A production process for LMC with high metal density

By analyzing film surface morphology and calculating deposition characteristics, the method optimizes the working current in the LMC process to enhance film quality and deposition rate, addressing defects and non-uniformity issues.

CN118754456BActive Publication Date: 2024-12-06INNETECH TIANJIN ELECTRONICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411219547.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-12-06
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

The challenge in the LMC process is determining the appropriate working current to achieve high metal density without defects such as large particles, cracks, and holes in the film, while maintaining efficient film deposition rates, as excessive current can lead to non-uniformity and reduced production efficiency.

Method used

A method involving ultrasonic cleaning, surface pretreatment, and metallization steps, followed by image analysis to detect connected domains and calculate target material deposition characteristics, allowing for the determination of an optimal working current based on film deposition rate and particle distribution coefficients.

Benefits of technology

This approach reduces the occurrence of defects like pits and cracks, optimizing the working current for improved film deposition rates and substrate quality by adaptively selecting the most suitable current for different substrates and metal targets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754456B_ABST
    Figure CN118754456B_ABST
Patent Text Reader

Abstract

The present application relates to the field of metallization coating technology, and specifically to a high metal density LMC production process method. The method comprises: obtaining a coated glass substrate after ultrasonic cleaning, surface pretreatment, and metallization; obtaining coating efficiency and coating surface image; obtaining target material deposition characteristic values ​​of the connected domain by analyzing all pixel points and edge pixel points of each connected domain of the coating surface image; classifying the connected domains by the characteristic values ​​of all connected domains, and obtaining the target material deposition particle distribution coefficient of a class with large characteristic values; obtaining the optimal working current of the glass substrate according to the target material deposition particle distribution coefficient and the efficiency of coating, and manufacturing the LMC film based on the optimal working current. The present application improves the film deposition rate of the substrate while reducing the quality problem of the target material deposition particle area with large particles on the film surface of the substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of metallization coating, and in particular to a production process method of LMC with high metal density. Background Art

[0002] The LMC process is a method that uses atomic-level electromagnetic impact to achieve metallization coating on non-metal surfaces. Compared with the traditional PVD metallization coating method, the LMC process does not require primer treatment, and the substrate is not restricted. It can be widely used in non-metallic materials such as plastics, glass, and ceramics, and has a higher coating speed;

[0003] In the metallization coating process of the LMC process, the magnitude of the working current directly affects the quality and deposition rate of the film on the substrate surface. However, due to the different target materials, such as metals, ceramics, compounds, etc., and the different requirements for film performance, such as hardness, wear resistance, optical properties, etc., it is difficult for workers to determine the appropriate working current. Excessive working current may cause defects such as large particles, cracks, and holes on the surface of the film, affecting the uniformity and density of the film. Excessive working current may cause the film deposition rate to be too slow, affecting production efficiency. Summary of the invention

[0004] In order to solve the technical problem that the working current affects the film layer sedimentation, the present application provides a high metal density LMC production process method, and the technical solution adopted is as follows:

[0005] The present application proposes a method for producing LMC with high metal density, which comprises the following steps:

[0006] Under any working current, the glass substrate is subjected to an ultrasonic cleaning step, a surface pretreatment step, and a metallization step to obtain a coated glass substrate; the coating efficiency is calculated according to the coating thickness and the coating time; an image of the surface of the glass substrate after coating is collected, and a surface morphology image of the film layer is obtained after preprocessing the surface image;

[0007] The surface topography image of the film layer is subjected to edge detection and connected domain analysis to obtain several connected domains, and the target material deposition characteristic values ​​of the connected domains are obtained according to the gray value distribution and difference of all pixels in the connected domains, the gradient of the pixels at the edge of the connected domains, and the difference between the gray value and the overall gray value of the surface topography image of the film layer;

[0008] All connected domains are divided into two categories according to the size of the target material deposition characteristic value, and the target material deposition particle distribution coefficient of the glass substrate under the working current is obtained according to the area of ​​all connected domains of the category with the larger target material deposition characteristic value;

[0009] The optimal working current of the glass substrate is obtained according to the target material deposition particle distribution coefficient and the coating efficiency of the glass substrate under the working current, and the LMC film is manufactured based on the optimal working current.

