Anti-reflection material and preparation method thereof, photovoltaic glass and optical glass

By using silica hollow particles with different porosity and particle size relationship in the double-layer anti-reflection material, combined with the transparent substrate and coating composition, the applicability and refractive index control problems of the high-temperature calcination method in the existing technology are solved. It achieves applicability to different substrates and good anti-reflection effect.

CN118754459APending Publication Date: 2024-10-11NINGBO DILATO MATERIALS CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202410979275.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The existing method of forming anti-reflective coatings by calcining them at high temperatures cannot be applied to organic polymer substrates that are not resistant to high temperatures, and the refractive index is difficult to control, resulting in poor anti-reflective effects and poor durability.

Method used

Using double-layer anti-reflective material, the base coating and top coating contain silica hollow particles with porosity of 20-60% and 40-70% respectively, and the particle size relationship is set to obtain a low refractive index, which can be used directly It does not require high-temperature calcination and is formed by combining a transparent substrate and a coating composition.

Benefits of technology

The applicability to different substrates is realized, good anti-reflection effect and anti-reflection effect in a wide wavelength range are achieved, while environmental tolerance is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754459A_ABST
    Figure CN118754459A_ABST
Patent Text Reader

Abstract

The invention relates to an antireflection material, which is provided with a transparent substrate, an undercoat layer arranged on the transparent substrate and a top coat layer arranged on the undercoat layer, the refractive index of the top coat layer is smaller than that of the undercoat layer, the undercoat layer contains first hollow silicon dioxide particles, the porosity of the first hollow silicon dioxide particles is 20-60%, and the porosity of the first hollow silicon dioxide particles is 20-60%. The surface coating contains second hollow silicon dioxide particles, and the porosity of the second hollow silicon dioxide particles is 40-70%. According to the antireflection material disclosed by the invention, the bottom coating and the surface coating respectively contain the silicon dioxide hollow particles with different particle sizes, and the average particle size of the transparent substrate and the silicon dioxide hollow particles used for forming the bottom coating and the surface coating is set, so that a good antireflection effect and a wide antireflection wavelength are obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of anti-reflection, in particular to a material with a double anti-reflection layer and a preparation method thereof. Background Art

[0002] In many real-life scenarios, excessive light reflection can cause inconvenience. For example, light reflection from a car's windshield can interfere with the driver's sight, and reflection from glass on mobile phone and computer screens can affect the clarity of displayed content. Reflection from the surface of photovoltaic glass can reduce energy conversion efficiency.

[0003] In the prior art, there is a method of applying an anti-reflection coating on the surface of a substrate such as glass and introducing a pore structure in the coating, thereby effectively reducing the refractive index of the coating and achieving a good anti-reflection effect. In early anti-reflection coatings, solid silica particles were used and the pore structure was introduced by using the gaps between the particles. However, the coating obtained by this method has a low porosity and a general anti-reflection effect. In addition, the gaps between the particles are an open-pore structure, which is easily corroded or blocked and has a short service life.

[0004] At present, there are reports that an anti-reflection coating containing hollow silica particles is formed by applying a coating liquid containing polymer-silica composite particles with core-shell structure and then calcining at high temperature to remove the polymer. For example, patent CN114620950 discloses an anti-reflection coating liquid containing polyacrylic acid-silica composite particles, which removes polypropylene by high-temperature calcination to obtain an anti-reflection coating for use in the field of photovoltaic glass. This method usually requires high-temperature calcination (greater than 500°C) to remove the polymer template, and is not applicable to organic transparent substrates such as polyethylene terephthalate (PET), polymethacrylic acid (PMMA), and polycarbonate (PC).

[0005] In addition, in order to overcome the defects of the single-layer anti-reflection film, such as the narrow effective anti-reflection wavelength range and poor durability, the prior art such as patent CN107572838 discloses a double-layer anti-reflection coating solution using a base coating (in contact with the substrate) formed by silica sol particles and a top coating (exposed to the air) containing composite particles with a core-shell structure, but the anti-reflection coating is also formed by high-temperature calcination and cannot be applied to various organic polymer substrates that are not resistant to high temperatures. In addition, the refractive index of the silica coating is mostly around 1.46, which cannot be flexibly adjusted to achieve different refractive indices, and is difficult to meet the anti-reflection requirements of different substrates.

