00 MPa, preferably a |CT_AV| of 4.00 MPa to 20.00 MPa, where |CT_AV| is the absolute value of the average tensile stress; and / or,
[0055] The reinforced glass-ceramic has a |CT_CV| of no more than 75.00 MPa, preferably a |CT_CV| of 5.00 MPa to 70.00 MPa, and preferably a |CT_CV| of 6.00 MPa to 25.00 MPa, where |CT_CV| is an absolute value of maximum tensile stress.
[0056] By making the reinforced glass ceramics have high Vickers hardness and fracture toughness, the reinforced glass ceramics are not easy to break when squeezed or impacted, which is conducive to improving the compressive resistance of the reinforced glass ceramics. By making the reinforced glass ceramics meet the appropriate stress structure, it is conducive to exerting the improvement effect of the stress structure on the mechanical strength performance, especially the improvement effect on the excellent compressive resistance to be achieved in this application.
[0057] As an optional embodiment, the Vickers hardness of the reinforced glass ceramic is 840 kgf / mm 2 、848kgf / mm 2 、855kgf / mm2 、879kgf / mm 2 、889kgf / mm 2 、836kgf / mm 2 、911kgf / mm 2 、897kgf / mm 2 、807kgf / mm 2 、894kgf / mm 2 、883kgf / mm 2 、873kgf / mm 2 、795kgf / mm 2 、863kgf / mm 2 、850kgf / mm 2 、856kgf / mm 2 or 860kgf / mm 2 and / or,
[0058] The fracture toughness value of the reinforced glass ceramic is 1.64 MPa·m 0.5 、1.65MPa·m 0.5 , 1.66MPa·m 0.5 , 1.70MPa·m 0.5 , 1.71MPa·m 0.5 , 1.63MPa·m 0.5 , 1.74MPa·m 0.5 , 1.72MPa·m 0.5 , 1.59MPa·m 0.5 , 1.69MPa·m 0.5 , 1.57MPa·m 0.5 or 1.67MPa·m 0.5 and / or,
[0059] The |CT_AV| of the strengthened glass-ceramic is 6.68 MPa, 5.85 MPa, 12.45 MPa, 5.45 MPa, 7.33 MPa, 7.79 MPa, 10.91 MPa, 14.64 MPa, 9.98 MPa, 6.25 MPa, 13.15 MPa, 8.58 MPa, 6.33 MPa, 7.91 MPa, 10.75 MPa, 12.77 MPa, 13.58 MPa, 9.47 MPa or 7.98 MPa; and / or,
[0060] The |CT_CV| of the strengthened glass-ceramic is 7.87 MPa, 6.96 MPa, 15.32 MPa, 6.84 MPa, 8.12 MPa, 9.01 MPa, 11.79 MPa, 17.92 MPa, 11.70 MPa, 7.76 MPa, 15.90 MPa, 9.45 MPa, 8.68 MPa, 9.13 MPa, 12.07 MPa, 14.12 MPa, 15.74 MPa, 10.75 MPa or 9.02 MPa.
[0061] As an optional implementation scheme, a 10mm diameter round-headed metal pressure rod is used to gradually apply load vertically downward at a rate of 10mm / min to squeeze the center of the main surface of the reinforced glass-ceramic to test the single-rod static pressure strength that the reinforced glass-ceramic can withstand. The single-rod static pressure strength that the reinforced glass-ceramic can withstand is greater than 800N.
[0062] As an optional embodiment, the reinforced glass ceramic has a fracture toughness of not less than 1.40 MPa·m 0.5 The glass ceramic is obtained by chemical strengthening treatment, preferably, the strengthened glass ceramic has a fracture toughness of not less than 1.40 MPa·m 0.5 The glass ceramic is obtained by a single-step chemical strengthening treatment, and more preferably, the fracture toughness is not less than 1.40 MPa·m 0.5 The glass ceramic is placed in a molten salt bath containing potassium salt with a mass percentage of potassium salt greater than or equal to 90%, and subjected to a single-step chemical strengthening treatment to obtain the strengthened glass ceramic.
[0063] In a second aspect, a cover glass is provided, wherein the cover glass is made of the tempered glass ceramic as described in any embodiment of the first aspect.
[0064] In a third aspect, an electronic device is provided, wherein the electronic device comprises the reinforced glass ceramic as described in any embodiment of the first aspect.
[0065] As an optional embodiment, the electronic device includes a housing assembled on the outside of the electronic device, and the housing includes the reinforced glass ceramic as described in any embodiment of the first aspect.
[0066] As an optional embodiment, the housing includes a display screen cover assembled on the front side of the electronic device, and the display screen cover includes the reinforced glass ceramic as described in any embodiment of the first aspect.
[0067] As an optional embodiment, the housing includes a back cover assembled on the back side of the electronic device, and the back cover includes the reinforced glass ceramic as described in any embodiment of the first aspect.
[0068] As an optional embodiment, the electronic device also includes a camera assembly located inside the housing, the housing includes a camera protection cover, the camera protection cover is covered on the camera assembly, and the camera protection cover includes the reinforced glass ceramic as described in any embodiment of the first aspect.
[0069] As an optional embodiment, the electronic device further includes a middle frame, and the middle frame includes the reinforced glass ceramic as described in any embodiment of the first aspect.
[0070] In some embodiments, the housing may be partially or entirely made of reinforced glass ceramics. The electronic device in the present application may be a display cover, a back cover, a camera protection cover, a middle frame, or one or more of which may be made of the reinforced glass ceramics described in any embodiment of the first aspect.
[0071] In a fourth aspect, a glass device is provided, wherein the glass device comprises the reinforced glass ceramic as described in any embodiment of the first aspect.
[0072] One or more of the above technical solutions provided by the present application, compared with the prior art, include the following advantages: the present application uses zinc aluminum spinel-magnesium aluminum spinel solid solution as the main crystal phase of glass ceramics, so that the glass ceramics obtain high intrinsic strength, and by chemically strengthening the glass ceramics with a thickness greater than 0.7 mm and containing a specific content of Li ions and Na ions, and making the surface composition of the obtained strengthened glass ceramics meet specific requirements, the compressive strength of the strengthened glass ceramics is significantly improved, so that the strengthened glass ceramics obtain excellent anti-extrusion performance. The strengthened glass ceramics are applied to electronic devices, so that the electronic devices can meet application environments with high requirements for compressive strength, such as being able to better match application requirements in water environments (such as deep sea environments), and can be applied to deep water environments, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0073] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0074] Figure 1 A comparison chart of XRD spectra of the glass ceramic and the reinforced glass ceramic provided in Example 1 of the present application;
[0075] Figure 2 This is a comparison chart of the transmittance curves of the glass ceramic and the reinforced glass ceramic provided in Example 1 of the present application;
[0076] Figure 3 A schematic diagram of the process of a single-rod static pressure strength test provided in an embodiment of the present application, wherein 30 is a pressure rod, 31 is a strengthened glass-ceramic sample / sample to be tested, and 32 is a fixture.
[0077] Figure 4 A schematic diagram of the structure of a fixture used for a single-rod static pressure strength test provided in an embodiment of the present application.
[0078] Figure 5 A schematic diagram of the cross-sectional structure of a fixture used for a single-rod static pressure strength test provided in an embodiment of the present application.
[0079] Figure 6 This is a morphological diagram of the reinforced glass-ceramic provided in an embodiment of the present application after being broken after a single-rod static pressure strength test.
[0080] Figure 7 This is a schematic diagram of the front structure of the electronic device mentioned in the implementation mode of this application.
[0081] Figure 8 This is a schematic diagram of the rear structure of the electronic device mentioned in the implementation mode of this application.
[0082] Fig. 9 The structure of the electronic device mentioned in the embodiment of this application is schematically shown. Figure 1 .
[0083] Fig.10 The structure of the electronic device mentioned in the embodiment of this application is schematically shown. Figure 2 .
[0084] Fig.11 Schematic diagram of the structure of the reinforced glass ceramic of the present invention; wherein t is the thickness of the glass, d is K + Diffusion depth DOL_K; 20 is the strengthened glass ceramic, 21 is the main surface of the strengthened glass ceramic, 22 is the tensile stress layer, and 23 is the compressive stress layer.
[0085] Figure numerals: 1-housing; 11-display screen cover; 12-back cover; 13-camera protection cover; 2-camera assembly; 3-middle frame; 4-display module. DETAILED DESCRIPTION
[0086] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0087] The endpoints and any values of the ranges disclosed in this article are not limited to the precise range or value, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Among them, the terms "optional" and "optional" all refer to including or not including (or may have or may not have). "And / or" as referred to herein is inclusive, for example, "A and / or B" means only A, or only B, or both A and B.
[0088] Explanation of terms and test methods:
[0089] In the present application, glass ceramics are a type of solid composite material that is prepared by targeted controlled heat treatment of substrate glass and contains both a glass phase and a crystal phase (also called microcrystalline phase, crystal phase, or crystalline phase). Glass ceramics are also called microcrystalline glass or crystallized glass.
[0090] In the present application, the strengthened glass ceramic refers to a solid composite material obtained by chemically strengthening the glass ceramic. It should be understood that during the chemical strengthening treatment, the alkali metal ions (such as potassium ions or sodium ions) with large ionic radius in the molten salt bath (or also called molten salt bath) will replace the alkali metal ions (such as sodium ions or lithium ions) with small ionic radius in the glass ceramic, thereby generating an exchange ion volume difference and generating compressive stress (or also called compressive stress) on the surface of the glass ceramic.
[0091] In the present application, substrate glass refers to glass that has not been subjected to nucleation treatment, crystallization treatment, and strengthening treatment, or is also called basic glass.
[0092] In the present application, the composition at the center of the strengthened glass-ceramic refers to the composition at the center of the depth or thickness of the strengthened glass-ceramic or near the center of the depth or thickness, that is, the composition of the region in the strengthened glass-ceramic where ion exchange has not been performed. It should be understood that the composition at the center of the strengthened glass-ceramic is the same or substantially the same as the composition of the glass-ceramic used to prepare the strengthened glass-ceramic but has not yet been chemically strengthened.
[0093] In the present application, the main crystalline phase (or also referred to as the main crystalline phase) refers to a crystalline phase having a higher weight content (or also referred to as weight percentage, mass percentage) than other crystalline phases present in the glass-ceramic.
[0094] In the present application, the total crystalline content refers to the percentage of the total mass of the crystalline phase or crystals in the glass-ceramic to the mass of the glass-ceramic, or is also called the crystallinity of the glass-ceramic.
[0095] In the present application, the main surface refers to the surface with the largest surface area, such as the upper surface or the lower surface of a horizontally placed glass ceramic sheet.
[0096] In the present application, the visible light wavelength range refers to 360nm to 740nm.
[0097] In the present application, when light of a certain wavelength is irradiated onto the main surface of the glass ceramic, the light will be reflected, absorbed and transmitted, wherein the ratio of the intensity of the transmitted part to the intensity of the incident light is the transmittance.
[0098] In the present application, nucleation treatment refers to forming stable crystal nuclei in the substrate glass by heat treatment; crystallization treatment refers to precipitating target crystals or crystalline phases in the substrate glass by heat treatment.
[0099] In this application, |CT_AV| refers to the absolute value of the average tensile stress, in MPa, specifically the absolute value of the average value of all tensile stresses in the tensile stress layer, obtained by testing with an SLP-2000 stress meter (or also known as a scattered light photoelastic stress meter).
[0100] In the present application, |CT_CV| refers to the absolute value of the maximum tensile stress, in MPa, specifically the absolute value of the maximum value of all tensile stresses in the tensile stress layer, obtained by testing with an SLP-2000 stress meter.
[0101] In this application, the test method of the aforementioned stress performance is as follows: using SLP 2000 stress meter to test |CT_CV| and |CT_AV| of the strengthened glass ceramic. The relevant parameter settings of the stress meter are: the light source wavelength is 518nm, the SOC (photoelastic coefficient) is set to 25.5 [(nm / cm) / MPa], the refractive index is set to 1.60, and the exposure time is 300μsec.
[0102] In this application, SOC, or photoelastic coefficient, mainly refers to the phenomenon of birefringence caused by anisotropy in transparent materials after being subjected to force. The value of residual stress inside the material can be obtained by measuring the photoelastic coefficient and birefringence.
[0103] In this application, DOL_K refers to K + Diffusion depth, or K + Diffusion layer depth, also known as K + The exchange depth refers to the depth measured from any main surface of the strengthened glass ceramic to the K measured by EPMA. + The depth at which the slope value of the concentration distribution curve (or also called the K element concentration distribution curve) is equal to 0.000 for the first time is obtained by Shimadzu electron probe EPMA-1720HT test. In this application, the K from the main surface to the inside of the strengthened glass-ceramic measured by EPMA is + In the concentration distribution curve, K +After ion exchange, it diffuses into the surface of glass ceramics, and with the increase of depth, K + The amount in the glass ceramic decreases, and finally reaches the depth where the slope of the curve is equal to 0.000 for the first time. + No longer spread inside.
[0104] Electron probe X-ray microanalysis (EPMA) test: Take the reinforced glass ceramic sample to be tested, mechanically grind one of the sides perpendicular to the main surface, remove the strengthening layer (wear removal is more than 500μm), and obtain a cross-sectional sample. The ground cross section is subjected to 30nm carbon spraying treatment, and the focused electron beam is selected along the ground cross section to perform line scanning along a straight line in the thickness direction to obtain the elemental composition and element concentration distribution in the thickness direction. The electron probe X-ray microanalysis instrument used in this application is Shimadzu's EPMA-1720HT, with an acceleration voltage of 15kV, a probe current of 100nA, a beam size of MIN, a step interval of 1μm, and a time of 1s / point; spectroscopic crystal RAP (Na Kα ray), spectroscopic crystal PET (K Kα ray); test elements: Na, K.
[0105] In the present application, Vickers hardness refers to a standard for expressing the hardness of materials proposed by Robert L. Smith and George E. Sandland of the United Kingdom at Vickers Ltd in 1921.
[0106] In this application, the test method of Vickers hardness is as follows: glass ceramics or reinforced glass ceramics are made into small discs with a diameter of 46mm and a thickness of 0.9mm, and a glass sample with a clean surface and no visible scratches, pits, cracks and other damage is selected as a test sample / sample, and then the Vickers hardness is measured using a Vickers hardness tester. The Vickers hardness tester used in this application test is a digital display small load Vickers hardness tester with model VTD405 of Beijing Kewei Technology Co., Ltd. Test conditions: load 300gf, load time 10s, the effectiveness of the indentation complies with the "GB / T37900-2019 Ultra-thin glass hardness and fracture toughness test method small load Vickers hardness indentation method" standard. Select 3 different positions on the surface of the same test sample / sample for measurement, and take the average of the 3 measurement results, which is recorded as the Vickers hardness result of the test sample / sample.