[0010] In the above scheme, the present application constructs the target material deposition particle feature value according to the grayscale distribution complexity and edge clarity constructed based on the distribution of each connected domain in the surface morphology image of the film layer of the glass substrate by analyzing the distribution characteristics between the target material deposition particle region formed by the target material droplet in the film layer and the pits, cracks and other regions formed by the high-speed impact of the metal atoms and metal ions generated on the surface of the metal target material, and the beneficial effect is that the possibility of the pits, cracks and other regions formed by the high-speed impact of the metal atoms and metal ions generated on the surface of the metal target material in the surface morphology image of the film layer of the glass substrate being identified as the target material deposition particle region appearing in the film layer is reduced;

[0011] The target material deposition particle distribution coefficient is constructed according to the distribution of connected domains in the target material deposition particle area set obtained according to the characteristic values ​​of the target material deposition particles, and the working current suitability index is constructed in combination with the film deposition rate. The most suitable working current for LMC metallization coating of the glass substrate is obtained based on the working current suitability index. The beneficial effect lies in that the distribution of larger target material deposition particle areas and the film deposition rate that appear on the substrate during LMC metallization coating are taken into account, and the most suitable working current can be adaptively obtained when LMC metallization coating is performed on different substrates using different metal targets, thereby improving the film deposition rate of the substrate while reducing the quality problem of target material deposition particle areas with large particles on the film surface of the substrate.

[0012] In one embodiment, when the glass substrate is subjected to metallization coating in the metallization step, the voltage used is 600V-1000V.

[0013] In one embodiment, the method for calculating the efficiency of the coating according to the thickness of the coating and the coating time is:

[0014] The average thickness of the film layer on the surface of the glass substrate is obtained by a surface profile measuring instrument, and the ratio of the average thickness of the film layer on the surface of the glass substrate to the deposition time of the film layer on the surface of the glass substrate is used as the film deposition rate of the glass substrate under the working current.

[0015] In one embodiment, the method for obtaining the target material deposition characteristic value of the connected domain according to the gray value distribution and difference of all pixels in the connected domain, the gradient of the pixels at the edge of the connected domain, and the difference between the gray value and the overall gray value of the film layer surface topography image is:

[0016] Calculate the standard deviation of the grayscale values ​​of all pixels in the connected domain; count the number of grayscale levels of all pixels in the connected domain, and obtain the grayscale distribution complexity of the connected domain according to the number of grayscale levels in the connected domain and the standard deviation of the grayscale values ​​of all pixels;

[0017] The grayscale distribution complexity of the connected domain is positively correlated with the number of grayscale levels in the connected domain and the standard deviation of all grayscale values ​​in the connected domain;

[0018] Count all edge pixels in a connected domain, group all edge pixels in a connected domain into a pixel set, and calculate the gradient amplitude of each pixel in the pixel set; calculate the mean of the gradient amplitudes of all pixels in the pixel set and the mean of the grayscale values ​​of all pixels, which are recorded as the first amplitude mean and the first grayscale mean, respectively;

[0019] The grayscale value average of all pixels in the film layer surface topography image is recorded as the second grayscale average;

[0020] Obtain edge clarity of the connected domain according to the difference between the first grayscale mean, the second grayscale mean, and the first amplitude mean;

[0021] The edge clarity of the connected domain is positively correlated with the difference between the first grayscale mean and the second grayscale mean, and the edge clarity of the connected domain is positively correlated with the first amplitude mean of the connected domain;

[0022] Obtaining target material deposition characteristic values ​​of the connected domain according to edge clarity of the connected domain and grayscale distribution complexity of the connected domain;

[0023] The target deposition characteristic values ​​of the connected domain are positively correlated with the edge clarity of the connected domain and the complexity of the grayscale distribution of the connected domain.

[0024] In the above scheme, the characteristic value of the target material deposition particles is constructed according to the grayscale distribution complexity and edge clarity constructed according to the distribution of each connected domain in the surface morphology image of the film layer of the glass substrate. The beneficial effect is that it reduces the possibility of pits, cracks and other areas formed by the high-speed impact of metal atoms and metal ions generated on the surface of the metal target material in the surface morphology image of the film layer of the glass substrate being identified as target material deposition particle areas appearing in the film layer.

[0025] In one embodiment, the method for obtaining the grayscale distribution complexity of the connected domain according to the number of grayscale levels in the connected domain and the standard deviation of the grayscale values ​​of all pixels is:

[0026] Let the product of the number of gray levels in the connected domain and the standard deviation of all gray values ​​in the connected domain be the gray distribution complexity of the connected domain.