[0006] Therefore, there is an urgent need for anti-reflection materials that can finely control the refractive index of the coating to meet the usage requirements of different scenarios such as photovoltaic glass, optical glass, automotive anti-reflection films, anti-reflection polarizers, etc. Summary of the invention

[0007] After conducting in-depth research on the above technical issues, the inventors found that the anti-reflection material of the present invention can be applied to transparent substrates such as glass, PET, PMMA, PC, etc., and has a good anti-reflection effect.

[0008] An object of the present invention is to provide an anti-reflection material having a good anti-reflection effect and a wide wavelength of enhanced transmission.

[0009] Another object of the present invention is to provide a method for preparing an anti-reflection material. The method for preparing an anti-reflection material directly uses a composition containing hollow silica particles as a material for a base coat and a top coat, does not require high-temperature calcination, and sets a transparent substrate and a coating composition for forming a base coat and a top coat, thereby obtaining a good anti-reflection effect and a wide anti-reflection wavelength.

[0010] Another object of the present invention is to provide a photovoltaic glass, which contains the aforementioned anti-reflection material. Thus, the photovoltaic glass of the present invention has a good anti-reflection effect and a wide anti-reflection wavelength.

[0011] Another object of the present invention is to provide an optical glass, which contains the aforementioned anti-reflection material. Thus, the optical glass of the present invention has a good anti-reflection effect and a wide anti-reflection wavelength.

[0012] Another object of the present invention is to provide a polarizing plate, which contains the aforementioned anti-reflection material. Thus, the polarizing plate of the present invention has a good anti-reflection effect and a wide anti-reflection wavelength.

[0013] In order to achieve the above object, the present invention provides the following technical solutions:

[0014] [1] An anti-reflection material comprising a transparent substrate, a primer layer on the transparent substrate, and a top layer on the primer layer, wherein the top layer has a refractive index lower than that of the primer layer.

[0015] The undercoat layer contains first hollow silica particles, and the porosity of the first hollow silica particles is 20-60%.

[0016] The top coating layer contains second hollow silica particles, and the porosity of the second hollow silica particles is 40-70%.

[0017] The average particle size D1 of the first hollow silica particles and the refractive index n0 of the transparent substrate satisfy the following relationship 1:

[0018]

[0019] The average particle size D1 of the first hollow silica particles and the average particle size D2 of the second hollow silica particles satisfy the following relationship 2, wherein the value of f is 4.5 to 5.5:

[0020] D2=f×D1.

[0021] [2] A method for preparing the anti-reflection material described in [1], comprising the following steps:

[0022] A first coating composition is applied on the transparent substrate and cured to form a base coating, and then a second coating composition is applied on the base coating and cured to form a top coating.

[0023] Based on 100 parts by mass of the first coating composition, the coating composition comprises:

[0024]

[0025] Based on 100 parts by mass of the second coating composition, the composition comprises:

[0026]

[0027] [3] The method for preparing an anti-reflection material according to [2], wherein the binder is an acidic silica sol or a polymer resin.

[0028] [4] The method for preparing an anti-reflection material according to [3], wherein the polymer resin is a photocurable resin.

[0029] [5] The method for preparing an anti-reflection material according to [4], wherein the photocurable resin is at least one selected from pentaerythritol triacrylate, pentaerythritol tetraacrylate, trimethylolpropane triacrylate, ethoxylated trimethylolpropane triacrylate, ditrimethylolpropane tetraacrylate, dipentaerythritol hexaacrylate, dipropylene glycol diacrylate, aliphatic polyurethane acrylate, and aliphatic polyurethane hexaacrylate.

[0030] [6] The method for preparing an anti-reflection material according to [2], wherein the curing agent is at least one selected from aluminum acetylacetonate, titanium acetylacetonate, photocuring agent 307, TPOJRCure-1108UV, Omnirad 127, and Omnirad 184.