[0107] In this application, the thickness of the glass ceramic is obtained by micrometer testing. It should be understood that in the thickness direction, the degree of ion exchange changes gradually from the surface to the center, and the overall Na-K and / or Li-Na exchange amount generally does not exceed 1.5% of the total mass of the sample, and the difference in ion radius is at the pm level, so the expansion effect in the thickness direction is extremely slight, and it can be approximately considered that the thickness has basically not changed. That is, before and after chemical strengthening, the thickness of the glass ceramic changes very little, which can be basically ignored, and the thickness of the glass ceramic is basically the same as the thickness of the reinforced glass ceramic obtained therefrom.
[0108] In this application, the density test uses the electronic density balance SD-200L of ALFAMIRAGE of Japan to test the density of glass ceramics. The measurement principle is the Archimedean principle.
[0109] In this application, the size specifications of the glass ceramic sheet are tested using a two-dimensional measuring machine (instrument model: MiyuMY-YXCL-4030).
[0110] In this application, the crystal phase composition, total crystal phase content (or also called crystallinity), and average crystal size of the glass ceramics are confirmed by XRD testing, as follows:
[0111] (1) XRD test: The glass ceramic or reinforced glass ceramic of the present application is crushed and ground into a sample with a particle size of less than 75 μm, and the ground sample is tested using an X-ray diffractometer to obtain an XRD diffraction peak curve and XRD diffraction data. The X-ray diffractometer used in the present application is Shimadzu XRD-6100, the target material is copper, the test range is 2θ=10°-80°, the scanning speed is 2° / min, the operating voltage is 40 kV, and the operating current is 30 mA.
[0112] (2) Determination of crystalline phase: XRD diffraction data were analyzed using Jade software (JADE Standard 8.6) to determine the crystalline phase in the sample.
[0113] (3) Determination of total crystalline content (also known as crystallinity): The XRD test results (RAW format) were imported into the Jade software (JADE Standard 8.6) for fitting, and the total crystalline content of the sample was determined by calculating the formula (diffraction peak intensity / total intensity) × 100%.
[0114] (4) Determination of average crystal size: The average crystal size (or also called average grain size) of the sample can be calculated using the result data obtained from the XRD test according to the Scherrer formula D = Kλ / (βcosθ). Wherein, λ is the X-ray wavelength, λ = 0.154056nm, β is the half-height width of the diffraction peak, K = 0.89, and θ is the Bragg diffraction angle. Specifically, the RAW format file output by the XRD instrument is curve fitted in the Jade software (JADEStandard8.6), and Jade outputs a fitting report. According to the angle 2θ value and Peak FWHM value corresponding to each diffraction peak in the fitting report, the Peak FWHM value is converted into radians: β = (FWHM / 180×3.14), and the grain size of each diffraction peak is calculated by the Scherrer formula D = Kλ / (βcosθ) and then averaged to obtain the average crystal size in the sample.
[0115] In this application, with reference to the national standard "GB / T7962.12-2010 Test Method for Colorless Optical Glass Part 12: Spectral Transmittance", a haze meter is used to test the transmittance of glass ceramics. Specifically, the haze meter is used to test the transmittance of 5 pieces of glass ceramics from the same batch to light of different wavelengths. The average value of the transmittance of the 5 pieces of glass ceramics measured under 550nm wavelength light is taken and recorded as the transmittance result of the glass ceramics under 550nm wavelength light. The haze meter used in the test of this application is a Japanese Konica Minolta spectrophotometer CM-3600A, the light receiving optical system is transmission, the splitting method is a plane reflective grating, the wavelength range is 360nm~740nm, the wavelength spacing is 10nm, the illumination light source is a pulse xenon lamp × 4, the ambient temperature of the instrument is 24℃, and the air humidity is 40%.
[0116] In the present application, the test method of the surface Na2O mass percentage (or also called, surface Na2O concentration) of the strengthened glass-ceramic is as follows: the surface Na2O mass percentage is measured by an X-ray fluorescence spectrometer (XRF) to strengthen the glass-ceramic, and then the surface Na2O mass percentage is calculated, and the calculation method is: surface Na2O mass percentage = (surface Na element content × relative molecular mass of Na2O) / (relative atomic mass of Na element × 2). It should be understood that the surface Na element content = Na element mass / total element mass, and the total element mass = total oxide mass. The equipment model of the X-ray fluorescence spectrometer (XRF) used is Thermo Scientific ARL PERFORM'X, the target material is Rh (rhodium), the light tube voltage is 30kV, the current is 80mA, the collimator is 0.40, the crystal selects AxO3, the detector selects FPC, the test range is a circle with a diameter of 29mm, and the test method adopts the X_UQ method in the OXSAS analysis software.
[0117] In the present application, the test method of the surface K2O mass percentage (or also called surface K2O concentration) of the strengthened glass-ceramic is as follows: the surface K element content in the strengthened glass-ceramic is measured by X-ray fluorescence spectrometer (XRF), and then the surface K2O mass percentage is calculated, and the calculation method refers to the calculation of the surface Na2O mass percentage. The equipment model of the X-ray fluorescence spectrometer (XRF) used is Thermo Scientific ARL PERFORM'X, the target material is Rh (rhodium), the light tube voltage is 40kV, the current is 60mA, the collimator is 0.15, the crystal is LiF200, the detector is FPC, the test range is a circle with a diameter of 29mm, and the test method adopts the X_UQ method in the OXSAS analysis software.
[0118] In this application, the XRF instrument is tested using a standardless test, and the concentration of elements or their oxides with atomic numbers 6 and below in the strengthened glass-ceramics is not tested. The surface K2O mass percentage of strengthened glass-ceramics = K2O mass / total oxide mass, and the surface Na2O mass percentage of strengthened glass-ceramics = Na2O mass / total oxide mass, where oxides include SiO2, Al2O3, ZrO2, Na2O, K2O and other oxides that can be accurately tested by XRF, and do not include B2O3 and other oxides that cannot be accurately tested by XRF.
[0119] In this application, when using an XRF instrument for testing, the strengthened glass ceramic sheet is directly cut into a suitable size (such as 34mm*34mm), placed flat in a sample box, and the test aperture is covered before testing.
[0120] In this application, the fracture toughness test is carried out according to the standard "GB / T 37900-2019 Ultra-thin glass hardness and fracture toughness test method - small load Vickers hardness indentation method".
[0121] Specifically, the indentation is prepared in the same way as the Vickers hardness measurement, and the crack lengths 2C1 and 2C2 in the diagonal direction of the indentation are measured, and their maximum values cannot exceed the thickness of the glass. At least five effective indentation morphologies are measured on the surface of one sample, and the average value is calculated as the final result value of the sample.
[0122] Indentation fracture toughness calculation formula:
[0123]
[0124] IFR: Indentation fracture toughness, unit is MPa·m 0.5) ; E: elastic modulus of the specimen, in GPa; 2C1, 2C2: crack extension length in the diagonal direction of the indentation, in millimeter (mm); d1, d2: diagonal length of the indentation, in millimeter (mm); F: test load value, in Newton (N).
[0125] In this application, the single rod static pressure strength test: the strengthened glass ceramic sample to be tested is placed in a customized fixture (such as Figure 3 As shown in the figure), then place it on the bottom ring of the tensile testing machine (LT-850A), start the test software, and set the moving speed of the extrusion rod (rod diameter 10mm, ball head diameter 10mm) to 10mm / min. Click to start the test, and the extrusion rod will apply force to the center of the strengthened glass-ceramic sample to be tested at the set moving speed until the strengthened glass-ceramic sample is broken. The test process is as follows Figure 3 shown.
[0126] The test software will automatically read the force (N) when the reinforced glass ceramic sample is broken, and record it as the single rod static pressure strength it can withstand. Take 10 reinforced glass ceramic samples in the same state for testing, and take the average value of the test results as the single rod static pressure strength of the reinforced glass ceramic sample to be tested.
[0127] The custom fixture in this test method is a cylindrical fixture with a diameter of 65 mm and a height of 20 mm. The specific structure of the custom fixture is as follows: Figure 4 , Figure 5 , where Φ1=65mm, Φ2=46.02mm, Φ3=44mm, h1=20mm, h2=thickness of the reinforced glass ceramic sample to be tested, and h3=15mm. The height h2 of the sample placement groove in the custom fixture is equal to the thickness of the reinforced glass ceramic sample to be tested, and the reinforced glass ceramic sample to be tested can just fit into the fixture. The stepped blind hole set in the custom fixture for placing the sample for testing is coaxial with the custom fixture. The fixture is made of acrylic.
[0128] Although the performance of current glass ceramics is better than that of ordinary glass, their compressive properties still need to be further improved.
[0129] Without being restricted by any theory, spinel crystals have excellent properties such as high hardness and high modulus. Chemical strengthening of glass ceramics with spinel crystal phase as the main crystal phase is used to prepare strengthened glass ceramics. Compared with the use of ordinary glass, it is more conducive to obtaining strengthened glass ceramic materials with excellent anti-extrusion properties.
[0130] The general chemical formula of spinel crystal is AB2O4, where A is a divalent metal ion such as Zn, Fe or Mg with tetrahedral coordination, and B is an Al, Cr or Fe metal ion with octahedral coordination. Since Al-O, Mg-O and Zn-O can form strong ionic bonds, their structure is strong, hardness is high and chemical properties are stable. The Mohs hardness of spinel crystal is basically between 7 and 8, close to 8. Therefore, by controllably precipitating zinc spinel (also called zinc aluminum spinel) and / or magnesium spinel (also called magnesium aluminum spinel) and / or zinc magnesium spinel solid solution (Zn, Mg) Al2O4 in glass, spinel glass ceramics with good mechanical properties can be obtained in theory.
[0131] To this end, the present application uses glass ceramics containing spinel crystals that meet specific composition and structure to prepare reinforced glass ceramic materials with desired anti-extrusion properties. The glass ceramics used in the present application are rich in high-strength spinel crystals and have a high-strength glass phase structure. Through the synergistic cooperation of the crystal phase structure and the glass phase structure, the glass ceramics are given higher inherent strength or intrinsic strength. The present application chemically strengthens the glass ceramic so that its surface composition meets specific requirements, thereby giving the prepared reinforced glass ceramics a stress structure and stress level that achieves high compressive resistance, thereby obtaining reinforced glass ceramics with excellent anti-extrusion properties.
[0132] It can be understood that the "surface composition" in the present application can be the material composition or component distribution of the material composition on the surface of the substrate glass, glass ceramic or strengthened glass ceramic, and can also be the mass percentage of a certain component on the surface of the substrate glass, glass ceramic or strengthened glass ceramic, the molar percentage of a certain component, the mass percentage relationship between two or more material components, the mass content relationship between two or more material components, the molar content relationship between two or more material components, and a combination of the above items, as well as others. For example: the surface Na2O mass percentage of strengthened glass ceramics or the surface K2O mass percentage of strengthened glass ceramics, and another example: the surface Na2O mass percentage of strengthened glass ceramics and the surface K2O mass percentage of strengthened glass ceramics, and another example: the K2O mass percentage calculated from the main surface of strengthened glass ceramics. + (K element) Diffusion depth.
[0133] In some embodiments of the present application, a reinforced glass ceramic is provided, wherein the reinforced glass ceramic is in a plate shape, and the thickness t of the reinforced glass ceramic is greater than 0.7 mm, preferably, the thickness t is not less than 0.8 mm, and more preferably, the thickness t is not less than 0.9 mm;
[0134] The reinforced glass ceramic comprises a main crystal phase of zinc aluminum spinel-magnesium aluminum spinel solid solution and a secondary crystal phase of zirconium oxide; the reinforced glass ceramic has a compressive stress layer on the surface and tensile stress inside;
[0135] In terms of the mass percentage of oxides, the composition at the center of the reinforced glass-ceramic includes Li2O and Na2O, and the mass percentage of Li2O is greater than 1.00%, preferably, the mass percentage of Li2O is greater than 1.30%, more preferably, the mass percentage of Li2O is greater than or equal to 1.50%, and the mass percentage of Na2O is greater than 1.00%, preferably, the mass percentage of Na2O is greater than 2.00%, more preferably, the mass percentage of Na2O is greater than 2.70%;
[0136] The surface K2O mass percentage of the reinforced glass-ceramic is 2.00% to 7.50% by mass, preferably 2.50% to 6.50% by mass, and more preferably 3.00% to 6.00% by mass.
[0137] The surface Na2O mass percentage of the reinforced glass-ceramic is less than or equal to 0.010% by mass, preferably less than or equal to 0.005% by mass, and more preferably less than or equal to 0.002% by mass, as measured by XRF, in terms of the mass percentage of oxides.
[0138] The reinforced glass ceramics satisfy the following conditions as determined by EPMA: 5.00 μm ≤ DOL_K ≤ 20.00 μm, preferably 5.50 μm ≤ DOL_K ≤ 18.00 μm, more preferably 6.00 μm ≤ DOL_K ≤ 16.00 μm, wherein DOL_K is the K value calculated from the main surface of the reinforced glass ceramics. + Diffusion depth.
[0139] In the present application, by making the glass ceramic contain a certain amount of Li2O and Na2O at the same time, it is possible to increase the fracture toughness of the glass ceramic and improve the overall strength of the glass phase (or also called residual glass phase), making it less likely to break when squeezed or impacted, and at the same time, it is beneficial to improve the chemical strengthening effect of the glass ceramic.
[0140] The present application uses zinc-aluminum spinel-magnesium-aluminum spinel solid solution as the main crystalline phase of glass ceramics, so that the glass ceramics obtain high intrinsic strength, and by chemically strengthening the glass ceramics having a thickness greater than 0.7 mm and containing a specific content of Li ions and Na ions, and making the surface composition of the obtained strengthened glass ceramics meet specific requirements, the compressive strength of the strengthened glass ceramics is significantly improved, and the strengthened glass ceramics obtain excellent anti-extrusion performance. In the present application, (Zn, Mg)Al2O4 is used to represent zinc-aluminum spinel-magnesium-aluminum spinel solid solution (or also called zinc-magnesium spinel solid solution, zinc spinel-magnesium spinel solid solution, zinc-magnesium-aluminum spinel solid solution). The strengthened glass ceramics are applied to electronic devices, so that the electronic devices can meet application environments with high requirements for compressive strength, such as being able to better match application requirements in water environments (such as deep-sea environments), and can be applied to deep-water environments, etc.