[0027] In one embodiment, the method for obtaining the edge clarity of the connected domain according to the difference between the first grayscale mean value, the second grayscale mean value, and the first amplitude mean value is:

[0028] The absolute value of the difference between the first grayscale mean and the second grayscale mean is recorded as the first grayscale difference, and the product of the first grayscale difference and the first amplitude mean is taken as the edge clarity of the connected domain.

[0029] In one embodiment, the method for obtaining the target material deposition characteristic value of the connected domain according to the edge clarity of the connected domain and the grayscale distribution complexity of the connected domain is:

[0030] The product of the edge clarity of the connected domain and the grayscale distribution complexity of the connected domain is taken as the target deposition characteristic value of the connected domain.

[0031] In one embodiment, the method for obtaining the target material deposition particle distribution coefficient of the glass substrate under the working current by using the area of ​​all connected domains of a class with large target material deposition characteristic values ​​is:

[0032] After all connected domains are divided into two categories according to the size of the target material deposition characteristic value, the connected domains in the category with a larger mean value of the target material deposition characteristic value are marked, and all marked connected domains are taken as a set and recorded as a target material deposition particle region set;

[0033] Obtain the number of pixel points of each connected domain in the target material deposition particle region set in the film layer surface topography image, and record it as the area of ​​each connected domain in the target material deposition particle region set;

[0034] The variation of the areas of all connected domains in the target material deposition particle region set is calculated and recorded as the first coefficient of variation, and the inverse of the first coefficient of variation is used as the target material deposition particle distribution coefficient of the glass substrate under the working current.

[0035] In one embodiment, the method for obtaining the optimal working current of the glass substrate according to the target material deposition particle distribution coefficient and the coating efficiency of the glass substrate under the working current is:

[0036] Obtaining a suitable working current index for the glass substrate at the working current according to a film deposition rate of the glass substrate at the working current and a target material deposition particle distribution coefficient of the glass substrate at the working current;

[0037] The working current suitability index of the glass substrate under the working current is positively correlated with the film deposition rate of the glass substrate under the working current and the target material deposition particle distribution coefficient of the glass substrate under the working current.

[0038] The optimal working current is obtained through working current suitability indexes of multiple glass substrates under working currents.

[0039] In one embodiment, the method for obtaining the optimal working current through working current suitability indexes of multiple glass substrates under working currents is:

[0040] Obtaining a working current suitability index of the glass substrate under a preset number of working currents;

[0041] Obtaining a working current suitability index corresponding to a maximum working current and a working current suitability index corresponding to a minimum working current;

[0042] All working current suitability indexes are curve-fitted, and the working current corresponding to the maximum working current suitability index is recorded as the optimal working current.

[0043] The beneficial effects of this application are as follows:

[0044] The present application constructs a target material deposition particle feature value by analyzing the distribution characteristics between the target material deposition particle region formed by the target material droplet in the film layer and the pits, cracks and other regions formed by the high-speed impact of metal atoms and metal ions generated on the surface of the metal target material, and constructs the grayscale distribution complexity and edge clarity constructed according to the distribution of each connected domain in the surface morphology image of the film layer of the glass substrate. The beneficial effect is that the possibility of pits, cracks and other regions formed by the high-speed impact of metal atoms and metal ions generated on the surface of the metal target material in the surface morphology image of the film layer of the glass substrate being identified as the target material deposition particle region appearing in the film layer is reduced;

[0045] The target material deposition particle distribution coefficient is constructed according to the distribution of connected domains in the target material deposition particle area set obtained according to the characteristic values ​​of the target material deposition particles, and the working current suitability index is constructed in combination with the film deposition rate. The most suitable working current for LMC metallization coating of the glass substrate is obtained based on the working current suitability index. The beneficial effect lies in that the distribution of larger target material deposition particle areas and the film deposition rate that appear on the substrate during LMC metallization coating are taken into account, and the most suitable working current can be adaptively obtained when LMC metallization coating is performed on different substrates using different metal targets, thereby improving the film deposition rate of the substrate while reducing the quality problem of target material deposition particle areas with large particles on the film surface of the substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] In order to more clearly illustrate the technical solutions and advantages in the embodiments of the present application or the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0047] Figure 1A flow chart of a high metal density LMC production process provided by one embodiment of the present application;

[0048] Figure 2 A specific flow chart for obtaining target deposition characteristic values. DETAILED DESCRIPTION

[0049] In order to further explain the technical means and effects adopted by the present application to achieve the predetermined invention purpose, the following is a detailed description of a high metal density LMC production process method proposed in the present application, its specific implementation method, structure, features and effects, in conjunction with the accompanying drawings and preferred embodiments. In the following description, different "one embodiment" or "another embodiment" does not necessarily refer to the same embodiment. In addition, specific features, structures or characteristics in one or more embodiments may be combined in any suitable form.