[0031] [7] A photovoltaic glass comprising the anti-reflection material described in [1].

[0032] [8] An optical glass comprising the anti-reflection material described in [1].

[0033] [9] A polarizing plate comprising the anti-reflection material described in [1].

[0034] Effects of the Invention

[0035] The anti-reflection material of the present invention contains hollow silica particles of different particle sizes in the base coat and the top coat, and sets the average particle size of the transparent substrate and the hollow silica particles used to form the base coat and the top coat, thereby obtaining a good anti-reflection effect and a wide anti-reflection wavelength.

[0036] The preparation method of the anti-reflection material of the present invention directly uses a composition containing hollow silica particles as the material of the base coat and the top coat, and does not require high-temperature calcination. In addition, by setting a transparent substrate and a coating composition for forming the base coat and the top coat, a good anti-reflection effect and a wide anti-reflection wavelength are obtained.

[0037] Ultraviolet light curing can be used to form the coating. The coating formed after curing has a low refractive index, excellent anti-reflection effect, and good environmental tolerance. It can be widely used in photovoltaics, displays, automobiles and other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 It is a schematic diagram of the structure of an anti-reflection material in which a base coating and a top coating exist on one side of a transparent substrate.

[0039] Figure 2 These are transmittance curves of the blank glass of Comparative Example 1, the anti-reflection material containing only a top coating prepared in Comparative Example 3, the anti-reflection material containing a primer and a top coating prepared in Comparative Example 5, and the anti-reflection material containing a primer and a top coating prepared in Example 1.

[0040] Figure 3 These are the reflectivity curves of the blank PET film of Comparative Example 2, the PET film containing only the top coating layer prepared in Comparative Example 4, and the PET film containing the primer layer and the top coating layer prepared in Example 2. DETAILED DESCRIPTION

[0041] The present invention is further described below in conjunction with the accompanying drawings and specific examples, but the scope of the present invention is not limited in any way. Unless otherwise stated, the reagents used in the specific examples can be obtained through commercial means or conventional experimental means.

[0042] [Anti-reflective materials]

[0043] The anti-reflection material of the present invention comprises a transparent substrate, a primer layer on the transparent substrate and a top layer on the primer layer, wherein the refractive index of the top layer is lower than that of the primer layer.

[0044] Examples of the transparent substrate include transparent substrates made of materials such as inorganic glass, organic glass, polycarbonate, polyethylene terephthalate (PET), polymethacrylic acid (PMMA), and polycarbonate (PC), but are not particularly limited.

[0045] The primer layer contains first hollow silica particles, wherein the porosity of the first hollow silica particles is 20 to 60%.

[0046] The top coating layer contains second hollow silica particles, wherein the porosity of the second hollow silica particles is 40 to 70%.

[0047] The average particle size D1 of the first hollow silica particles and the refractive index n0 of the transparent substrate satisfy the following relationship 1:

[0048]

[0049] The average particle size D1 of the first hollow silica particles and the average particle size D2 of the second hollow silica particles satisfy the following relationship 2, wherein the value of f is 4.5 to 5.5:

[0050] D2=f×D1.

[0051] The aforementioned “average particle size” refers to the average value of the particle sizes of 500 particles obtained by particle size statistics on transmission electron microscope photographs of hollow silica particles.

[0052] The inventors of the present invention have found in their research that by setting the average particle size D1 of the first hollow silica particles, the average particle size D2 of the second hollow silica particles and the refractive index n0 of the transparent substrate in the anti-reflection material to satisfy the aforementioned relationship, a good anti-reflection effect can be obtained, and a wide anti-reflection wavelength range can be obtained.

[0053] In the antireflection material of the present invention, the primer layer and the topcoat layer may be present on both surfaces of the transparent substrate, or may be present on only one surface of the transparent substrate, as required. Figure 1 A schematic diagram showing a case where a primer layer and a top coat layer are present on one side of a transparent substrate is shown. Figure 1 The low-reflection material shown comprises a transparent substrate 1 , a primer layer 2 , and a top layer 3 . The primer layer 2 contains first hollow silica particles 4 , and the top layer 3 contains second hollow silica particles 5 .