[0141] In some embodiments, the surface K2O mass percentage of the strengthened glass-ceramic may be 3.20% to 5.80%, 3.80% to 5.60%, or 4.10% to 5.5%. In some embodiments, the surface K2O mass percentage of the strengthened glass-ceramic can be 2.00%, 2.50%, 3.00%, 3.50%, 4.00%, 4.50%, 5.00%, 5.50%, 6.00%, 6.50%, 7.00%, 7.50%, 3.91%, 4.16%, 3.96%, 4.12%, 4.53%, 3.24%, 4.55%, 4.51%, 4.68%, 5.75%, 3.85%, 4.48%, 5.69%, 5.45%, 5.57% or 5.54%, or can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the strengthened glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the strengthened glass-ceramic with the desired performance of the present application can be obtained.
[0142] In some embodiments, the surface Na2O mass percentage of the strengthened glass-ceramic can be 0.000%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009% or 0.010%, or can be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the strengthened glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the strengthened glass-ceramic with the desired performance of the present application can be obtained.
[0143] In some embodiments, the DOL_K of the strengthened glass-ceramic may satisfy: 10.00 μm≤DOL_K≤17.00 μm, 5.00 μm≤DOL_K≤10.00 μm, 17.00 μm≤DOL_K≤20.00 μm, 11.00 μm≤DOL_K≤15.00 μm, 12.00 μm≤DOL_K≤14.00 μm, or 12.00 μm≤DOL_K≤13.00 μm. In some embodiments, the DOL_K of the strengthened glass-ceramic can be 5.00 μm, 5.50 μm, 6.00 μm, 6.50 μm, 7.00 μm, 7.50 μm, 8.00 μm, 8.50 μm, 9.00 μm, 9.50 μm, 10.00 μm, 10.50 μm, 11.00 μm, 11.50 μm, 12.00 μm, 12.50 μm, 13.00 μm, 13.50 μm, 14.00 μm, 14.50 μm, 15.00 μm, 15.50 μm, 16.00 μm, 16.50 μm, 17.00 μm, 17.50 μm, 18.00 μm, 18. 18.50μm, 19.00μm, 19.50μm, 20.00μm, 7.70μm, 9.60μm, 10.30μm, 8.40μm, 10.40μm, 8.60μm, 14.10μm, 12.50μm, 6.20μm, 9.80μm, 12.80μm, 9.10μm, 8.30μm, 8.80μm, 11.40μm, 12.80μm, 10.60μm, 11.80μm or 11.70μm, or it can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained.
[0144] In some embodiments, the thickness t of the reinforced glass ceramic can be not less than 0.95 mm, not less than 1.00 mm, not less than 1.05 mm, 0.85 mm to 2.00 mm, or 0.90 mm to 1.50 mm. The thickness of the reinforced glass ceramic is positively correlated with its anti-extrusion performance. The thicker the thickness of the reinforced glass ceramic, the better its anti-extrusion performance. When the thickness of the reinforced glass ceramic is small, its compression resistance will be significantly reduced. By controlling the thickness of the reinforced glass ceramic to be not less than 0.70 mm, it is beneficial to make the reinforced glass ceramic have better anti-extrusion performance. When the thickness of the reinforced glass ceramic is too large, on the one hand, it will lead to an increase in weight, which is not conducive to achieving lightweight electronic equipment. On the other hand, too large a thickness will cause the transmittance of the glass ceramic to decrease, making its transmittance performance worse. In some embodiments, the thickness of the reinforced glass-ceramic of the present application can be 0.80 mm, 0.85 mm, 0.90 mm, 1.00 mm, 1.10 mm, 1.20 mm, 1.30 mm, 1.40 mm or 1.50 mm, or can be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained.
[0145] In some embodiments of the present application, the reinforced glass ceramic or the glass ceramic used to prepare the reinforced glass ceramic is 2D, 2.5D, 3D or a special shape, that is, the glass ceramic can be a 2D, 2.5D, 3D or a special shape product, and the reinforced glass ceramic can also be a 2D, 2.5D, 3D or a special shape product; and / or, the reinforced glass ceramic or the glass ceramic used to prepare the reinforced glass ceramic is of equal thickness or unequal thickness. "Unequal thickness" means that the reinforced glass ceramic or the glass ceramic used to prepare the reinforced glass ceramic includes at least two parts with different thicknesses.
[0146] In some embodiments of the present application, the reinforced glass-ceramic satisfies: when tested by EPMA, along the thickness direction of the reinforced glass-ceramic, the concentration of K element decreases nonlinearly from the main surface of the reinforced glass-ceramic to the center of the reinforced glass-ceramic. In the present application, the K from the main surface to the inside of the reinforced glass-ceramic measured by EPMA is + In the concentration distribution curve, K + After ion exchange, it diffuses into the surface of glass ceramics, and with the increase of depth, K + The amount in the glass ceramic decreases, and finally reaches the depth where the slope of the curve is equal to 0.000 for the first time. + No longer spread inside.
[0147] It should be understood that the reinforced glass ceramic of the present application is made of glass ceramics subjected to chemical strengthening treatment, and the composition at the center of the reinforced glass ceramic is the same or substantially the same as the composition of the glass ceramic. Compared with the glass ceramic before the chemical strengthening treatment (chemical strengthening treatment will perform ion exchange), the composition at the surface of the glass ceramic product after the chemical strengthening treatment may be different from the composition of the glass ceramic before the chemical strengthening treatment. This is because when the chemical strengthening treatment is performed, a type of alkali metal ion (for example, Li ions) at the surface of the glass ceramic in the newly formed glass ceramic is + Or Na + ) are replaced by larger alkali metal ions (e.g., Na + or K + ) is replaced. However, in an embodiment, the glass composition and phase assembly at or near the depth or thickness center of the glass-ceramic product will still have the composition and phase assembly of the newly formed glass-ceramic. That is, in the present application, the composition (e.g., the composition of the tensile stress layer) and phase assembly at the center of the strengthened glass-ceramic are the same or substantially the same as those of the glass-ceramic that has not been chemically strengthened.
[0148] Meanwhile, in the present application, the glass ceramics used to prepare the reinforced glass ceramics can be obtained by heat treating the substrate glass, and the composition of the substrate glass is the same or substantially the same as that of the glass ceramics in terms of the mass percentage of oxides.
[0149] In some embodiments of the present application, the composition at the center of the reinforced glass-ceramic or the composition of the glass ceramic used to prepare the reinforced glass-ceramic or the composition of the substrate glass contains Al2O3 greater than or equal to 30.00% by mass, measured as a percentage of oxide by mass.
[0150] In the present application, by controlling the mass percentage of Al2O3 in the glass ceramic to be greater than or equal to 30%, on the one hand, it is possible to ensure the precipitation of the desired content of the main crystal phase, so that the glass ceramic obtains a high intrinsic strength (or also called, inherent strength), and on the other hand, it is possible to make the glass phase also contain a certain amount of aluminum oxide, and the aluminum oxide present in the glass phase can enter the glass network structure as [AlO4] tetrahedrons, and form a unified grid with [SiO4], so that the degree of network connection is enhanced, and the strength and stability of the glass network structure are improved, thereby further improving the intrinsic strength of the glass ceramic. At the same time, the [AlO4] tetrahedron in the glass phase can appropriately expand the ion exchange channel, improve the chemical strengthening effect of the glass ceramic, and is more conducive to the preparation of strengthened glass ceramics with excellent mechanical strength properties.
[0151] In some embodiments of the present application, the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass contains ZrO2 at a mass percentage greater than or equal to 3.00%, measured as a mass percentage of oxide.
[0152] In the present application, by controlling the mass percentage of zirconium oxide in the glass ceramic to be greater than or equal to 3.00%, it is beneficial to improve the intrinsic strength of the glass ceramic and improve the surface stress level of the reinforced glass ceramic obtained therefrom. On the one hand, zirconium oxide, as a nucleating agent, will be dispersed in the glass phase in the form of nano-scale grains after heat treatment, which can increase the hardness of the glass ceramic, thereby effectively improving the crushing resistance of the glass ceramic. On the other hand, zirconium oxide exists in the glass phase in the form of cubes [ZrO8], which can enhance the inter-ionic force and make the glass structure more compact, thereby helping to improve the mechanical strength of the glass phase. At the same time, zirconium oxide can significantly increase the surface compressive stress formed by ion exchange, thereby improving the surface stress level of the reinforced glass ceramic obtained.
[0153] In some embodiments of the present application, the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass comprises, in terms of the mass percentage of oxides:
[0154] SiO2: 25.00% to 55.00%, Al2O3: 30.00% to 55.00%, ZrO2: 3.00% to 8.00%, MgO: 2.00% to 5.00%, ZnO: 5.00% to 15.00%, Na2O: 1.00% to 10.00%, K2O: 0% to 5.00%, Li2O: 1.00% to 6.00%, CaO: 0% to 6.00%, B2O3: 0% to 10.00%, BaO: 0% to 10.00%, Y2O3: 0% to 6.00%, La2O3: 0% to 12.00%. By adjusting and controlling the content range of each oxide component, it is beneficial to ensure that the reinforced glass ceramics that meet the desired crystal phase structure are obtained, and at the same time, it is beneficial to ensure that the reinforced glass ceramics obtain excellent optical properties and high intrinsic strength.
[0155] In the present application, SiO2 is a glass network forming oxide and an indispensable component of the glass network structure. Increasing the content of SiO2 can increase the stability and mechanical strength of the glass, but excessive SiO2 will increase the viscosity of the base glass, making it more difficult to melt the glass, thereby reducing the formability of the base glass. In the present application, the mass percentage of SiO2 in the composition at the center of the strengthened glass ceramic or the composition of the glass ceramic used to prepare the strengthened glass ceramic or the composition of the base glass is 25.00% to 55.00%, preferably 30.00% to 42.00%, and more preferably 35.00% to 40.00%.
[0156] In some embodiments of the present application, the content of SiO2 in the composition at the center of the reinforced glass-ceramic or the composition of the glass-ceramic used to prepare the reinforced glass-ceramic or the composition of the substrate glass, measured as a percentage by mass of the oxide, may be 25.00% to 55.00%, 25.00% to 40.00%, 40.00% to 55.00% or 30.00% to 40.00%. In some embodiments of the present application, the content of SiO2 in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass can be 25.00%, 26.00%, 27.00%, 28.00%, 29.00%, 30.00%, 31.00%, 32.00%, 33.00%, 34.00%, 35.00%, 35.50%, 36.00%, 37.00%, 38.00%, 39.00%, 40.00%, 41.00%, 42.00%, 43.00%, 44.00%, 45.00%, 46.00%, 47.00%, 48.00%, 49.00%, 50.00%, 51.00%, 52.00%, 53.00%, 54.00%, 55.00%, 56.00%, 57.00%, 58.00%, 59.00%, 60.00%, 61.00%, 62.00%, 63.00%, 64.00%, 65.00%, 66.00%, 67.00%, 68.00%, 69.00%, 70.00%, 71.00%, 72.00%, 73.00%, 74.00%, 75.00%, 76.00%, 77.00%, 78.00%, 79.00%, 80.00%, 81.00%, 82.00%, 83.00%, 84.00%, 85.00%, 86.00%, 87.00%, 88.00 5.00%, 46.00%, 47.00%, 48.00%, 49.00%, 50.00%, 51.00%, 52.00%, 53.00%, 54.00%, 55.00%, 37.08%, 36.87%, 33.23%, 37.43%, 37.40%, 38.33%, 36.05%, 35.67%, 32.39%, 37.50%, 35.64%, 37.32% or 36.31%, or it can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained.
[0157] In the present application, Al2O3 is one of the components of the main crystal phase of zinc-magnesium spinel solid solution crystal phase formed after the substrate glass is crystallized. The increase of Al2O3 can promote the precipitation of spinel and inhibit the precipitation of other impurities such as quartz, which will directly affect the content of the main crystal phase (Zn, Mg)Al2O4. As the Al2O3 content increases, the strength of the glass phase in the glass ceramic is also enhanced, and the mechanical properties of the glass ceramic are enhanced. At the same time, since [AlO4] is larger in volume than [SiO4], it can provide more space for ion exchange, which is conducive to promoting chemical strengthening. However, excessive Al2O3 will increase the viscosity of the substrate glass, reduce the formability of the substrate glass, and easily lead to a faster crystallization rate, causing the substrate glass to lose transparency during normal cooling. In the present application, the mass percentage of Al2O3 in the composition at the center of the reinforced glass-ceramic or the composition of the glass-ceramic used to prepare the reinforced glass-ceramic or the composition of the substrate glass is 30.00% to 55.00%, preferably 32.00% to 42.00%, and more preferably 34.00% to 42.00%.
[0158] In some embodiments of the present application, the content of Al2O3, measured as a percentage by mass of oxide, in the composition at the center of the reinforced glass-ceramic or in the composition of the glass-ceramic used to prepare the reinforced glass-ceramic or in the composition of the substrate glass may be 30.00% to 55.00%, 30.00% to 40.00% or 40.00% to 55.00%. In some embodiments of the present application, the content of Al2O3 in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass, measured by mass percentage of oxide, may be 30.00%, 31.00%, 32.00%, 33.00%, 34.00%, 34.50%, 35.00%, 35.50%, 36.00%, 36.50%, 37.00%, 38.00%, 39.00%, 40.00%, 41.00%, 42.00%, 43.00%, 44.00%, 45.00%, 46.00%, 47.00%, 48.00%, 49.00%, 50.00%, 51.00%, 52.00%, 53.00%, 54.00%, 55.00%, 56.00%, 57.00%, 58.00%, 59.00%, 60.00%, 61.00%, 62.00%, 63.00%, 64.00%, 65.00%, 66.00%, 67.00%, 68.00%, 69.00%, 70.00%, 71.00%, 72.00%, 73.00%, 74.00%, 75.00%, 76.00%, 77.00%, 78.00%, 79.00%, 80.00%, 81.00%, 82.00%, 83.00%, 84.00%, 85.00%, 86.00%, 87.00%, 88.00%, 89.00%, 90. 0%, 47.00%, 48.00%, 49.00%, 50.00%, 51.00%, 52.00%, 53.00%, 54.00%, 54.50%, 55.00%, 35.83%, 36.98%, 36.27%, 37.52%, 36.60%, 37.07%, 34.84%, 34.55%, 35.88%, 38.63%, 36.23% or 35.10%, or it can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained.