[0050] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs.

[0051] An embodiment of a high metal density LMC production process method:

[0052] The specific scheme of a high metal density LMC production process method provided by the present application is described in detail below with reference to the accompanying drawings.

[0053] See also Figure 1 , which shows a flow chart of a high metal density LMC production process method provided by an embodiment of the present application, the method comprising the following steps:

[0054] Step S001, under any working current, obtain a coated glass substrate after the glass substrate is subjected to an ultrasonic cleaning step, a surface pretreatment step, and a metallization step; calculate the coating efficiency according to the coating thickness and the coating time; collect an image of the surface of the glass substrate after coating, and obtain a surface morphology image of the film layer after preprocessing the surface image.

[0055] The process of processing the LMC film in the LMC preparation process includes a cleaning step, a surface pretreatment step and a metallization step.

[0056] In the ultrasonic cleaning step, the glass substrate is placed in a cleaning tank solution for ultrasonic cleaning to remove dirt remaining on the surface of the glass substrate, and then the glass substrate after ultrasonic cleaning is cleaned using pure water with a pH of 7.

[0057] In the surface pretreatment step, the surface of the glass substrate after ultrasonic cleaning is plasma cleaned. Argon gas is used for plasma cleaning. Argon gas is separated into argon ions under the action of the electrode. The argon ions fly to the negative electrode to perform ion cleaning on the surface. The voltage during plasma cleaning is 100V.

[0058] In the metallization step, when the glass substrate is metallized, a metal target is selected. Then, under a preset voltage, the staff selects a working current, and then uses glow discharge to allow argon ions to impact the target, generating metal nuclei and metal ions that impact the surface of the glass substrate alternately at high speed under the action of the electric field. Then, wait for the mold layer on the surface of the glass substrate to settle for several hours.

[0059] Preferably, in one embodiment, the metal target material can be aluminum metal, the preset voltage is 600V, and the precipitation time is 3 hours;

[0060] Preferably, in one embodiment, the metal target material can be nickel metal, the preset voltage is 800V, and the precipitation time is 2 hours;

[0061] Preferably, in one embodiment, the metal target material may be aluminum metal, the preset voltage is 1000 V, and the precipitation time is 4 hours.

[0062] The average thickness of the film layer on the surface of the glass substrate after LMC metallization coating was obtained using a surface profiler, and the ratio between the obtained average thickness of the film layer and the deposition time of the film layer on the surface of the glass substrate was recorded as the film layer deposition rate of the glass substrate under the working current.

[0063] A scanning electron microscope is used to collect the surface morphology image of the glass substrate after LMC metallization coating. The surface morphology image is a grayscale image, and a Gaussian filter is used to denoise the collected surface morphology image to reduce the influence of environmental noise on subsequent data processing. Gaussian filtering is a well-known technology, and the specific process is not repeated here. The denoised image is recorded as the film layer surface morphology image of the glass substrate.

[0064] At this point, the surface morphology image of the film layer and the film deposition rate of the glass substrate under the working current were obtained.

[0065] Step S002, obtain several connected domains through edge detection and connected domain analysis of the film surface morphology image, and obtain the target material deposition characteristic value of the connected domain based on the gray value distribution and difference of all pixels in the connected domain, the gradient of the pixels at the edge of the connected domain, and the difference between the gray value and the overall gray value of the film surface morphology image.

[0066] Generally speaking, during the LMC metallization coating process, as the working current increases, the current density formed on the surface of the metal target will increase, which will cause the local temperature of the metal target surface to rise, and then form target droplets. If the working current is too large, the current density on the target surface will be too high, and larger target droplets will be produced, and more serious target droplet splashing may occur.