[0054] When the primer and topcoat are present on both sides of the transparent substrate, the composition of the primer on the two sides may be the same or different, preferably the same. When the primer and topcoat are present on both sides of the transparent substrate, the composition of the topcoat on the two sides may be the same or different, preferably the same.

[0055] In some embodiments of the anti-reflection material, the refractive index n0 of the transparent substrate, the average particle size D1 of the first hollow silica particles, and the average particle size D2 of the second hollow silica particles may be the values ​​listed in Table 1 below.

[0056] Table 1 Numerical examples of the refractive index n0 of the transparent substrate, the first hollow silica particles D1 and the second hollow silica particles D2 in the anti-reflection material

[0057]

[0058] The aforementioned anti-reflection material can be prepared by, for example, the method for preparing the anti-reflection material described below.

[0059] [Preparation method of anti-reflection material]

[0060] The method for preparing the anti-reflection material of the present invention comprises the following steps:

[0061] A first coating composition is coated on a transparent substrate and cured to form a base coating, and then a second coating composition is coated on the base coating and cured to form a top coating.

[0062] Based on 100 parts by mass of the first coating composition, the coating composition comprises:

[0063]

[0064] Based on 100 parts by mass of the second coating composition, the composition comprises:

[0065]

[0066] It should be noted that, when the first hollow silica particles and the second hollow silica particles are made of a dispersion liquid as a raw material, their "parts by mass" are calculated according to the solid content of the first hollow silica particles and the second hollow silica particles actually contained in the dispersion liquid. When other raw materials are made of a dispersion liquid, they are calculated similarly according to the solid content.

[0067] The first hollow silica particles and the second hollow silica particles have different average particle sizes, and their sizes are selected according to the refractive index of the coated transparent substrate. By setting the average particle size D1 of the first hollow silica particles, the refractive index n0 of the second hollow silica particles D2 and the transparent substrate to satisfy the following relationship 1 and relationship 2, the value range of f in equation 2 is 4.5 to 5.5. Thus, a good anti-reflection effect can be obtained, and a wide anti-reflection wavelength range is obtained.

[0068] Relation 1:

[0069]

[0070] Relation 2:

[0071] D2=f×D1

[0072] The preparation method of the anti-reflection material directly uses a composition containing hollow silica particles as the material of the base coat and the top coat, does not need to be calcined at high temperature, and can be applied to organic transparent substrates such as polyethylene terephthalate (PET), polymethacrylic acid (PMMA), and polycarbonate (PC). In addition, the average particle size of the hollow silica particles used in the appropriate base coat and the top coat can be selected according to the material of the transparent substrate used to obtain a good anti-reflection effect. The hollow silica particles with an average particle size of D1 added to the base coat can make the refractive index of the base coat lower than the refractive index n0 of the substrate; hollow silica particles with a larger average particle size (D2) are added to the top coat, so that the top coat contains more pores, so that the refractive index of the top coat is lower than the refractive index of the base coat, and the anti-reflection material formed can more effectively reduce the reflection of light on the surface of the substrate.

[0073] In the preparation method of the anti-reflective material of some embodiments, the first coating composition can be prepared as follows: 0.5 to 2.5 parts by mass (solid content) of the first hollow silica particles and 0.6 to 3 parts by mass (solid content) of the binder are dispersed in 50 parts by mass of the solvent, and stirred evenly. Then, 0.002 to 0.05 parts by mass of the leveling agent and 0.1 to 0.5 parts by mass of the curing agent are added, and the solvent is added to make the mass of the final composition 100 parts by mass, and stirred evenly to obtain a dispersion containing the first hollow silica particles. Preferably, a sieve of 500 to 1200 mesh is further used for filtering.

[0074] In the preparation method of the anti-reflective material of some embodiments, the aforementioned second coating composition can be prepared as follows: 0.5 to 2.5 parts by mass (solid content) of the second hollow silica particles and 0.6 to 3 parts by mass (solid content) of the binder are dispersed in 50 parts by mass of the solvent, stirred evenly, and then 0.002 to 0.05 parts by mass of the leveling agent and 0.1 to 0.5 parts by mass of the curing agent are added, and the solvent is added to make the mass of the final composition 100 parts by mass, and stirred evenly to obtain a dispersion containing the second hollow silica particles. Preferably, the dispersion is further filtered using a sieve of 500 to 1200 meshes.