[0159] In the present application, ZrO2 is an effective nucleating agent. During the heat treatment of glass, ZrO2 is first precipitated in the form of crystals, and the ZrO2 crystals become crystal nuclei for the subsequent crystal growth. Within a certain glass composition range, the content of ZrO2 will affect the formation of glass, the crystal shape, crystal type and crystal size of the glass ceramics obtained after the glass heat treatment, etc. By regulating the glass composition, ZrO2 can be preferentially precipitated at the same temperature, and then the main crystal phase spinel crystal growth can be achieved. When the ZrO2 content is too low, it will affect the precipitation of the main crystal phase zinc-magnesium spinel solid solution crystal phase; when the ZrO2 content is too high, it will cause the melting difficulty of the substrate glass to become greater, resulting in the generation of white unmelted materials in the substrate glass. In the present application, the mass percentage of ZrO2 in the composition at the center of the strengthened glass ceramic or the composition of the glass ceramic used to prepare the strengthened glass ceramic or the composition of the substrate glass is 3.00% to 8.00%, preferably 4.00% to 7.00%, and more preferably 5.00% to 6.00%.
[0160] In some embodiments of the present application, the content of ZrO2 in the composition at the center of the strengthened glass-ceramic or in the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or in the composition of the substrate glass, as measured by the mass percentage of the oxide, may be 3.00% to 8.00%, 3.00% to 6.00%, or 6.00% to 8.00%. In some embodiments of the present application, the content of ZrO2 in the composition at the center of the strengthened glass-ceramic or in the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or in the composition of the substrate glass, as measured by the mass percentage of the oxide, may be 3.00%, 3.20%, 3.50%, 3.70%, 4.00%, 4.20%, 4.50%, 4.70%, 5.00%, 5.20%, 5.50%, 5.70%, 6.00%, 7.00%, 7.50%, 7.7 ... 6.50%, 7.00%, 7.50%, 8.00%, 5.69%, 5.65%, 5.61%, 5.74%, 5.81%, 5.89%, 5.54%, 5.48%, 5.76%, 5.72%, 5.99% or 5.58%, or it can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained.
[0161] In the present application, ZnO provides the zinc necessary for the substrate glass to form the main crystal phase, zinc-magnesium spinel solid solution crystal phase after crystallization. ZnO can reduce the thermal expansion coefficient of the glass and improve the chemical stability, thermal stability and refractive index of the glass. MgO provides the magnesium necessary for the substrate glass to crystallize and form the main crystal phase, zinc-magnesium spinel solid solution crystal phase. MgO can slow down the hardening speed of the glass and improve the forming properties of the glass; MgO can also reduce the crystallization tendency and crystallization speed, increase the high-temperature viscosity of the glass, and improve the chemical stability and mechanical strength of the glass. However, the addition of excessive MgO and ZnO often leads to excessively large spinel grains, making it difficult to obtain glass ceramics with high transparency. In the present application, the composition at the center of the reinforced glass-ceramic or the composition of the glass-ceramic used to prepare the reinforced glass-ceramic or the composition of the substrate glass is as follows: the mass percentage of ZnO is 5.00% to 15.00%, preferably 9.00% to 13.00%, and more preferably 9.00% to 11.00%; the mass percentage of MgO is 2.00% to 5.00%, preferably 2.50% to 4.00%, and more preferably 2.50% to 3.50%.
[0162] In some embodiments of the present application, the content of ZnO in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass, measured by mass percentage of the oxide, may be 5.00%, 5.50%, 6.00%, 6.50%, 7.00%, 7.50%, 8.00%, 8.50%, 9.00%, 9.50%, 10.00%, 10.50%, 11.00%, 11.50%, 12.00%, 12.50%, 13.00%, 13.50%, 14.00%, 15.50%, 16.00%, 17.50%, 18.00%, 18.50%, 19.00%, 20.00%, 21.00%, 22.50%, 23.50%, 24.00%, 25.50%, 26.00%, 27.50%, 28.00%, 29.00%, 30.50%, 31.00%, 32.50%, 33.50%, 34.00%, 35.50%, 36.00%, 37.50%, 38.00%, 39.00%, 40.50%, 41.00%, 42.50%, 43.50%, 44.50%, 45.50%, 46.50%, 47.50%, 48.00%, 49.00%, 50.50%, 51.00%, 51.50%, 52.50%, 53.50%, 54.50%, 55.50%, 56.50%, 57.50%, 58.50%, 12.00%, 12.50%, 13.00%, 10.77%, 10.71%, 10.55%, 10.87%, 11.01%, 11.15%, 10.46%, 10.37%, 12.50%, 10.82%, 11.33% or 10.54%, or it can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained.
[0163] In some embodiments of the present application, the content of MgO in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass can be 2.00%, 2.50%, 3.00%, 3.50%, 4.00%, 4.50%, 5.00%, 2.98%, 3.04%, 3.03%, 3.06%, 3.10%, 2.92%, 2.89%, 3.01%, 3.27% or 2.94%, or can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass-ceramic or strengthened glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass-ceramic or strengthened glass-ceramic with the desired performance of the present application can be obtained.
[0164] In the present application, the increase of Na2O content helps to obtain higher surface compressive stress, and can also reduce the melting temperature and the temperature of crystal precipitation. However, its excessive addition will cause the glass to ceramicize during annealing, or cause other impurities that affect the transmittance of glass ceramics to precipitate during heat treatment, thereby reducing the transmittance of the obtained glass ceramics. Too low Na2O content will lead to increased heat treatment temperature, direct phase separation or precipitation of impurities during heat treatment, and obtain opaque or poorly transparent glass ceramics. In the present application, the mass percentage of Na2O in the composition at the center of the strengthened glass ceramic or the composition of the glass ceramic used to prepare the strengthened glass ceramic or the composition of the substrate glass is 1.00% to 10.00%, preferably 1.00% to 8.00%, and more preferably 2.00% to 6.00%.
[0165] In some embodiments of the present application, the content of Na2O in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass can be 1.00%, 1.50%, 2.00%, 2.50%, 3.00%, 3.50%, 4.00%, 4.50%, 5.00%, 5.50%, 6.00%, 6.50%, 7.00%, 7.50%, 8.00%, 8.50%, 9.00%, 9.50%, 10.0 ... 0%, 8.00%, 8.50%, 9.00%, 9.50%, 10.00%, 2.86%, 2.85%, 2.89%, 3.00%, 1.69%, 2.79%, 2.76%, 3.31%, 4.61%, 3.01% or 8.00%, or it can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained.
[0166] In the present application, Li2O helps to obtain a higher depth of the compressive stress layer, improve Young's modulus and fracture toughness; at the same time, it can reduce the melting temperature and the temperature of crystal precipitation, but its excessive addition will cause the glass to ceramicize during annealing, or cause the precipitation of other impurities that affect the transmittance of glass ceramics during heat treatment, or cause excessive crystal growth during heat treatment, so that the transmittance of the obtained glass ceramics decreases. If the amount of Li2O added is too low, the heat treatment temperature will increase and the deep stress will decrease. In the present application, the mass percentage of Li2O in the composition at the center of the strengthened glass ceramic or the composition of the glass ceramic used to prepare the strengthened glass ceramic or the composition of the substrate glass is 1.00% to 6.00%, preferably 1.00% to 4.00%, and more preferably 2.00% to 3.00%.
[0167] In some embodiments of the present application, the content of Li2O in the composition at the center of the strengthened glass-ceramic, the composition of the glass-ceramic used to prepare the strengthened glass-ceramic, or the composition of the substrate glass, measured by mass percentage of oxide, can be 1.00%, 1.50%, 2.00%, 2.50%, 3.00%, 3.50%, 4.00%, 4.50%, 5.00%, 5.50%, 6.00%, 2.35%, 1.55%, 1.50%, 1.77%, 1.60%, 1.62%, 2.28%, 2.27%, 2.24%, 1.60%, 1.57%, 2.85% or 1.53%, or can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass-ceramic or strengthened glass-ceramic with the required performance of the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass ceramic or reinforced glass ceramic having the desired properties of the present application can be obtained.
[0168] In the present application, K2O is an optional component, and its mass percentage can be 0-5.00%, preferably 0-3.00%, and more preferably 0-1.00%. In some embodiments, it is preferred that the composition at the center of the reinforced glass-ceramic or the composition of the glass ceramic used to prepare the reinforced glass-ceramic or the composition of the substrate glass does not contain K2O.
[0169] In the present application, CaO is an optional component. Adding an appropriate amount of CaO is beneficial to reducing the viscosity of the glass, improving the formability, strain point and Young's modulus of the substrate glass, and improving the ion exchange capacity. At the same time, calcium oxide can also increase the gloss and transparency of the glass, reduce the crystallization tendency of the glass, and slow down the hardening rate of the glass. However, when the CaO content is too much, the density and CTE of the glass composition will increase, and the ion exchange performance of the glass ceramic will be significantly reduced. In the present application, the mass percentage of CaO in the composition at the center of the strengthened glass ceramic or the composition of the glass ceramic used to prepare the strengthened glass ceramic or the composition of the substrate glass is 0% to 6.00%, preferably 0% to 3.00%, and more preferably 0% to 1.50%.
[0170] In some embodiments of the present application, the content of CaO in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass can be 0%, 0.50%, 1.00%, 1.50%, 2.00%, 2.50%, 3.00%, 3.50%, 4.00%, 4.50%, 5.00%, 5.50%, 6.00%, 0.75%, 1.15% or 0.92%, or can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass-ceramic or strengthened glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass-ceramic or strengthened glass-ceramic with the desired performance of the present application can be obtained.
[0171] In the present application, B2O3 is an optional component. An appropriate amount of B2O3 is beneficial to significantly reduce the difficulty of melting glass and promote the precipitation of spinel. However, the addition of excessive B2O3 will cause opacity when the substrate glass is heat-treated to prepare glass ceramics. At the same time, it may cause the precipitation of other crystalline phases that seriously affect the transparency of the glass. In the present application, the mass percentage of B2O3 in the composition at the center of the strengthened glass ceramic or the composition of the glass ceramic used to prepare the strengthened glass ceramic or the composition of the substrate glass is 0% to 10.00%, preferably 0% to 8.00%, and more preferably 0% to 4.00%.
[0172] In some embodiments of the present application, the content of B2O3 in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass can be 0%, 0.50%, 1.00%, 1.50%, 2.00%, 2.50%, 3.00%, 3.50%, 4.00%, 4.50%, 5.00%, 6.00%, 7.00%, 8.00%, 9.00%, 10.00% or 7.07%, or can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass-ceramic or strengthened glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass-ceramic or strengthened glass-ceramic with the desired performance of the present application can be obtained.
[0173] In the present application, BaO is an optional component. An appropriate amount of BaO is beneficial to improving the melting effect of glass, increasing the density of glass, improving Young's modulus, and inhibiting the growth of grains to a certain extent, and improving the optical properties of glass ceramics. However, the presence of too much BaO has a strong inhibitory effect on the exchange process of Na ions and K ions. In the present application, the mass percentage of BaO in the composition at the center of the strengthened glass ceramic or the composition of the glass ceramic used to prepare the strengthened glass ceramic or the composition of the substrate glass is 0% to 10.00%, preferably 0% to 7.00%, and more preferably 0% to 4.00%.
[0174] In some embodiments of the present application, the content of BaO in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass can be 0%, 0.50%, 1.00%, 1.50%, 2.00%, 2.50%, 3.00%, 3.50%, 4.00%, 4.50%, 5.00%, 6.00%, 7.00%, 8.00%, 9.00%, 10.00%, 2.42%, 2.41%, 6.94%, 2.35% or 2.32%, or can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass-ceramic or strengthened glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass-ceramic or strengthened glass-ceramic with the desired performance of the present application can be obtained.
[0175] In this application, Y2O3 has the effect of making the glass structure compact. An appropriate amount of Y2O3 can increase the packing density inside the glass, which is manifested as increasing the density of the glass, thereby helping to increase the intrinsic strength of the glass. For ion exchange performance, it can increase the Na + , Li + The stress effect produced by the unit ion exchange of plasma during the chemical strengthening process may reduce its exchange rate. However, when too much Y2O3 is added, it is not conducive to obtaining transparent spinel glass ceramics. In the present application, the mass percentage of Y2O3 in the composition at the center of the strengthened glass ceramic or the composition of the glass ceramic used to prepare the strengthened glass ceramic or the composition of the substrate glass is 0% to 6.00%, preferably 0% to 4.00%, and more preferably 0% to 2.00%.
[0176] In some embodiments of the present application, the content of Y2O3 in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass can be 0%, 0.50%, 1.00%, 1.50%, 2.00%, 2.50%, 3.00%, 3.50%, 4.00%, 4.50%, 5.00%, 5.50%, 6.00%, 1.52% or 0.60%, or can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass-ceramic or strengthened glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass-ceramic or strengthened glass-ceramic with the desired performance of the present application can be obtained.
[0177] In the present application, La2O3 is a network modification component of glass. An appropriate amount of La2O3 can increase the refractive index of glass, reduce the high-temperature viscosity of glass, and help improve the glass melting effect and eliminate its inherent defects. At the same time, an appropriate amount of La2O3 can significantly improve the Young's modulus and micro-Vickers hardness of glass, and also has the effect of improving the chemical strengthening properties of glass ceramics and improving the stress effect produced by unit ion exchange of strengthened glass ceramics. However, when too much La2O3 is added, it is not conducive to obtaining transparent spinel glass ceramics. In the present application, the mass percentage of La2O3 in the composition at the center of the strengthened glass ceramic or the composition of the glass ceramic used to prepare the strengthened glass ceramic or the composition of the substrate glass is 0% to 12.00%, preferably 0% to 5.00%, and more preferably 0% to 3.00%.
[0178] In some embodiments of the present application, the content of La2O3 in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass can be 0%, 0.50%, 1.00%, 1.50%, 2.00%, 2.50%, 3.00%, 3.50%, 4.00%, 5.00%, 6.00%, 7.00%, 8.00%, 9.00%, 10.00%, 11.00%, 12.00%, 2.17% or 3.69%, or can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass-ceramic or strengthened glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass-ceramic or strengthened glass-ceramic with the desired performance of the present application can be obtained.