[0067] When coating thin films, such large-particle target droplets cannot fully react with the gas in the vacuum chamber, and a target material deposition particle area formed by the aggregation of large target material particles will appear in the high-hardness film layer, and the target material deposition particle area appearing in the film layer will appear as a circular or irregular shape in the surface morphology image of the film layer. However, the metal atoms and metal ions generated on the surface of the metal target will alternately impact the surface of the plated object at high speed under the action of the electric field, thereby forming pits, cracks and other areas on the surface of the plated object, and these areas may also appear as a circular or irregular shape in the surface morphology image of the film layer.

[0068] Based on the above analysis, in order to reduce the possibility that pits, cracks and other areas formed by the high-speed impact of metal atoms and metal ions generated on the surface of the metal target material in the film layer surface topography image of the glass substrate are identified as target material deposition particle areas appearing in the film layer, the Canny edge detection algorithm is used to obtain the edge image of the film layer surface topography image of the glass substrate, which is used to characterize the boundary information of the target material deposition particle areas, pits, cracks and other areas in the film layer surface topography image. The edge image is a binary image.

[0069] It should be noted that in this embodiment, the purpose of the Canny edge detection algorithm is to obtain the edge image of the film surface morphology image, and it has no other function. Therefore, the implementer can obtain the edge image of the film surface morphology image by other methods of obtaining edge images, such as the Sobel operator.

[0070] The connected domain analysis is performed on the edge image using the two-side scanning method to obtain several connected domains in the film surface morphology image.

[0071] It should be noted that, in this embodiment, the two-side scanning method is used to analyze the connected domain of the edge image, so the implementer can use other algorithms for connected domain analysis, such as the seed filling method, to process.

[0072] Since the surface of the target material deposited particle area formed by the target material droplets in the film layer has a higher roughness than the surrounding film layer, and the microstructure (such as grain size, porosity) of the target material deposited particle area is different from the surrounding film layer, the light will be scattered in different ways, which will cause the target material deposited particle area to present a more complex grayscale distribution feature and clearer edge feature in the surface morphology image of the film layer, while the pits, cracks and other areas formed by the impact of metal atoms and metal ions in the surface morphology image of the film layer have a closer roughness and a more similar microstructure to the surrounding areas, so that the pits, cracks and other areas have a relatively single grayscale distribution feature and unclear edge features in the surface morphology image of the film layer.

[0073] Through the above analysis, for each connected domain of the film surface morphology image, the standard deviation of the grayscale values ​​of all pixels in the connected domain is calculated; the number of grayscale levels of all pixels in the connected domain is counted, and the grayscale distribution complexity of the connected domain is obtained according to the number of grayscale levels in the connected domain and the standard deviation of the grayscale values ​​of all pixels.

[0074] The grayscale distribution complexity of the connected domain is positively correlated with the number of grayscale levels in the connected domain and the standard deviation of all grayscale values ​​in the connected domain.

[0075] It should be noted that positive correlation means that when one variable increases, the other variable also increases, and the two variables change in the same direction. When one variable changes from large to small or from small to large, the other variable also changes from large to small or from small to large. The specific relationship can be a multiplication relationship, an addition relationship, or the idempotence of an exponential function, which is determined by actual application and is not specifically limited in this application.

[0076] Preferably, in one embodiment of the present application, the product of the number of gray levels in a connected domain and the standard deviation of all gray values ​​in the connected domain is taken as the gray distribution complexity of the connected domain.

[0077] Preferably, in one embodiment of the present application, the number of gray levels in the connected domain is taken as the true number of the logarithmic function, the reciprocal of the standard deviation of all gray values ​​in the connected domain is taken as the base of the logarithmic function, and the value of the logarithmic function is taken as the gray distribution complexity of the connected domain.

[0078] Among them, the larger the standard deviation of all gray values ​​in the connected domain and the greater the number of gray levels, the more complex the distribution of pixels in the connected domain is, and the greater the complexity of the gray distribution of the connected domain is.

[0079] Count all edge pixels in a connected domain, group all edge pixels in a connected domain into a pixel set, and calculate the gradient amplitude of each pixel in the pixel set by using the Sobel operator; calculate the mean of the gradient amplitudes of all pixels in the pixel set and the mean of the grayscale values ​​of all pixels, which are recorded as the first amplitude mean and the first grayscale mean, respectively.