[0075] The coating method of the above-mentioned base coating layer and / or top coating layer can be selected in different coating methods according to the transparent substrate, the composition of the first hollow silica particles, and the second hollow silica particles. For example, a dip coating method, a spin coating method, a floating roller method, a wire rod coating method, etc. can be used without special restrictions.

[0076] The aforementioned curing method can be appropriately selected according to the transparent substrate. For example, when glass is used as the substrate, it can be cured by high temperature calcination, and for polymer substrates, it can be cured by heating at a temperature of 80 to 100° C., or it can also be cured by ultraviolet light initiation.

[0077] Preferably, the transparent substrate is cleaned before the above-mentioned base coating and / or top coating is applied. The above-mentioned cleaning can be carried out by, for example, washing with water or wiping with a clean non-woven fabric.

[0078] The binder used in the aforementioned preparation method may be, for example, an acidic silica sol or a polymer resin, preferably a light-curable resin. The aforementioned light-curable resin may be, for example, at least one selected from pentaerythritol triacrylate, pentaerythritol tetraacrylate, trimethylolpropane triacrylate, ethoxylated trimethylolpropane triacrylate, ditrimethylolpropane tetraacrylate, dipentaerythritol hexaacrylate, dipropylene glycol diacrylate, aliphatic polyurethane acrylate, and aliphatic polyurethane hexaacrylate.

[0079] The curing agent used in the aforementioned preparation method can be at least one selected from aluminum acetylacetonate, titanium acetylacetonate, photocuring agent 307 (World Chemical), TPOJRCure-1108UV, Omnirad127, and Omnirad184, for example.

[0080] [Photovoltaic glass]

[0081] The photovoltaic glass of the present invention contains the aforementioned anti-reflection material, so the photovoltaic glass of the present invention has a good anti-reflection effect and a wide anti-reflection wavelength.

[0082] [Optical glass]

[0083] The optical glass of the present invention contains the aforementioned anti-reflection material. Therefore, the photovoltaic glass of the present invention has a good anti-reflection effect and a wide anti-reflection wavelength.

[0084] [Polarizing plate]

[0085] The polarizing plate of the present invention contains the aforementioned anti-reflection material. Therefore, the photovoltaic glass of the present invention has a good anti-reflection effect and a wide anti-reflection wavelength.

[0086] Example

[0087] Example 1

[0088] 5 parts by mass of an aqueous dispersion of hollow silica nanoparticles with an average particle size of 15 nm produced by Ningbo Particle Technology Co., Ltd. (HKT-A20-15, the content of hollow particles is 20 wt%) and 6.7 parts by mass of an acidic silica sol (Grace, Ludox HAS, concentration is 30 wt%) are dispersed in 50 parts by mass of ethanol and stirred well. Then, 0.002 parts by mass of SURFYNOL 104E as a leveling agent and 0.1 parts by mass of aluminum acetylacetonate as a curing agent are added, and ethanol is supplemented so that the final composition is 100 parts by mass, stirred well, and then filtered using a 1000-mesh sieve to obtain a coating composition for forming a primer layer.

[0089] 10 parts by weight of an aqueous dispersion of hollow silicon dioxide nanoparticles with an average particle size of 80 nm produced by Ningbo Particle Technology Co., Ltd. (HKT-A20-80, 20 wt% of hollow particles) and 6.7 parts by weight of acidic silica sol (Grace, Ludox HAS, 30 wt% concentration) were dispersed in 50 parts by weight of ethanol and stirred well. Then, 0.002 parts by weight of SURFYNOL 104E as a leveling agent and 0.1 parts by weight of aluminum acetylacetonate as a curing agent were added, and ethanol was supplemented so that the final composition was 100 parts by weight, stirred well, and then filtered using a sieve of 800 meshes to obtain a coating composition for forming a top coating.