[0179] In the present application, in order to obtain the desired strengthened glass ceramics with excellent performance, in addition to Y2O3 and La2O3, in terms of oxides, metal oxides of cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium or scandium, or mixtures of the aforementioned metal oxides, can be added to the composition of the glass ceramic or the composition of the substrate glass used to prepare the strengthened glass ceramics, as long as the glass ceramics or strengthened glass ceramics with the desired performance of the present application can be obtained. If the aforementioned metal oxides are added to the composition of the glass ceramic or the composition of the substrate glass used to prepare the strengthened glass ceramics, the composition at the center of the obtained strengthened glass ceramics should also contain these metal oxides.
[0180] In the present application, on the basis of adjusting and controlling the content range of each oxide component, by adjusting and controlling the ratio between the oxide components, especially the mass percentage relationship between Na2O and Li2O and Li2O and SiO2, it is beneficial to improve the intrinsic strength and chemical strengthening effect of glass ceramics, and thus to obtain strengthened glass ceramics with excellent mechanical strength properties.
[0181] In some embodiments of the present application, the mass percentage of Na2O [Na2O] and the mass percentage of Li2O [Li2O] in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass, measured by mass percentage of oxides, satisfy the following relationship: [Na2O] / [Li2O]=0.60~6.00, preferably [Na2O] / [Li2O]=0.90~5.00, and more preferably [Na2O] / [Li2O]=1.00~3.00.
[0182] In some embodiments, in the composition at the center of the reinforced glass-ceramic or the composition of the glass-ceramic used to prepare the reinforced glass-ceramic or the composition of the substrate glass, the ratio [Na2O] / [Li2O] of the mass percentage of Na2O [Na2O] and the mass percentage of Li2O [Li2O] may be 0.60, 0.9, 1.00, 1.50, 2.00, 2.50, 3.00, 3.50, 4.00, 4.50, 5.00, 5.50 or 6.00, or may be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the glass-ceramic or reinforced glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges may be combined with any other ranges, as long as the glass-ceramic or reinforced glass-ceramic with the desired performance of the present application can be obtained.
[0183] In some embodiments of the present application, the mass percentage of Li2O [Li2O] and the mass percentage of SiO2 [SiO2] in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass, measured by mass percentage of oxides, satisfy the following relationship: [Li2O] / [SiO2]=0.03~0.20, preferably [Li2O] / [SiO2]=0.04~0.15, and more preferably [Li2O] / [SiO2]=0.04~0.10.
[0184] In some embodiments, in the composition at the center of the reinforced glass-ceramic or the composition of the glass-ceramic used to prepare the reinforced glass-ceramic or the composition of the substrate glass, the ratio of the mass percentage of Li2O [Li2O] to the mass percentage of SiO2 [SiO2] [Li2O] / [SiO2] can be 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19 or 0.20, or can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass-ceramic or reinforced glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass-ceramic or reinforced glass-ceramic with the desired performance of the present application can be obtained.
[0185] In the present application, the zinc-magnesium spinel solid solution (Zn,Mg)Al2O4 as the main crystalline phase and the tetragonal ZrO2 secondary crystalline phase do not contain alkali metal ions, so they do not participate in the ion exchange during the chemical strengthening process. Based on this, the crystal phase structure of the strengthened glass ceramics obtained by chemical strengthening treatment in the present application is basically the same as the glass ceramics used for chemical strengthening. That is, the crystal phase content, crystal composition, crystal size and other crystal phase structure characteristics of the strengthened glass ceramics obtained by chemical strengthening treatment in the present application are basically the same as the glass ceramics used for chemical strengthening used to prepare the strengthened glass ceramics in the present application. Figure 1 As shown in FIG. 1 , in Example 1, the XRD patterns of the glass ceramic before chemical strengthening and the strengthened glass ceramic after chemical strengthening are substantially the same. Figure 2 As shown, in the present application, the transmittance of the glass ceramics before and after chemical strengthening is basically the same as the transmittance of the strengthened glass ceramics. That is to say, in the present application, by using glass ceramics with high transmittance, chemical strengthening treatment can be performed to obtain strengthened glass ceramic products with the same excellent transmittance.
[0186] It should be understood that the stress structure generated by the chemical strengthening process can appropriately improve the mechanical properties of glass products. Therefore, in the present application, after the glass ceramics are chemically strengthened to obtain strengthened glass ceramics, their mechanical properties such as Young's modulus and Vickers hardness will not decrease.
[0187] In some embodiments of the present application, the average crystal size of the reinforced glass ceramic or the glass ceramic used to prepare the reinforced glass ceramic is no more than 20.0 nm, preferably 1.0 nm to 10.0 nm, more preferably 4.0 nm to 9.0 nm, and more preferably 4.0 nm to 8.0 nm. An appropriate average grain size is conducive to making the glass ceramic have both excellent optical properties and high intrinsic strength, while if the average grain size is too high, the glass ceramic is prone to devitrification and the chemical strengthening effect will also be affected.
[0188] In some embodiments, in the glass ceramic or reinforced glass ceramic, the average crystal size can be 4.0nm, 5.0nm, 6.0nm, 7.0nm, 8.0nm, 9.0nm, 10.0nm, 11nm, 12nm, 13nm, 14nm, 15nm, 16nm, 17nm, 18nm, 19nm, 20nm, 6.8nm, 6.4nm, 6.5nm, 8.1nm, 6.1nm, 5.1nm or 6.2nm, or can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained.
[0189] In some embodiments of the present application, the total crystalline phase content of the reinforced glass ceramic or the glass ceramic used to prepare the reinforced glass ceramic is 25% to 60%, preferably 30% to 55%, and more preferably 40% to 50%, by mass percentage. The higher the total crystalline phase content of the glass ceramic or the reinforced glass ceramic, the more conducive it is for the glass ceramic or the reinforced glass ceramic to obtain high intrinsic strength. However, if the total crystalline phase content is too high, it will not only affect the chemical strengthening effect of the glass ceramic, prolong the chemical strengthening time of the reinforced glass ceramic with a high stress level, but also may affect the optical properties of the glass ceramic. In some embodiments, the total crystalline content of the reinforced glass-ceramic or the glass-ceramic used to prepare the reinforced glass-ceramic can be 30.00%, 31.00%, 32.00%, 33.00%, 34.00%, 35.00%, 36.00%, 37.00%, 38.00%, 39.00%, 40.00%, 41.00%, 42.00%, 43.00%, 44.00%, 45.00%, 46.00%, 47.00%, 48.00%. %, 49.00%, 50.00%, 55.00%, 60.00%, 48.69%, 45.11%, 49.52%, 47.85%, 54.07%, 51.56%, 45.49%, 44.77%, 52.28%, 35.52%, 48.75% or 44.33%, or it can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained.
[0190] In the present application, "main crystalline phase zinc aluminum spinel-magnesium aluminum spinel solid solution" or other similar expressions means that the zinc aluminum spinel-magnesium aluminum spinel solid solution accounts for more than 50% by mass of all crystalline phases of the glass ceramic or reinforced glass ceramic according to the embodiment of the present application. In some embodiments, the mass of the zinc aluminum spinel-magnesium aluminum spinel solid solution accounts for more than 50% of all crystalline phases of the glass ceramic or the reinforced glass ceramic made of the glass ceramic, and preferably, the mass of the zinc aluminum spinel-magnesium aluminum spinel solid solution accounts for more than 70% of all crystalline phases of the glass ceramic or the reinforced glass ceramic made of the glass ceramic. Exemplarily, in all crystalline phases of the glass ceramic or the reinforced glass ceramic obtained from the glass ceramic, the mass proportion (or also called weight proportion, mass percentage, weight percentage) of the zinc aluminum spinel-magnesium aluminum spinel solid solution crystal phase can be 50%, 60%, 70%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86% or 90%, or can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass ceramic or reinforced glass ceramic with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass ceramic or reinforced glass ceramic with the required performance of the present application can be obtained.
[0191] In the present application, by making the glass ceramics or reinforced glass ceramics meet the desired total crystalline content / crystallinity and appropriate average crystal size, it is beneficial to make the glass ceramics or reinforced glass ceramics maintain excellent optical properties while meeting excellent mechanical strength properties and high intrinsic strength, and obtain the desired chemical strengthening effect.
[0192] In some embodiments of the present application, the reinforced glass ceramic or the glass ceramic used to prepare the reinforced glass ceramic is transparent in the visible light wavelength range, preferably, at a thickness of 0.90 mm, for 550 nm wavelength light, the transmittance of the reinforced glass ceramic or the glass ceramic used to prepare the reinforced glass ceramic is ≥ 85.00%, preferably ≥ 87.00%. Glass ceramics or reinforced glass ceramics that meet this transmittance can ensure good light transmittance and good transparency, and are suitable for use in electronic device display screens that require display effects. The "visible light wavelength range" here refers to light with a wavelength of 360 nm-740 nm.
[0193] In some embodiments, at a thickness of 0.90 mm, for light with a wavelength of 550 nm, the transmittance of the strengthened glass-ceramic or the glass-ceramic used to prepare the strengthened glass-ceramic can be: 86.00%, 87.00%, 88.00%, 88.50%, 89.00%, 89.10%, 89.20%, 89.30%, 89.40%, 89.50%, 89.60%, 89.70%, 89.80%, 89.90%, 90.00%, 90.10%, 90.20%, 90. 0.30%, 90.40%, 90.50%, 91.00%, 92.00%, 89.73%, 89.48%, 89.87%, 89.66%, 89.15%, 89.43%, 89.65%, 89.71%, 89.14%, 89.75%, 89.90%, 89.85% or 88.53%, or it can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained.
[0194] In some embodiments of the present application, the Vickers hardness of the reinforced glass-ceramic is greater than or equal to 750 kgf / mm 2 Preferably, the Vickers hardness of the reinforced glass ceramic is greater than or equal to 790 kgf / mm 2 The Vickers hardness of the reinforced glass-ceramics is within the above range, indicating that the reinforced glass-ceramics have high hardness and high intrinsic strength, thereby ensuring excellent mechanical properties.
[0195] In some embodiments, the Vickers hardness of the reinforced glass-ceramic may be: 790 kgf / mm 2 、795kgf / mm 2 、800kgf / mm 2 、805kgf / mm 2 、810kgf / mm 2 、815kgf / mm 2 、820kgf / mm 2 、825kgf / mm 2 、830kgf / mm 2 、835kgf / mm 2 、840kgf / mm 2 、845kgf / mm 2 、850kgf / mm 2 、855kgf / mm 2 、860kgf / mm 2、865kgf / mm 2 、870kgf / mm 2 、875kgf / mm 2 、880kgf / mm 2 、885kgf / mm 2 、890kgf / mm 2 、895kgf / mm 2 、900kgf / mm 2 、848kgf / mm 2 、879kgf / mm 2 、889kgf / mm 2 、836kgf / mm 2 、911kgf / mm 2 、897kgf / mm 2 、807kgf / mm 2 、894kgf / mm 2 、883kgf / mm 2 、873kgf / mm 2 、863kgf / mm 2 or 856kgf / mm 2 , or can be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained.
[0196] In some embodiments of the present application, the fracture toughness value of the reinforced glass-ceramic is greater than or equal to 1.00 MPa·m 0.5 Preferably, the fracture toughness value of the reinforced glass ceramic is greater than or equal to 1.20 MPa·m 0.5 More preferably, the fracture toughness value of the reinforced glass ceramic is greater than or equal to 1.50 MPa·m 0.5 .
[0197] In the present application, by making the reinforced glass ceramics have high Vickers hardness and fracture toughness, the reinforced glass ceramics are not easily broken when being squeezed or impacted, which is beneficial to improving the compressive resistance of the reinforced glass ceramics.
[0198] In some embodiments, the fracture toughness value of the reinforced glass-ceramic can be 1.20 MPa·m 0.5 , 1.30MPa·m 0.5 、1.45MPa·m 0.5 、1.50MPa·m 0.5 、1.55MPa·m 0.5, 1.60MPa·m 0.5 、1.65MPa·m 0.5 , 1.70MPa·m 0.5 , 1.75MPa·m 0.5 , 1.80MPa·m 0.5 、1.85MPa·m 0.5 , 1.90MPa·m 0.5 , 1.95MPa·m 0.5 、2.00MPa·m 0.5 , 1.64MPa·m 0.5 , 1.66MPa·m 0.5 , 1.71MPa·m 0.5 , 1.63MPa·m 0.5 , 1.74MPa·m 0.5 , 1.72MPa·m 0.5 , 1.59MPa·m 0.5 , 1.69MPa·m 0.5 , 1.57MPa·m 0.5 or 1.67MPa·m 0.5 , or can be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained.
[0199] In some embodiments of the present application, the reinforced glass-ceramic has a |CT_AV| not exceeding 60 MPa, preferably a |CT_AV| of 4.00 MPa to 55.00 MPa, preferably a |CT_AV| of 4.00 MPa to 20.00 MPa, where |CT_AV| is the absolute value of the average tensile stress measured by SLP_2000.
[0200] In some embodiments, the |CT_AV| of the strengthened glass-ceramic can be 4.00MPa, 5.00MPa, 6.00MPa, 7.00MPa, 8.00MPa, 9.00MPa, 10.00MPa, 11.00MPa, 12.00MPa, 13.00MPa, 14.00MPa, 15.00MPa, 16.00MPa, 17.00MPa, 18.00MPa, 19.00MPa, 20.00MPa, 30.00MPa, 40.00MPa, 50.00MPa, 60.00MPa, 61.00MPa, 62.00MPa, 63.00MPa, 64.00MPa, 65.00MPa, 66.00MPa, 67.00MPa, 68.00MPa, 69.00MPa, 70.00MPa, 71.00MPa, 72.00MPa, 73.00MPa, 74.00MPa .68MPa, 5.85MPa, 12.45MPa, 5.45MPa, 7.33MPa, 7.79MPa, 10.91MPa, 14.64MPa, 9.98MPa, 6.25MPa, 13.15MPa, 8.58MPa, 6.33MPa, 7.91MPa, 10.75MPa, 12.77MPa, 13.58MPa, 9.47MPa or 7.98MPa, or it can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained.