[0080] The grayscale value mean of all pixels in the film layer surface topography image is calculated and recorded as the second grayscale mean. The edge clarity of the connected domain is obtained according to the difference between the first grayscale mean, the second grayscale mean and the first amplitude mean.

[0081] The edge clarity of the connected domain is positively correlated with the difference between the first grayscale mean and the second grayscale mean, and the edge clarity of the connected domain is positively correlated with the first amplitude mean of the connected domain.

[0082] Preferably, in one embodiment of the present application, the absolute value of the difference between the first grayscale mean and the second grayscale mean is recorded as the first grayscale difference, and the product of the first grayscale difference and the first amplitude mean is taken as the edge clarity of the connected domain.

[0083] Preferably, in one embodiment of the present application, the absolute value of the difference between the first grayscale mean and the second grayscale mean is recorded as the first grayscale difference, and the square of the sum of the first grayscale difference and the first amplitude mean is taken as the edge clarity of the connected domain.

[0084] Among them, the larger the gradient amplitude of the edge pixel points in the connected domain, the larger the first amplitude mean, and the larger the difference between the grayscale value of the edge pixel points in the connected domain and the grayscale values ​​of the surrounding pixels, the larger the first grayscale difference, then the higher the contrast between the edge of the connected domain and its surrounding area, the higher the clarity at the edge of the connected domain, and the greater the edge clarity.

[0085] The target material deposition characteristic value of the connected domain is obtained according to the edge clarity of the connected domain and the grayscale distribution complexity of the connected domain. The specific process of obtaining the target material deposition characteristic value is as follows: Figure 2 shown.

[0086] The target deposition characteristic values ​​of the connected domain are positively correlated with the edge clarity of the connected domain and the complexity of the grayscale distribution of the connected domain.

[0087] Preferably, in one embodiment of the present application, the product of the edge clarity of the connected domain and the grayscale distribution complexity of the connected domain is used as the target material deposition characteristic value of the connected domain.

[0088] Preferably, in one embodiment of the present application, the sum of the squares of the edge clarity of the connected domain and the grayscale distribution complexity of the connected domain is used as the target material deposition characteristic value of the connected domain.

[0089] Among them, the more complex the distribution of the grayscale values ​​of the pixels in the connected domain, the greater the complexity of the grayscale distribution, and the higher the clarity at the edge of the connected domain, the greater the edge clarity, the more likely the connected domain is to be the target material deposition particle area in the film surface morphology image, and the greater the target material deposition characteristic value.

[0090] Step S003, dividing all connected domains into two categories according to the size of the target deposition characteristic value, and obtaining the target deposition particle distribution coefficient of the glass substrate under the working current according to the area of ​​all connected domains of the category with the larger target deposition characteristic value.

[0091] The target material deposition characteristic values ​​of all connected domains in the film surface morphology image are obtained, and all target material deposition characteristic values ​​are used as the input of the maximum inter-class variance. The output is the target material deposition threshold, which is used to subsequently screen out the connected domains in the film surface morphology image that are suspected to be target material deposition particle areas.

[0092] The connected domains in the film surface topography image whose target deposition characteristic values ​​are greater than the target deposition threshold are marked. The marked connected domains may be connected domains suspected to be target deposition particle regions in the film surface topography image. The marked connected domains are placed in a set, and this set is recorded as the target deposition particle region set.

[0093] It should be noted that the role of the maximum inter-class variance in this embodiment is to divide all connected domains into two categories based on the target material deposition characteristic values. The implementer can also use other methods to divide the connected domains into two categories based on the target material deposition characteristic values, such as taking the mean as the threshold to divide the connected domains into two categories.

[0094] The number of pixel points of each connected domain in the target material deposition particle area set in the film surface topography image is obtained and recorded as the area of ​​each connected domain in the target material deposition particle area set, which is used to characterize the distribution of the area size of the target material deposition particle area in the surface topography image.

[0095] The variation of the areas of all connected domains in the target material deposition particle region set is calculated and recorded as the first coefficient of variation, and the inverse of the first coefficient of variation is used as the target material deposition particle distribution coefficient of the glass substrate under the working current.

[0096] The larger the area of ​​the connected domain, the smaller the coefficient of variation, and the larger the distribution coefficient of the target material deposition particles; the closer the areas between the connected domains, the smaller the standard deviation, the smaller the coefficient of variation, and the larger the distribution coefficient of the target material deposition particles. If the area of ​​the connected domain is larger and the areas between the connected domains are closer, it means that the number of target material deposition particle areas is larger, the target material deposition particle areas are more similar, the larger the distribution coefficient of the target material deposition particles, and the worse the film quality obtained by coating the glass substrate under the working current I.