[0090] Commercially available ultra-white glass (Shenzhen Huiqi Glass Technology Co., Ltd., thickness 2mm, refractive index 1.52) was cut into a size of 80mm*150mm*2mm, and cleaned using an ultrasonic cleaner with a mixed solvent of ethanol: water (volume ratio of 1:1) at a power of 500W, time: 30 minutes, temperature: room temperature. Then it was hung in a 100℃ oven to dry for 20 minutes before use.

[0091] The prepared coating composition is poured into a material tank, and then the cleaned ultra-white glass is fixed on a vertical lift, lowered at a speed of 500 mm / min and immersed in the material tank, and then the glass is raised at a speed of 180 mm / min, thereby coating the glass with the coating composition for forming a primer layer. The glass is hung in an oven at 150°C for 2 minutes, taken out and naturally cooled to room temperature to obtain glass with a primer layer.

[0092] Then, the prepared coating composition for forming the top coating layer is poured into another material tank, the glass with the bottom coating layer formed is fixed on a vertical lifter, lowered at a speed of 500 mm / min and immersed in the material tank containing the coating composition for forming the top coating layer, and then the glass is raised at a speed of 130 mm / min, so as to apply the top coating layer on the bottom coating layer. Then, the glass is placed in a muffle furnace at 700°C and baked for 2 minutes, and then taken out and cooled naturally to obtain an anti-reflection material 1 with a bottom coating layer and a top coating layer formed.

[0093] The transmittance of the anti-reflection material 1 obtained above was tested using Shimadzu UV-2600i. The results showed that its maximum transmittance was 99.0%, corresponding to a wavelength of 560nm. The transmittance curve is shown in Figure 1 shown.

[0094] Example 2

[0095] 4 parts by mass of propylene glycol methyl ether dispersion of hollow silica nanoparticles with an average particle size of 10 nm produced by Ningbo Granular Technology Co., Ltd. (HKT-MM20-10-PM, hollow particle content 20wt%) and 0.5 parts by mass of pentaerythritol triacrylate and 1.5 parts by mass of dipentaerythritol hexaacrylate were dispersed in a mixed solvent of 50 parts by mass of propylene glycol methyl ether and ethyl acetate (the mass ratio of propylene glycol methyl ether to ethyl acetate was 2:1), and stirred well. Then, 0.0125 parts by mass of BYK-UV-3575 as a leveling agent and 0.3 parts by mass of 307 (Ward Chemical) as a photocuring agent were added, and ethanol was added to make the final composition 100 parts by mass, stirred well, and finally filtered using a 1000-mesh sieve to obtain a coating composition for forming a primer layer.

[0096] 10 parts by mass of propylene glycol methyl ether dispersion of hollow silica nanoparticles with an average particle size of 50 nm produced by Ningbo Granular Technology Co., Ltd. (HKT-MM20-50-PM, hollow particle content 20wt%) and 0.5 parts by mass of pentaerythritol triacrylate and 1.25 parts by mass of dipentaerythritol hexaacrylate were dispersed in a mixed solvent of 50 parts by mass of propylene glycol methyl ether and ethyl acetate (the mass ratio of propylene glycol methyl ether to ethyl acetate was 2:1), and stirred well. Then, 0.02 parts by mass of BYK-UV-3575 as a leveling agent and 0.125 parts by mass of photocuring agent Omnirad 127 were added, ethanol was added to make the final composition 100 parts by mass, stirred well, and finally filtered using a sieve of 800 mesh to obtain a coating composition for forming a top coating.

[0097] Cut the commercially available PET film (Huizhou Yingbo New Materials 100μm PET, refractive index 1.66) into a size of 200mm*300mm, use a dust-free cloth dipped in ethyl acetate solvent, carefully wipe the surface of the PET film, and dry at room temperature. Then fix the cleaned PET film on the wire rod coater, use a dropper to absorb about 1mL of the aforementioned prepared coating composition for forming a primer layer, and drip it on one end of one side of the aforementioned PET film. Use No. 3 wire rod, fix it on the coater, and evenly apply the aforementioned coating composition for forming a primer layer on the surface of the PET film at a speed of 20mm / s, dry it in a 60°C oven for 2 minutes, then take it out and cool it naturally to room temperature, then put it into a UV light curing machine, and cure it at a power of 1000W for 30s to obtain a PET film with a primer layer.