[0201] In some embodiments of the present application, the reinforced glass-ceramic has a |CT_CV| not exceeding 75 MPa, preferably a |CT_CV| of 5.00 MPa to 70.00 MPa, and preferably a |CT_CV| of 6.00 MPa to 25.00 MPa, where |CT_CV| is the absolute value of the maximum tensile stress measured by SLP_2000.
[0202] In some embodiments, the |CT_CV| of the strengthened glass-ceramic is 5.00MPa, 6.00MPa, 7.00MPa, 8.00MPa, 9.00MPa, 10.00MPa, 11.00MPa, 12.00MPa, 13.00MPa, 14.00MPa, 15.00MPa, 16.00MPa, 17.00MPa, 18.00MPa, 19.00MPa, 20.00MPa, 21.00MPa, 22.00MPa, 23.00MPa, 24.00MPa, 25.00MPa, 35.00MPa, 45.00MPa, 55.00MPa a, 65.00MPa, 75.00MPa, 7.87MPa, 6.96MPa, 15.32MPa, 6.84MPa, 8.12MPa, 9.01MPa, 11.79MPa, 17.92MPa, 11.70MPa, 7.76MPa, 15.90MPa, 9.45MPa, 8.68MPa, 9.13MPa, 12.07MPa, 14.12MPa, 15.74MPa, 10.75MPa or 9.02MPa, or it can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the reinforced glass-ceramic with the desired performance of the application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the reinforced glass-ceramic with the desired performance of the application can be obtained.
[0203] In the present application, by making the strengthened glass-ceramics satisfy a suitable stress structure, the stress structure is beneficial to improving the mechanical strength performance, especially the excellent compressive performance to be achieved in the present application.
[0204] In some embodiments of the present application, a 10 mm diameter round head metal pressure rod is used to gradually apply a load vertically downward at 10 mm / min to compress the center of the main surface of the reinforced glass ceramic, and the single rod static pressure strength that the reinforced glass ceramic can withstand is tested. The single rod static pressure strength that the reinforced glass ceramic can withstand is greater than 800 N. In the present application, the single rod static pressure strength is used to characterize the compressive strength of the reinforced glass ceramic. The greater the single rod static pressure strength that the reinforced glass ceramic can withstand, the better its compressive strength.
[0205] After introducing the composition, crystal structure and stress structure of the strengthened glass-ceramics, the preparation method of the strengthened glass-ceramics is introduced in detail below.
[0206] In the present application, the preparation process of strengthened glass ceramics mainly includes: the preparation process of glass ceramics and the chemical strengthening treatment process, and the preparation process of glass ceramics mainly includes: the preparation process of substrate glass and the heat treatment process of substrate glass.
[0207] In the present application, the substrate glass can be prepared by a molding method in the prior art, and the present application has no limitation on this. For example, the molding method of the substrate glass can include but is not limited to float, overflow, rolling or casting processes. For example, the substrate glass can be obtained by uniformly mixing the components according to the formula, melting and molding, cooling and annealing.
[0208] Exemplarily, each raw material (conventional industrial raw material) is configured according to the formula ratio, a clarifier is added, and then mixed for a period of time to obtain a uniform raw material mixture. The raw material mixture is placed in a platinum crucible, heated to 1450°C to 1800°C, preferably the melting temperature is 1550°C to 1680°C, and preferably kept warm for 3 to 12 hours under this temperature condition, and then poured into a molding mold for cooling and molding, preferably cooled to 800°C to 1000°C, and then placed in an annealing furnace for annealing treatment, preferably the annealing temperature is 500°C to 700°C, and the annealing time is preferably 4h to 48h; then cooled to room temperature with the furnace, the substrate glass can be obtained. Those skilled in the art can select the type and amount of clarifier according to needs, and they do not need to pay creative labor. Further, the clarifier may include but is not limited to one or more of sodium chloride, tin oxide, antimony oxide or arsenic oxide, and the amount of clarifier added may be 0wt% to 1wt% of the total amount of each raw material.
[0209] In some embodiments of the present application, the heat treatment process of the substrate glass may include nucleation treatment and / or crystallization treatment, preferably nucleation treatment and crystallization treatment. In some embodiments, the crystallization treatment includes a one-step crystallization treatment or a multi-step crystallization treatment.
[0210] In some embodiments of the present application, in order to obtain the desired physical and chemical properties of the glass ceramic, when the substrate glass is heat treated, a one-step heat treatment may be performed, or two-step or multi-step heat treatment may be performed. If a one-step heat treatment is performed, it means that a nucleation treatment (i.e., nucleation treatment) is not performed separately, and a one-step heating is directly performed, and nucleation and target crystal growth are performed at the temperature reached in the one-step heating process, which can be understood as a direct crystallization treatment. If a two-step heat treatment is performed, it means that a two-step heating process is performed, first a nucleation treatment, i.e., nucleation treatment, is performed, and then a target crystal growth treatment, i.e., crystallization treatment, is performed.
[0211] In the present application, in order to make the glass ceramics precipitate the desired crystalline phase and obtain the desired physical and chemical properties, further, the temperature of the nucleation treatment can be 600℃~850℃, and the time of the nucleation treatment can be 0h~72h, preferably 0h~10h; the temperature of the crystallization treatment can be 700℃~1000℃, and the time of the crystallization treatment can be 0.10h~24h, preferably 0.1h~6h. When performing heat treatment, it is preferred to control the heating rate to 5℃ / min~15℃ / min, and more preferably the heating rate is 10℃ / min. Among them, the temperature of the nucleation treatment refers to the temperature at which the crystal nucleus can be formed. The temperature of the crystallization treatment refers to the temperature at which the target crystal is suitable for controllable growth.
[0212] After heat treatment, technicians in this field can also perform other conventional steps to obtain glass-ceramic samples / samples that meet the required specifications or requirements, such as shaping, cutting (such as cutting using a multi-wire cutting machine), CNC machining (computer numerical control, i.e., CNC machine tools), thinning or polishing.
[0213] In some embodiments of the present application, by subjecting the aforementioned glass-ceramics to a specific chemical strengthening treatment, a strengthened glass-ceramic satisfying the desired performance can be prepared.
[0214] In the present application, the chemical strengthening treatment, i.e., the ion exchange method, is performed by immersing the glass ceramic in a molten salt bath to exchange the alkali metal ions with smaller ion radius in the glass ceramic with the alkali metal ions with larger ion radius in the molten salt bath, thereby forming a compressive stress layer on the surface of the glass ceramic to obtain strengthened glass ceramics with better mechanical properties.
[0215] In some embodiments of the present application, the chemical strengthening treatment may adopt a single-step strengthening method or a multi-step strengthening method. The molten salt bath for chemical strengthening treatment is a molten salt bath containing sodium salt and / or potassium salt. Preferably, in the present application, the chemical strengthening adopts a single-step strengthening method, and the molten salt bath used in the strengthening process is a salt bath containing pure potassium salt, or a mixed salt bath in which the mass percentage of potassium salt in the salt bath is not less than 90%. Preferably, the temperature of the molten salt bath is 380°C to 600°C, more preferably 400 to 500°C. In some embodiments of the present application, a certain amount (e.g., 0wt% to 0.5wt%) of lithium salt may be added to the salt bath. In some embodiments of the present application, the time for chemical strengthening treatment is preferably 0.1h to 48h, preferably 0.1h to 24h. Among them, the sodium salt can be selected from at least one of sodium nitrate, sodium sulfate, and sodium carbonate, preferably sodium nitrate; the potassium salt can be selected from at least one of potassium nitrate, potassium sulfate, and potassium carbonate, preferably potassium nitrate; the lithium salt can be selected from at least one of lithium nitrate, lithium sulfate, and lithium carbonate, preferably lithium nitrate.
[0216] In some embodiments of the present application, the reinforced glass ceramic may have a fracture toughness of not less than 1.40 MPa·m 0.5 The glass ceramic is obtained by chemical strengthening treatment. Preferably, the strengthened glass ceramic can have a fracture toughness of not less than 1.40 MPa·m 0.5 The glass ceramic is obtained by a single-step chemical strengthening treatment. More preferably, the fracture toughness can be not less than 1.40 MPa·m 0.5 The glass ceramic is placed in a molten salt bath containing potassium salt with a mass percentage of potassium salt greater than or equal to 90%, and subjected to a single-step chemical strengthening treatment to obtain the strengthened glass ceramic with a specific surface composition and excellent anti-extrusion performance.
[0217] The glass ceramics or strengthened glass ceramics with excellent performance (especially excellent anti-extrusion performance) provided in the present application can be used in electronic devices, including but not limited to mobile phones, tablet computers, handheld game consoles, portable digital devices (such as digital cameras), vehicle-mounted central control, electronic whiteboard glass, smart home, smart wear (such as smart bracelets, smart watches, smart glasses), and can also be used in vehicles, aircraft or aircraft, and can also be used in any glass device of glass ceramics or strengthened glass ceramics. For example, it can be used for display screens, cover glass, touch screens, glass inner screens or inner frames of electronic devices; for example, it can be used for windshields of vehicles, aircraft or aircraft, such as front windshields or side windshields. For example, it can be used for worktops, other surfaces, appliance doors, floor tiles, wall panels or storage containers. Other surfaces may include but are not limited to exterior wall surfaces, stair tread surfaces, column veneers or counter surfaces, and storage containers may include but are not limited to cups, plates, medicine bottles or beverage bottles.
[0218] For example, the glass ceramics or reinforced glass ceramics with excellent performance provided in the present application can be used to manufacture glass devices. The glass devices referred to here can be regular or irregular, and those skilled in the art can manufacture them according to needs.
[0219] For example, the glass ceramic or reinforced glass ceramic with excellent performance (especially excellent anti-extrusion performance) provided by the present application can be used to manufacture cover glass, and the cover glass can be a display cover, back cover or camera protection cover of an electronic device. For example, the glass ceramic or reinforced glass ceramic with excellent performance provided by the present application can be used in electronic devices. Figure 7 , Figure 8 , Fig. 9 and Fig.10 In some embodiments of the present application, an electronic device is provided, which may be a mobile phone (such as Figure 7 ), tablet computers, smart wearable devices (such as Fig.10) and other electronic products, the electronic device includes a shell 1 assembled on the outside of the electronic device, the shell 1 includes a display screen cover 11 assembled on the front side and a back cover 12 assembled on the back side, the display screen cover 11 is covered on the display module 4, wherein the display screen cover 11 and / or the back cover 12 are made of the aforementioned glass ceramics or reinforced glass ceramics. In the present application, the display screen cover 11 and the back cover 12 may be made of the aforementioned glass ceramics or reinforced glass ceramics in their entirety, or only partially of the aforementioned glass ceramics or reinforced glass ceramics. In the present application, the display screen may be a touch screen, and the display screen cover 11 may be a protective cover provided on the touch screen. In the present application, the back cover 12 may cover only the back side (and the side away from the display screen) of the electronic device, or may cover both the back side and the side frame of the electronic device. Optionally, the back cover 12 may cover all the side frames around the electronic device, or may cover part of the side frames.
[0220] In some implementation modes of the present application, Figure 8 As shown, the electronic device may further include a camera assembly 2 located inside the housing 1, and the housing 1 may include a camera protection cover 13, the camera protection cover 13 is covered on the camera assembly 2 for protecting the camera assembly 2, and the camera protection cover 13 adopts the aforementioned glass ceramics or reinforced glass ceramics. In the present application, the camera protection cover 13 may be partially made of the aforementioned glass ceramics or reinforced glass ceramics, or may be entirely made of the aforementioned glass ceramics or reinforced glass ceramics. In the present application, the setting position of the camera protection cover 13 is determined according to the setting position of the camera assembly 2, and may be located on the front side of the electronic device, or may be located on the back side of the electronic device. In some embodiments of the present application, the camera protection cover 13 may be a separate structure from the display screen cover 11 or the back cover 12. In other embodiments of the present application, the camera protection cover 13 may also be an integrated structure with the display screen cover 11 or the back cover 12.
[0221] In some embodiments of the present application, Fig. 9 As shown, the electronic device may further include a middle frame 3 located between the display module 4 and the housing 1 , and the middle frame 3 may include the aforementioned glass ceramic or reinforced glass ceramic.
[0222] In the embodiments of the present application, the display cover, back cover, camera protection cover, and middle frame in the electronic device can be any one, any two, any three, or any four of the four, and use the aforementioned glass ceramics or reinforced glass ceramics.
[0223] In some embodiments of the present application, the display screen cover, back cover, camera protection cover or middle frame in the electronic device may be 2D, 2.5D, 3D or special-shaped. In some embodiments of the present application, the display screen cover, back cover, camera protection cover or middle frame in the electronic device may be of equal thickness or unequal thickness.
[0224] The technical solution of the present application is further described in detail below in conjunction with the embodiments. The embodiments of the present application described in detail below are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application.
[0225] Example 1
[0226] A reinforced glass ceramic, the preparation process of which is as follows:
[0227] (1) Preparation of substrate glass:
[0228] The raw materials (conventional industrial raw materials) were prepared according to the proportions of the components in Table 1. The total mass of the prepared raw materials was 1000 g. 5 g of clarifier sodium chloride (NaCl) was added to the prepared raw materials, and then mixed with a V-type mixer for 30 minutes to obtain a uniform raw material mixture.
[0229] The raw material mixture is transferred to a platinum crucible, and then melted in the platinum crucible at 1650°C for 5 hours, and then poured into a molding mold for molding and cooling, cooled to 900°C, and then placed in a 600°C annealing furnace for annealing for 24 hours, and then cooled to room temperature with the furnace to obtain the base material glass brick.
[0230] (2) Preparation of glass ceramics: According to the heat treatment process in Table 2, the base glass brick is placed in an annealing furnace, and the temperature is raised from room temperature to 750°C at a heating rate of 10°C / min for nucleation treatment. After heat treatment at this temperature for 240 minutes, the temperature is raised to 765°C at a heating rate of 10°C / min for crystallization treatment. The temperature is kept at this temperature for 120 minutes, and then the temperature is cooled to room temperature at a cooling rate of 1°C / min to obtain a glass ceramic sample brick. The composition of the obtained glass ceramic is the same as that of the base glass in terms of the mass percentage of oxides, as shown in Table 1.