[0097] At this point, the target material deposition particle distribution coefficient of the glass substrate under the working current is obtained.

[0098] Step S004, obtaining the optimal working current of the glass substrate according to the target material deposition particle distribution coefficient and the coating efficiency of the glass substrate under the working current, and manufacturing the LMC film based on the optimal working current.

[0099] The working current suitability index of the glass substrate under the working current is obtained according to the film deposition rate of the glass substrate under the working current and the target material deposition particle distribution coefficient of the glass substrate under the working current.

[0100] The working current suitability index of the glass substrate under the working current is positively correlated with the film deposition rate of the glass substrate under the working current and the target material deposition particle distribution coefficient of the glass substrate under the working current.

[0101] Preferably, in one embodiment of the present application, the product of the film deposition rate of the glass substrate under the working current and the target material deposition particle distribution coefficient of the glass substrate under the working current is used as the film deposition rate of the glass substrate under the working current and the target material deposition particle distribution coefficient of the glass substrate under the working current.

[0102] Preferably, in one embodiment of the present application, the average of the film deposition rate of the glass substrate under the working current and the target material deposition particle distribution coefficient of the glass substrate under the working current is used as the film deposition rate of the glass substrate under the working current and the target material deposition particle distribution coefficient of the glass substrate under the working current.

[0103] Obtain a suitable working current index of the glass substrate under N working currents. In this embodiment, N is 50, and the implementer can select the value by himself. Obtain a maximum working current I1 and a minimum working current I2 when the glass substrate is subjected to LMC metallization coating, construct a coordinate system with the working current as the horizontal coordinate and the suitable working current index as the vertical coordinate, perform curve fitting on the data points in the coordinate system, obtain the data point with the largest vertical coordinate within the horizontal coordinate range [I2, I1] of the obtained fitting curve, record the working current corresponding to the obtained data point as the most suitable working current IM when the glass substrate is subjected to LMC metallization coating, and use the working current IM to perform LMC metallization coating on the subsequent glass substrate to manufacture a LMC film with high metal density.