[0098] The PET film with the primer layer formed above is fixed on the wire rod coater, and about 1 mL of the coating composition for forming the top coat prepared above is sucked with a dropper, and dripped on one end of the side of the PET film coated with the primer layer. A No. 5 wire rod is selected and fixed on the coater, and the coating composition plating liquid for forming the top coat is evenly applied to the surface of the primer layer at a speed of 20 mm / s. Then it is placed in a 60°C oven for 2 minutes, taken out and naturally cooled to room temperature, and then placed in a UV light curing machine, and cured at a power of 1500W for 40s to obtain an anti-reflection material 2 with a primer layer and a top coat.

[0099] The back side of the anti-reflection material 2 obtained above (the uncoated side of the PET film) was attached with 3M tape (model 1712), and the reflectivity at an angle of 5 degrees was tested using Shimadzu UV-2600i. The reflectivity curve is as follows: Figure 3 As shown, the minimum reflectivity is 0.32%, corresponding to a wavelength of 600 nm, and the reflectivity in the wavelength range of 500-700 nm is lower than 0.5%, which has a wide range of anti-reflection effect.

[0100] Comparative Example 1 Transmittance Test of Blank Glass

[0101] The transmittance of blank glass was tested using Shimadzu UV-2600i, and the results are shown in Figure 2 , the highest transmittance is 91.3%.

[0102] Comparative Example 2 Reflectivity Test of Uncoated Polyethylene Terephthalate (PET) Film

[0103] Uncoated polyethylene terephthalate (PET) film was used, and 3M tape (model 1712) was attached to one side. The reflectivity at a 5-degree angle was tested using Shimadzu UV-2600i. The results are shown in Figure 3 , among which the lowest reflectivity is 5.8%.

[0104] Comparative Example 3 Anti-reflection material coated only with top coating on glass substrate

[0105] Compared with Example 1, the difference is that the glass substrate is not coated with a primer layer, but only a top coat layer is coated. The rest is carried out in the same manner as in Example 1 to obtain an anti-reflection material 3 having only a top coat layer formed thereon. The transmittance thereof is measured in the same manner as in Example 1, and the results are shown in Figure 2 , its maximum transmittance is 98.9%, corresponding to a wavelength of 550nm.

[0106] Comparative Example 4 Anti-reflection material with only top coating applied on polyethylene terephthalate (PET) film

[0107] Compared with Example 2, the difference is that the primer layer is not coated on the PET film, but only the top coat layer is coated. The rest is carried out in the same manner as in Example 2 to obtain an anti-reflection material 4 having only the top coat layer formed thereon. The reflectivity thereof is measured in the same manner as in Example 2, and the results are shown in Figure 3 , its minimum reflectivity is 0.39%, corresponding to a wavelength of 540nm.

[0108] Comparative Example 5 Anti-reflection material coated with a base coating (without hollow particles) and a top coating on a glass substrate

[0109] The difference from Example 1 is that the coating composition used to form the primer layer does not contain hollow particles. The specific preparation method is as follows: 2 parts by mass of acidic silica sol (Grace, Ludox HAS, concentration 30%) is dispersed in 50 parts by mass of ethanol, and stirred well, then, 0.002 parts by mass of SURFYNOL 104E as a leveling agent and 0.1 parts by mass of aluminum acetylacetonate as a curing agent are added, and ethanol is supplemented to make the final composition 100 parts by mass, and stirred well, and then filtered using a 1000-mesh sieve to obtain a coating composition for forming the primer layer.

[0110] The preparation and coating process of the top coating composition were the same as those in Example 1, and a material 5 having a primer layer (without hollow particles) and a top coating layer was obtained. The transmittance was measured in the same manner as in Example 1, and the results are shown in FIG. Figure 2 , its maximum transmittance is 98.8%, corresponding to a wavelength of 550nm.