[0231] The obtained glass ceramic sample bricks are subjected to the cold working treatments of cutting, CNC processing (the CNC instrument model used in this application is: RCG500S), and polishing in sequence, and glass ceramic samples / samples that meet the required specifications and requirements can be obtained. In Examples 1 to 20 and Comparative Examples 1 to 15 of the present application, the glass ceramic sample bricks are subjected to the aforementioned cold working treatment to be made into glass ceramic samples / samples with a thickness of 0.70 mm, 0.90 mm, 0.95 mm or 1.05 mm, respectively, specifically, circular glass ceramic polished sheet samples / samples with a diameter of 46 mm and a thickness of 0.70 mm, 0.90 mm, 0.95 mm or 1.05 mm, respectively.
[0232] The glass ceramic samples / samples obtained in Example 1 were tested as follows:
[0233] The crystal phase composition, average crystal size, total crystal content, transmittance (under 550nm wavelength light), density, Vickers hardness and fracture toughness of the glass-ceramics were tested respectively, and the results are shown in Table 2.
[0234] (3) Preparation of strengthened glass ceramics: According to the chemical strengthening process in Table 3, the obtained glass ceramic samples / samples are placed in the strengthening furnace cavity for preheating for 5 minutes. After preheating, they are quickly placed in a molten salt bath at 430°C for chemical strengthening treatment. The composition of the molten salt is 100wt% KNO3. The chemical strengthening treatment time is 1 hour. Then, the glass ceramic samples / samples are taken out and placed on the strengthening furnace body to slowly cool to room temperature. The salt wrapped on the surface of the glass ceramics is washed off with clean water. After the glass ceramic samples / samples are dried, the strengthened glass ceramics can be obtained.
[0235] The test results of the reinforced glass ceramic samples / samples obtained in Example 1 are as follows:
[0236] Ⅰ. The strengthened glass-ceramics were measured under the SLP-2000 stress meter (the light source wavelength used was 518nm, SOC=25.5 (nm / cm) / MPa, the refractive index was set to 1.60, and the exposure time was 300μsec). The results are shown in Table 3.
[0237] Ⅱ. The surface Na2O mass percentage and surface K2O mass percentage of the strengthened glass-ceramics were determined by XRF. The results are shown in Table 3.
[0238] III. The strengthened glass ceramics were subjected to micro-area composition analysis using Shimadzu electron probe EPMA-1720HT, using the characteristic X-rays produced by the electron beam acting on the sample, and DOL_K was measured. The results are shown in Table 3.
[0239] IV. The Vickers hardness and fracture toughness of the reinforced glass-ceramics, as well as the single-rod static pressure strength that the reinforced glass-ceramics can withstand, were tested. The results are shown in Table 3.
[0240] Example 2 to Example 19
[0241] The above methods are respectively carried out with reference to Example 1, except that the raw material composition, different process parameters and corresponding test results of each example are shown in Tables 1 to 3, respectively.
[0242] Among them, the XRD spectrum comparison diagram of the glass ceramic of Example 1 and the reinforced glass ceramic is as follows: Figure 1 As shown in the figure, ① the main crystal phase of the glass ceramic and the strengthened glass ceramic is zinc aluminum spinel-magnesium aluminum spinel solid solution (Zn, Mg)Al2O4, and the secondary crystal phase is ZrO2; ② the XRD spectra of the glass ceramic and the strengthened glass ceramic are basically overlapped, indicating that the crystal phase structure is basically unchanged before and after chemical strengthening.
[0243] The transmittance curve comparison of the glass ceramic of Example 1 and the reinforced glass ceramic is shown in FIG. Figure 2 As shown in the figure, it can be seen that the glass ceramics and the strengthened glass ceramics prepared therefrom are both transparent in the visible light range, both have high transmittance, and the transmittance remains basically unchanged before and after chemical strengthening.
[0244] Comparative Example 1 to Comparative Example 15
[0245] The methods are respectively carried out with reference to Example 1, except that the raw material compositions, different process parameters and corresponding test results of each comparative example are shown in Tables 1 to 3, respectively.
[0246]
[0247]
[0248]
[0249]
[0250]
[0251] Note: 1. The surface K2O concentration in Table 3 refers to the mass percentage of K2O on the surface of the strengthened glass-ceramics, and the surface Na2O concentration refers to the mass percentage of Na2O on the surface of the strengthened glass-ceramics.
[0252] 2. In Table 3, if the data in the "Surface K2O Concentration" column or the "Surface Na2O Concentration" column is recorded as "0.000", it means that the content of K element or Na element contained in the strengthened glass-ceramic of the tested solution is less than 0.0013%, that is, it is lower than the test accuracy (0.0013%) of the XRF instrument used in this application. Since when the content is lower than the test accuracy of the XRF instrument, the instrument will not display the element and its content, therefore, "0.000" is used for recording in this application.
[0253] 3. In Table 3, in the "Salt bath composition" column of each embodiment or comparative example, if the expression "first step strengthening" or "second step strengthening" is not clearly recorded, it means that the embodiment or comparative example adopts single-step strengthening, that is, only one step of chemical strengthening treatment is performed.
[0254] 4. In Table 3, the "Salt bath composition" column clearly records "first step strengthening" and "second step strengthening", indicating that the comparative example was subjected to two-step chemical strengthening treatment, and |CT-CV| and |CT-AV| tests were carried out after each step of strengthening treatment. After the second step of strengthening treatment, the surface K2O concentration, surface Na2O concentration, DOL_K, Vickers hardness and fracture toughness of the obtained strengthened glass-ceramics were tested, and the single-rod static pressure strength that the strengthened glass-ceramics could withstand was tested.
[0255] It can be seen from the embodiments and comparative examples in Tables 1 to 3 above that the embodiments of the present application adopt glass-ceramics having a specific composition and a specific crystal structure and a thickness greater than 0.70 mm for chemical strengthening, and the surface composition of the obtained strengthened glass-ceramics meets specific requirements, especially the surface Na2O mass percentage of the strengthened glass-ceramics (i.e., the surface Na2O concentration in Table 3) and the surface K2O mass percentage of the strengthened glass-ceramics (i.e., the surface K2O concentration in Table 3) and the K2O concentration calculated from the main surface of the strengthened glass-ceramics. + The (K element) diffusion depth (ie, DOL_K in Table 3) meets specific requirements at the same time, significantly improving the compressive resistance of the reinforced glass-ceramics, so that the reinforced glass-ceramics have excellent anti-extrusion properties and can withstand a single-rod static pressure strength of more than 800N.
[0256] However, in the schemes of Comparative Examples 1 to 15, the composition of the glass ceramics used to prepare the reinforced glass ceramics, the thickness of the glass ceramics or the surface composition of the prepared reinforced glass ceramics do not meet the specific requirements of the present application, which ultimately results in the prepared reinforced glass ceramics having an anti-extrusion performance that is significantly inferior to the embodiments that meet the requirements of the scheme of the present application.
[0257] The following is an example analysis of some comparative proportions:
[0258] The glass composition of the substrate of Comparative Example 1 does not contain Li2O, and does not meet the composition requirements of the center of the strengthened glass-ceramic of this application. The Vickers hardness of the glass-ceramic obtained after heat treatment is 650 kgf / mm 2 , fracture toughness value is 1.32MPa·m 0.5 After chemical strengthening treatment, the obtained strengthened glass ceramic has a DOL_K of 16.80 μm and a surface K2O concentration of 6.33%, but a surface Na2O concentration of 1.450%, which does not meet the requirements of the present application for the surface composition of strengthened glass ceramics. Finally, after testing, the Vickers hardness of the strengthened glass ceramic is 774 kgf / mm 2 , fracture toughness is 1.53MPa·m 0.5 The single-rod static pressure strength that the reinforced glass-ceramic can withstand is only 599N, which is significantly lower than the embodiment of the present application.
[0259] The Na2O content in the glass composition of the substrate of Comparative Example 2 is 0.87%, which is too low and does not meet the composition requirements of the center of the strengthened glass-ceramic of this application. The Vickers hardness of the glass-ceramic obtained after heat treatment is 721 kgf / mm 2 , fracture toughness value is 1.47MPa·m 1 / 2 After chemical strengthening treatment of the glass ceramic, the surface K2O concentration of the obtained strengthened glass ceramic was 1.58%, the surface Na2O concentration was 0.000%, and the DOL_K was 4.00μm, which did not meet the requirements of the present application for the surface composition of the strengthened glass ceramic. Finally, after testing, the Vickers hardness of the strengthened glass ceramic was 759kgf / mm 2 , fracture toughness is 1.53MPa·m 0.5 The single-rod static pressure strength that the reinforced glass-ceramic can withstand is only 558N, which is obviously lower than the embodiment of the present application.
[0260] The Li2O concentration in the substrate glass composition of Comparative Example 3 is 0.62%, which is too low and does not meet the composition requirements of the center of the strengthened glass-ceramic of this application. The Vickers hardness of the glass-ceramic obtained after heat treatment is 657 kgf / mm 2 , fracture toughness value is 1.36MPa·m 0.5 After chemical strengthening treatment of the glass ceramic, the surface K2O concentration of the obtained strengthened glass ceramic was 3.92%, the surface Na2O concentration was 0.000%, and the DOL_K was 9.40μm. Finally, after testing, the Vickers hardness of the strengthened glass ceramic was 766kgf / mm 2 , fracture toughness is 1.53MPa·m 0.5 The single-rod static pressure strength that the reinforced glass-ceramic can withstand is only 661N, which is obviously lower than the embodiment of the present application.
[0261] The Li2O concentration in the substrate glass composition of Comparative Example 4 is 0.79%, which is too low and does not meet the composition requirements of the center of the strengthened glass-ceramic of this application. The Vickers hardness of the glass-ceramic obtained after heat treatment is 670 kgf / mm 2 , fracture toughness value is 1.38MPa·m 0.5 After chemical strengthening treatment of the glass ceramic, the surface K2O concentration of the obtained strengthened glass ceramic was 5.12%, and the surface Na2O concentration was 2.350%, which did not meet the requirements of the present application for the surface composition of strengthened glass ceramics; DOL_K was 9.30μm. Finally, after testing, the Vickers hardness of the strengthened glass ceramic was 774kgf / mm 2 , fracture toughness is 1.54MPa·m 0.5 The single-rod static pressure strength that the reinforced glass-ceramic can withstand is only 711N, which is obviously lower than the embodiment of the present application.
[0262] Comparative Examples 5 to 11 are obtained by using the glass ceramics of Example 1 under different strengthening conditions, but the surface compositions of the strengthened glass ceramics obtained in Comparative Examples 5 to 11, especially the surface Na2O concentration, surface K2O concentration, K + The diffusion depth DOL_K of (K element) cannot meet the requirements of the present application for the strengthened glass ceramics. Finally, after testing, the single rod static pressure strength that the strengthened glass ceramics prepared in Comparative Examples 5 to 11 can withstand is also less than 800N.
[0263] Comparative Example 12 is obtained by using the glass ceramics of Example 11 under different strengthening conditions. The surface Na2O concentration, surface K2O concentration, K + The diffusion depth DOL_K of (K element) cannot also meet the requirements of the present application for the strengthened glass ceramics. Finally, after testing, the strengthened glass ceramics prepared in Comparative Example 12 can withstand a single rod static pressure strength of 790N, which is lower than 800N.
[0264] The composition of the glass ceramics of Comparative Examples 13 to 15 is the same as that of the glass ceramics of Example 1, but a different thickness is used from that of the glass ceramics of Example 1. Finally, although the surface composition of the reinforced glass ceramics obtained in Comparative Examples 13 and 15 can meet the requirements of the present application for reinforced glass ceramics, after testing, the single-rod static pressure strength that the reinforced glass ceramics obtained in Comparative Examples 13 to 15 can withstand is also less than 800N. It can be seen that thickness has a positive effect on improving the compressive resistance of reinforced glass ceramics.
[0265] The above description is only a specific embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A reinforced glass ceramic, It is characterized in that The thickness t of the reinforced glass ceramic is greater than 0.7 mm, preferably, the thickness t is not less than 0.8 mm, and more preferably, the thickness t is not less than 0.9 mm; The reinforced glass ceramic comprises a main crystal phase of zinc aluminum spinel-magnesium aluminum spinel solid solution and a secondary crystal phase of zirconium oxide; the reinforced glass ceramic has a compressive stress layer on the surface and tensile stress inside; The composition at the center of the reinforced glass-ceramic comprises Li 2 O and Na 2 O, and the Li 2 The mass percentage of O is greater than 1.00%, preferably, the Li 2 The mass percentage of O is greater than 1.30%, and more preferably, the Li 2 The mass percentage of O is greater than or equal to 1.50%, and the Na 2 The mass percentage of O is greater than 1.00%, preferably, the Na 2 The mass percentage of O is greater than 2.00%, and more preferably, the Na 2 The mass percentage of O is greater than 2.70%; The surface K of the reinforced glass ceramic is measured in terms of mass percentage of oxides. 2 O mass percentage is 2.00% to 7.50%, preferably, the surface K 2 O mass percentage is 2.50% to 6.50%, more preferably, the surface K 2 The mass percentage of O is 3.00% to 6.00%; The surface Na of the reinforced glass ceramic is measured in terms of the mass percentage of oxides. 2 O mass percentage is less than or equal to 0.010%, preferably, the surface Na 2 O mass percentage is less than or equal to 0.005%, more preferably, the surface Na 2 O mass percentage is less than or equal to 0.002%; The strengthened glass ceramic satisfies: 5.00 μm ≤ DOL_K ≤ 20.00 μm, preferably, 5.50 μm ≤ DOL_K ≤ 18.00 μm, more preferably, 6.00 μm ≤ DOL_K ≤ 16.00 μm, wherein DOL_K is K measured from the main surface of the strengthened glass ceramic. + Diffusion depth.
2. The reinforced glass ceramic according to claim 1, It is characterized in that The reinforced glass ceramic satisfies: along the thickness direction of the reinforced glass ceramic, K + The concentration of the reinforced glass-ceramic decreases nonlinearly from the main surface of the reinforced glass-ceramic toward the center of the reinforced glass-ceramic.
3. The reinforced glass ceramic according to any one of claims 1 to 2, It is characterized in that The composition at the center of the reinforced glass-ceramic contains 30.00% by mass of Al 2 O 3 and / or, the composition at the center of the reinforced glass-ceramic contains ZrO at a mass percentage greater than or equal to 3.00% 2 .
4. The reinforced glass ceramic according to any one of claims 1 to 3, It is characterized in that The thickness t of the reinforced glass ceramic is 0.85 mm to 2.00 mm, preferably, the thickness t is 0.90 mm to 1.50 mm; and / or, The reinforced glass ceramic is 2D, 2.5D, 3D or special-shaped; and / or, The reinforced glass ceramics have uniform thickness or unequal thickness.