Claims

1. A process for producing LMC with high metal density, characterized in that: The method comprises the following steps: Under any working current, the glass substrate is subjected to an ultrasonic cleaning step, a surface pretreatment step, and a metallization step to obtain a coated glass substrate; the coating efficiency is calculated according to the coating thickness and the coating time; an image of the surface of the glass substrate after coating is collected, and a surface morphology image of the film layer is obtained after preprocessing the surface image; The surface topography image of the film layer is subjected to edge detection and connected domain analysis to obtain several connected domains, and the target material deposition characteristic values ​​of the connected domains are obtained according to the gray value distribution and difference of all pixels in the connected domains, the gradient of the pixels at the edge of the connected domains, and the difference between the gray value and the overall gray value of the surface topography image of the film layer; All connected domains are divided into two categories according to the size of the target material deposition characteristic value, and the target material deposition particle distribution coefficient of the glass substrate under the working current is obtained according to the area of ​​all connected domains of the category with the larger target material deposition characteristic value; The optimal working current of the glass substrate is obtained according to the target material deposition particle distribution coefficient and the coating efficiency of the glass substrate under the working current, and the LMC film is manufactured based on the optimal working current; The method for calculating the efficiency of the coating according to the coating thickness and the coating time is: The average thickness of the film layer on the surface of the glass substrate is obtained by a surface profile measuring instrument, and the ratio of the average thickness of the film layer on the surface of the glass substrate to the deposition time of the film layer on the surface of the glass substrate is used as the film deposition rate of the glass substrate under the working current; The method for obtaining the target material deposition characteristic value of the connected domain according to the gray value distribution and difference of all pixels in the connected domain, the gradient of the pixels at the edge of the connected domain, and the difference between the gray value and the overall gray value of the film layer surface topography image is: Calculate the standard deviation of the grayscale values ​​of all pixels in the connected domain; count the number of grayscale levels of all pixels in the connected domain, and obtain the grayscale distribution complexity of the connected domain according to the number of grayscale levels in the connected domain and the standard deviation of the grayscale values ​​of all pixels; The grayscale distribution complexity of the connected domain is positively correlated with the number of grayscale levels in the connected domain and the standard deviation of all grayscale values ​​in the connected domain; Count all edge pixels in a connected domain, group all edge pixels in a connected domain into a pixel set, and calculate the gradient amplitude of each pixel in the pixel set; calculate the mean of the gradient amplitudes of all pixels in the pixel set and the mean of the grayscale values ​​of all pixels, which are recorded as the first amplitude mean and the first grayscale mean, respectively; The grayscale value average of all pixels in the film layer surface topography image is recorded as the second grayscale average; Obtain edge clarity of the connected domain according to the difference between the first grayscale mean, the second grayscale mean, and the first amplitude mean; The edge clarity of the connected domain is positively correlated with the difference between the first grayscale mean and the second grayscale mean, and the edge clarity of the connected domain is positively correlated with the first amplitude mean of the connected domain; Obtaining target material deposition characteristic values ​​of the connected domain according to edge clarity of the connected domain and grayscale distribution complexity of the connected domain; The target deposition characteristic values ​​of the connected domain are positively correlated with the edge clarity of the connected domain and the grayscale distribution complexity of the connected domain. The method for obtaining the target material deposition particle distribution coefficient of the glass substrate under the working current by using the area of ​​all connected domains of a class with large target material deposition characteristic values ​​is: After all connected domains are divided into two categories according to the size of the target material deposition characteristic value, the connected domains in the category with a larger mean value of the target material deposition characteristic value are marked, and all marked connected domains are taken as a set and recorded as a target material deposition particle region set; Obtain the number of pixel points of each connected domain in the target material deposition particle region set in the film layer surface topography image, and record it as the area of ​​each connected domain in the target material deposition particle region set; The variation of the area of ​​all connected domains in the target material deposition particle area set is calculated and recorded as the first coefficient of variation, and the reciprocal of the first coefficient of variation is used as the distribution coefficient of the target material deposition particles on the glass substrate under the working current; The method for obtaining the optimal working current of the glass substrate according to the target material deposition particle distribution coefficient and the coating efficiency of the glass substrate under the working current is: Obtaining a suitable working current index for the glass substrate at the working current according to a film deposition rate of the glass substrate at the working current and a target material deposition particle distribution coefficient of the glass substrate at the working current; The working current suitability index of the glass substrate under the working current is positively correlated with the film deposition rate of the glass substrate under the working current and the target material deposition particle distribution coefficient of the glass substrate under the working current. The optimal working current is obtained through working current suitability indexes of multiple glass substrates under working currents.

2. A high metal density LMC production process as claimed in claim 1, characterized in that: When the glass substrate is subjected to metallization coating in the metallization step, the voltage used is 600V-1000V.

3. A process for producing LMC with high metal density as claimed in claim 1, characterized in that: The method for obtaining the grayscale distribution complexity of the connected domain according to the number of grayscale levels in the connected domain and the standard deviation of the grayscale values ​​of all pixels is: Let the product of the number of gray levels in the connected domain and the standard deviation of all gray values ​​in the connected domain be the gray distribution complexity of the connected domain.

4. A high metal density LMC production process as claimed in claim 1, characterized in that: The method for obtaining the edge clarity of the connected domain according to the difference between the first grayscale mean, the second grayscale mean, and the first amplitude mean is: The absolute value of the difference between the first grayscale mean and the second grayscale mean is recorded as the first grayscale difference, and the product of the first grayscale difference and the first amplitude mean is taken as the edge clarity of the connected domain.

5. A method for producing LMC with high metal density as claimed in claim 1, characterized in that: The method for obtaining the target material deposition characteristic value of the connected domain according to the edge clarity of the connected domain and the grayscale distribution complexity of the connected domain is: The product of the edge clarity of the connected domain and the grayscale distribution complexity of the connected domain is taken as the target deposition characteristic value of the connected domain.

6. A method for producing LMC with high metal density as claimed in claim 1, characterized in that: The method for obtaining the optimal working current through working current suitability indexes of multiple glass substrates under working currents is: Obtaining a working current suitability index of the glass substrate under a preset number of working currents; Obtaining a working current suitability index corresponding to a maximum working current and a working current suitability index corresponding to a minimum working current; All working current suitability indexes are curve-fitted, and the working current corresponding to the maximum working current suitability index is recorded as the optimal working current.