[0111] From the comparison between the above-mentioned Example 1 and Comparative Examples 1, 3, and 5, it can be seen that compared with Comparative Examples 1, 3, and 5, the anti-reflection material 1 prepared in Example 1, which has a base coating and a top coating formed on a glass substrate, has the highest transmittance, and exhibits a good anti-reflection effect in a wide wavelength range (the transmittance of 400-700 nm is higher than 98%), while the anti-reflection film prepared in Comparative Example 3, which only contains a top coating, has a shorter wavelength range of anti-reflection, and the anti-reflection material prepared in Comparative Example 5, which does not contain hollow particles in the base coating, has a maximum transmittance of 98.8%, which is lower than 99.0% of Example 1, and the comprehensive gain effect is lower than that of Example 1. In this field, when the visible light transmittance exceeds 98.5%, every increase of 0.1% can be considered as a significant increase.

[0112] By comparing Example 2 with Comparative Examples 2 and 4, it can be seen that the PET film containing the primer layer and the top coating layer prepared in Example 2 has the lowest reflectivity and exhibits a good anti-reflection effect in a wider wavelength range (the transmittance of 500-700nm is less than 0.5%), while the anti-reflection material containing only the top coating layer prepared in Comparative Example 2, which is a blank PET film, and Comparative Example 4 has a significant anti-reflection effect only in a narrow area, and the comprehensive anti-reflection effect is lower than that of the PET film containing a double-layer anti-reflection film.

Claims

1. An anti-reflection material comprising a transparent substrate, a primer layer on the transparent substrate, and a top layer on the primer layer, wherein the refractive index of the top layer is less than the refractive index of the primer layer. The undercoat layer contains first hollow silica particles, and the porosity of the first hollow silica particles is 20-60%. The top coating layer contains second hollow silica particles, and the porosity of the second hollow silica particles is 40-70%. The average particle size D1 of the first hollow silica particles and the refractive index n0 of the transparent substrate satisfy the following relationship 1: The average particle size D1 of the first hollow silica particles and the average particle size D2 of the second hollow silica particles satisfy the following relationship 2, wherein the value of f is 4.5 to 5.5: D2=f×D1.

2. A method for preparing the anti-reflection material according to claim 1, characterized in that: The steps include: A first coating composition is applied on the transparent substrate and cured to form a base coating, and then a second coating composition is applied on the base coating and cured to form a top coating. Based on 100 parts by mass of the first coating composition, the coating composition comprises: Based on 100 parts by mass of the second coating composition, the composition comprises:

3. The method for preparing an anti-reflection material according to claim 2, wherein: The binder is acidic silica sol or polymer resin.

4. The method for preparing an anti-reflection material according to claim 3, wherein: The polymer resin is a photocurable resin.

5. The method for preparing an anti-reflection material according to claim 4, wherein: The photocurable resin is at least one selected from pentaerythritol triacrylate, pentaerythritol tetraacrylate, trimethylolpropane triacrylate, ethoxylated trimethylolpropane triacrylate, ditrimethylolpropane tetraacrylate, dipentaerythritol hexaacrylate, dipropylene glycol diacrylate, aliphatic polyurethane acrylate, and aliphatic polyurethane hexaacrylate.

6. The method for preparing an anti-reflection material according to claim 2, wherein: The curing agent is at least one selected from aluminum acetylacetonate, titanium acetylacetonate, light curing agent 307, TPOJRCure-1108UV, Omnirad 127, and Omnirad 184.

7. A photovoltaic glass comprising the anti-reflection material according to claim 1.

8. An optical glass comprising the anti-reflection material according to claim 1.

9. A polarizing plate comprising the anti-reflection material according to claim 1.

Citation Information

Cited By

  • Preparation method of efficient anti-reflection film for photovoltaic glass and film

    CN119349894A

  • Preparation method of high-efficiency anti-reflection film for photovoltaic glass and film

    CN119349894B

  • Refractive index regulation and control method for optical material based on silicon oxide hollow nanospheres

    CN119620437A

  • Organosilicon composite coating with low refractive index and preparation method thereof

    CN122790540A