5. The reinforced glass ceramic according to any one of claims 1 to 4, It is characterized in that The composition at the center of the reinforced glass-ceramic, measured in percentage by mass of oxides, comprises: SiO 2 :25.00%~55.00%、Al 2 O 3 :30.00%~55.00%、ZrO 2 :3.00%~8.00%、MgO:2.00%~5.00%、ZnO:5.00%~15.00%、Na 2 O:1.00%~10.00%、K 2 O:0%~5.00%、Li 2 O:1.00%~6.00%、CaO:0%~6.00%、B 2 O 3 :0%~10.00%、BaO:0%~10.00%、Y 2 O 3 :0%~6.00%、Sun 2 O 3 :0%~12.00% 6. The reinforced glass ceramic according to any one of claims 1 to 5, It is characterized in that The composition at the center of the reinforced glass-ceramic, measured in percentage by mass of oxides, comprises: SiO 2 The mass percentage is 30.00% to 42.00%, preferably, SiO 2 The mass percentage is 35.00% to 40.00%; and / or, Al 2 O 3 The mass percentage is 32.00% to 42.00%, preferably, Al 2 O 3 The mass percentage is 34.00% to 42.00%; and / or, ZrO 2 The mass percentage is 4.00% to 7.00%, preferably, ZrO 2 The mass percentage is 5.00% to 6.00%; and / or, The mass percentage of MgO is 2.50% to 4.00%, preferably, the mass percentage of MgO is 2.50% to 3.50%; and / or, The mass percentage of ZnO is 9.00% to 13.00%, preferably, the mass percentage of ZnO is 9.00% to 11.00%; and / or, Na 2 The mass percentage of O is 1.00% to 8.00%, preferably, Na 2 The mass percentage of O is 2.00% to 6.00%; and / or, K 2 The mass percentage of O is 0% to 3.00%, preferably, K 2 The mass percentage of O is 0% to 1.00%; and / or, Li 2 The mass percentage of O is 1.00% to 4.00%, preferably, Li 2 The mass percentage of O is 2.00% to 3.00%; and / or, The mass percentage of CaO is 0% to 3.00%, preferably, the mass percentage of CaO is 0% to 1.50%; and / or, B 2 O 3 The mass percentage is 0% to 8.00%, preferably, B 2 O 3 The mass percentage is 0% to 4.00%; and / or, The mass percentage of BaO is 0% to 7.00%, preferably, the mass percentage of BaO is 0% to 4.00%; and / or, Y 2 O 3 The mass percentage is 0% to 4.00%, preferably, Y 2 O 3 The mass percentage is 0% to 2.00%; and / or, La 2 O 3 The mass percentage is 0% to 5.00%, preferably, La 2 O 3 The mass percentage is 0% to 3.00%.
7. The reinforced glass ceramic according to any one of claims 1 to 6, It is characterized in that In terms of percentage by mass of oxides, in the composition at the center of the reinforced glass-ceramic, the Na 2 The mass percentage of O 2 O] and the Li 2 O mass percentage [Li 2 O], satisfying the following relationship: [Na 2 O] / [Li 2 O] = 0.60 to 6.00, preferably 0.90 to 5.00, more preferably 1.00 to 3.00; and / or In the composition at the center of the reinforced glass-ceramic, the Li 2 O mass percentage [Li 2 O] and the SiO 2 The mass percentage [SiO 2 ], satisfying the following relationship: [Li 2 O] / [SiO 2 ]=0.03~0.20, preferably 0.04~0.15, more preferably 0.04~0.
10.
8. The reinforced glass ceramic according to any one of claims 1 to 7, It is characterized in that In the reinforced glass-ceramic, the average crystal size does not exceed 20 nm, preferably 1.0 nm to 10.0 nm, more preferably 4.0 nm to 9.0 nm, more preferably 4.0 nm to 8.0 nm; and / or In terms of mass percentage, the total content of the crystalline phase in the reinforced glass-ceramic is 25% to 60%, preferably 30% to 55%, and more preferably 40% to 50%.
9. The reinforced glass ceramic according to any one of claims 1 to 8, It is characterized in that The reinforced glass ceramic is transparent in the visible light wavelength range. Preferably, at a thickness of 0.90 mm, for light with a wavelength of 550 nm, the transmittance of the reinforced glass ceramic is ≥ 85.00%, preferably ≥ 87.00%.
10. The reinforced glass ceramic according to any one of claims 1 to 9, It is characterized in that The Vickers hardness of the reinforced glass ceramic is greater than or equal to 750 kgf / mm 2 Preferably, the Vickers hardness of the reinforced glass ceramic is greater than or equal to 790 kgf / mm 2 and / or, The fracture toughness value of the reinforced glass ceramic is greater than or equal to 1.00 MPa·m 0.5 Preferably, the fracture toughness value of the reinforced glass ceramic is greater than or equal to 1.20 MPa·m 0.5 More preferably, the fracture toughness value of the reinforced glass-ceramic is greater than or equal to 1.50 MPa·m 0.5 and / or, The reinforced glass-ceramic has a |CT_AV| not exceeding 60 MPa, preferably a |CT_AV| of 4.00 MPa to 55.00 MPa, preferably a |CT_AV| of 4.00 MPa to 20.00 MPa, where |CT_AV| is the absolute value of the average tensile stress; and / or, The reinforced glass-ceramic has a |CT_CV| of no more than 75 MPa, preferably a |CT_CV| of 5.00 MPa to 70.00 MPa, and preferably a |CT_CV| of 6.00 MPa to 25.00 MPa, where |CT_CV| is the absolute value of the maximum tensile stress.
11. The reinforced glass ceramic according to any one of claims 1 to 10, It is characterized in that The surface K of the strengthened glass ceramic 2 O mass percentage is 3.91%, 4.16%, 3.96%, 4.12%, 4.53%, 3.24%, 4.55%, 4.51%, 4.68%, 5.75%, 3.85%, 4.48%, 5.69%, 5.45%, 5.57% or 5.54%; and / or, The DOL_K of the reinforced glass ceramic is 7.70 μm, 9.60 μm, 10.30 μm, 8.40 μm, 10.40 μm, 8.60 μm, 14.10 μm, 12.50 μm, 6.20μm, 9.80μm, 12.80μm, 9.10μm, 8.30μm, 8.80μm, 11.40μm, 10.60μm, 11.80μm or 11.70μm.
12. The reinforced glass ceramic according to any one of claims 1 to 11, It is characterized in that The composition at the center of the reinforced glass-ceramic, measured in percentage by mass of oxides, comprises: SiO 2 The mass percentage is 37.08%, 36.87%, 33.23%, 37.43%, 37.40%, 38.33%, 36.05%, 35.67%, 32.39%, 37.50%, 35.64%, 37.32% or 36.31%; and / or, Al 2 O 3 The mass percentage is 35.83%, 36.98%, 36.27%, 37.52%, 36.60%, 37.07%, 34.84%, 34.55%, 35.88%, 38.63%, 36.23% or 35.10%; and / or, ZrO 2 The mass percentage is 5.69%, 5.65%, 5.61%, 5.74%, 5.81%, 5.89%, 5.54%, 5.48%, 5.76%, 5.72%, 5.99% or 5.58%; and / or, The mass percentage of MgO is 3.00%, 2.98%, 3.04%, 3.03%, 3.06%, 3.10%, 2.92%, 2.89%, 3.01%, 3.27% or 2.94%; and / or, The mass percentage of ZnO is 10.77%, 10.71%, 10.55%, 10.87%, 11.01%, 11.15%, 10.46%, 10.37%, 12.50%, 10.82%, 11.33% or 10.54%; and / or, Na 2 The mass percentage of O is 2.86%, 2.85%, 2.89%, 3.00%, 1.69%, 2.79%, 2.76%, 3.31%, 4.61%, 3.01% or 8.00%; and / or, Preferably without K 2 O; and / or, Li 2 The mass percentage of O is 2.35%, 1.55%, 1.50%, 1.77%, 1.60%, 1.62%, 2.28%, 2.27%, 2.24%, 1.60%, 1.57%, 2.85% or 1.53%; and / or, The mass percentage of CaO is 0%, 0.75%, 1.15% or 0.92%; and / or, B 2 O 3 The mass percentage of is 0% or 7.07%; and / or, The mass percentage of BaO is 2.42%, 2.41%, 6.94%, 0%, 2.35% or 2.32%; and / or, Y 2 O 3 The mass percentage of is 0%, 1.52% or 0.60%; and / or, La 2 O 3 The mass percentage is 0%, 2.17% or 3.69%.
13. The reinforced glass ceramic according to any one of claims 1 to 12, It is characterized in that In the reinforced glass-ceramic, the average crystal size is 5.0nm, 6.8nm, 6.4nm, 6.5nm, 8.1nm, 7.0nm, 6.1nm, 5.1nm or 6.2nm; and / or In terms of mass percentage, the total crystalline content of the reinforced glass-ceramic is 48.69%, 45.11%, 49.52%, 47.85%, 54.07%, 51.56%, 45.49%, 44.77%, 52.28%, 35.52%, 48.75% or 44.33%.
14. The reinforced glass ceramic according to any one of claims 1 to 13, It is characterized in that The Vickers hardness of the reinforced glass ceramic is 840 kgf / mm 2 、848kgf / mm 2 、855kgf / mm 2 、879kgf / mm 2 、889kgf / mm 2 、836kgf / mm 2 、911kgf / mm 2 、897kgf / mm 2 、807kgf / mm 2 、894kgf / mm 2 、883kgf / mm 2 、873kgf / mm 2 、795kgf / mm 2 、863kgf / mm 2 、850kgf / mm 2 、856kgf / mm 2 or 860kgf / mm 2 and / or, The fracture toughness value of the reinforced glass ceramic is 1.64 MPa·m 0.5 、1.65MPa·m 0.5 , 1.66MPa·m 0.5 , 1.70MPa·m 0.5 , 1.71MPa·m 0.5 , 1.63MPa·m 0.5 , 1.74MPa·m 0.5 , 1.72MPa·m 0.5 , 1.59MPa·m 0.5 , 1.69MPa·m 0.5 、1.57MPa·m 0.5 or 1.67MPa·m 0.5 and / or, The |CT_AV| of the strengthened glass-ceramic is 6.68 MPa, 5.85 MPa, 12.45 MPa, 5.45 MPa, 7.33 MPa, 7.79 MPa, 10.91 MPa, 14.64 MPa, 9.98 MPa, 6.25 MPa, 13.15 MPa, 8.58 MPa, 6.33 MPa, 7.91 MPa, 10.75 MPa, 12.77 MPa, 13.58 MPa, 9.47 MPa or 7.98 MPa; and / or, The |CT_CV| of the strengthened glass-ceramic is 7.87 MPa, 6.96 MPa, 15.32 MPa, 6.84 MPa, 8.12 MPa, 9.01 MPa, 11.79 MPa, 17.92 MPa, 11.70 MPa, 7.76 MPa, 15.90 MPa, 9.45 MPa, 8.68 MPa, 9.13 MPa, 12.07 MPa, 14.12 MPa, 15.74 MPa, 10.75 MPa or 9.02 MPa.
15. The reinforced glass ceramic according to any one of claims 1 to 14, It is characterized in that A 10mm diameter round-headed metal pressure rod is used to gradually apply a load vertically downward at a rate of 10mm / min to squeeze the center of the main surface of the reinforced glass-ceramic to test the single-rod static pressure strength that the reinforced glass-ceramic can withstand. The single-rod static pressure strength that the reinforced glass-ceramic can withstand is greater than 800N.
16. The reinforced glass ceramic according to any one of claims 1 to 15, It is characterized in that The reinforced glass ceramic has a fracture toughness of not less than 1.40 MPa·m 0.5 The glass ceramic is obtained by chemical strengthening treatment, preferably, the strengthened glass ceramic has a fracture toughness of not less than 1.40 MPa·m 0.5 The glass ceramic is obtained by a single-step chemical strengthening treatment, and more preferably, the fracture toughness is not less than 1.40 MPa·m 0.5 The glass ceramic is placed in a molten salt bath containing potassium salt with a mass percentage of potassium salt greater than or equal to 90%, and subjected to a single-step chemical strengthening treatment to obtain the strengthened glass ceramic.
17. A cover glass, It is characterized in that The cover glass is made of the tempered glass ceramic according to any one of claims 1 to 16.
18. An electronic device, It is characterized in that The electronic device comprises the reinforced glass-ceramic as described in any one of Claims 116.
19. The electronic device according to claim 18, It is characterized in that The electronic device comprises a housing comprising the reinforced glass-ceramic according to any one of claims 1-16.
20. The electronic device according to claim 19, It is characterized in that The housing comprises a display cover plate, and the display cover plate comprises the strengthened glass-ceramic according to any one of claims 1-16.
21. The electronic device according to claim 19 or 20, It is characterized in that The housing comprises a back cover comprising the reinforced glass-ceramic according to any one of claims 1-16.
22. The electronic device according to any one of claims 19 to 21, It is characterized in that The electronic device further comprises a camera assembly, the housing comprises a camera protection cover, the camera protection cover is disposed on the camera assembly, and the camera protection cover comprises the reinforced glass ceramic according to any one of claims 1-16.
23. The electronic device according to any one of claims 18 to 22, It is characterized in that The electronic device further comprises a middle frame, wherein the middle frame comprises the reinforced glass ceramic according to any one of claims 1 to 16.
24. A glass device, It is characterized in that The glass device comprises the strengthened glass-ceramic according to any one of claims 1 to 16.
Citation Information
Patent Citations
Microcrystalline glass for 5G intelligent communication equipment backboard and preparation method of microcrystalline glass
CN113816611A
Spinel microcrystalline glass capable of being chemically strengthened as well as preparation method and application of spinel microcrystalline glass
CN115010369A
Compression-resistant deep sea transparent microcrystalline glass and preparation method thereof
CN116903253A
Toughened glass ceramic with high strength and application thereof
CN117776534A
Glass ceramic substrate for magnetic storage medium
JP2002308647A
Cited By
Chemically strengthened microcrystalline glass and preparation thereof
CN121672942A
Chemically strengthened microcrystalline glass and preparation thereof
CN121672942B
Precursor glass for preparing spinel glass ceramics
CN121698567A
Spinel glass ceramic and preparation method thereof
CN121698570A
Spinel microcrystalline glass and preparation method thereof
CN121698570B