A high damping grouting material for railway engineering
By adding silicon nitride nanofibers@ZIF-8 composite material and polyvinyl alcohol fibers to the grout, along with acrylate emulsion, the problems of unstable performance and high cost of grout in railway engineering were solved, and the performance of high-damping grout was significantly improved.
Patent Information
- Application Number
- CN202411251219.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-07
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-09-07
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of grouting materials, and more specifically, relates to a high-damping grouting material for railway engineering. Background Art
[0002] Cement-based grouting material is a material formed by adding appropriate amounts of mineral admixtures and admixtures to cement as a gelling material. It has the characteristics of high fluidity and high strength. It is widely used in the fields of secondary grouting of equipment foundations, installation of large equipment, reinforcement of concrete structures, and road repair. However, cement-based grouting materials still generally have problems such as unstable performance, high cost, and difficulty in controlling shrinkage.
[0003] Polyvinyl alcohol (PVA) fiber has the advantages of high strength, high elastic modulus, low elongation, wear resistance, good affinity and adhesion with cement and other base materials. It is widely used in cement-based reinforced and toughened materials, increasing the toughness of the grouting matrix, improving the energy dissipation capacity of connectors and connection nodes, and ultimately improving the seismic performance of the entire building.
[0004] CN118005341A discloses a high-strength grouting material for installation of a large-power wind turbine foundation and a preparation method thereof. The grouting material is prepared by mixing water and powder in a mass ratio of 0.083 to 0.098; the powder is composed of the following mass parts: 30 to 38 parts of silicate cement, 40 to 55 parts of sand, 10 to 20 parts of composite mineral admixtures, 0.008 to 0.013 parts of expansion agent, 0.25 to 0.55 parts of water reducer, 0.35 to 0.65 parts of early strength agent, 0.12 to 0.28 parts of defoamer, and 0.06 to 0.2 parts of activator combination. The high-strength grouting material prepared by the method is convenient for construction and can meet the installation requirements of the foundation of a large-power wind turbine. Compared with other grouting materials, the grouting material has ultra-high strength and reduces the amount of cement used in the preparation process through the synergistic effect of chemical excitation and skeleton design, so that the grouting material has the characteristics of green environmental protection and low cost.
[0005] CN117985988A discloses a high-performance cement-based early-strength grouting material and a preparation method thereof, comprising: quartz sand, microsilica fume, and also comprising: P·C 42.5 composite silicate cement, 42.5 rapid-hardening sulphoaluminate cement and PCA-I type mother liquid polycarboxylic acid high-efficiency water reducing agent. The preparation method comprises the following steps: step 1: firstly taking quartz sand and putting it into a high-speed grinding mill for grinding, grinding the quartz sand to 26-40 mesh, 40-70 mesh and 70-110 mesh respectively, taking P·C 42.5 composite silicate cement, then taking 42.5 rapid-hardening sulphoaluminate cement, and taking microsilica fume for grinding to 1500 mesh; step 2: adding the weight ratio of each group into a mortar stirring pot at a time and stirring, and after stirring, putting the grouting material into a 40×40×160mm triple test mold, and curing it naturally at ambient temperature for 3 days, 7 days and 28 days respectively. The high-performance cement-based early-strength grouting material and the preparation method thereof can quickly improve the strength of the prepared cement-based early-strength grouting material, and the cement-based early-strength grouting material has good fluidity.
[0006] CN117865584A discloses a ternary early strength grouting material, comprising the following raw materials in parts by weight: 100 parts of ternary gelling material, 1.54-2.3 parts of early strength agent, 0.3-1 parts of retarder, 0.8-2 parts of water reducer, 30-40 parts of water, and 5-15 parts of polymer emulsion. The ternary early strength grouting material described herein uses polymer emulsion to modify the ternary early strength gelling system, and the high molecular polymer in the polymer emulsion and the products of the ternary early strength hydrolysis - calcium sulfoxide (AFt) and aluminum gel (AH3) are cross-linked to form a network structure, which can effectively improve the density and flexibility of the grouting material. In addition, the organic properties of the polymer itself can enhance the interfacial bonding strength between the grouting material and the base asphalt mixture, which is beneficial to improve the crack resistance of the grouting asphalt mixture.
[0007] CN117776646A discloses an early-strength cement grouting material with controllable initial setting time, comprising component A and component B; wherein the mass percentages of component A and component B are as follows: the mass percentages of component A are 60-78% of ordinary Portland cement, 1-4% of water reducing agent, 8-12% of mineral powder, 8-12% of gypsum, 4-6% of slaked lime, 0.05-0.1% of modified epoxy resin, 0.06-0.12% of defoaming agent and 0.2-0.4% of sodium gluconate; the mass percentages of component B are 6-18% of Portland cement, 52-68% of aluminate cement, 1-4% of water reducing agent, 2-6% of silica fume, 6-12% of calcium aluminate, 0.05-0.1% of modified epoxy resin, 0.06-0.12% of defoaming agent and 0.2-0.4% of sodium gluconate. The cement grouting material has the characteristics of good fluidity, controllable initial setting time, good toughness, smooth surface and high early strength. It has good applications in construction, water conservancy, transportation, mining and other fields.
[0008] Based on the above content, it can be seen that the mechanical properties of the grouting material can be improved by adding modified components or fiber materials, but the modification effect is not obvious or cannot meet the use requirements of railway engineering. Summary of the invention
[0009] The technical problem to be solved by the present invention is to overcome the defects and shortcomings in the prior art and provide a high-damping grouting material for railway engineering. In parts by weight, the grouting material includes the following raw materials: 60-100 parts of PII52.5 cement; 15-25 parts of silica fume; 90-130 parts of quartz sand; 2-6 parts of silicon nitride nanofiber @ ZIF-8 composite material; 0.5-1.5 parts of polyvinyl alcohol fiber; 4-12 parts of acrylic emulsion; 1-3 parts of water reducer; 3-5 parts of expansion agent; 2-4 parts of defoamer; 80-160 parts of water. The present invention can improve the mechanical properties and anti-permeability of the grouting material by adding silicon nitride nanofiber @ ZIF-8 composite material and coordinating polyvinyl alcohol fiber and acrylic emulsion.
[0010] The purpose of the invention is to provide a high-damping grouting material for railway engineering.
[0011] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0012] A high-damping grouting material for railway engineering, comprising the following raw materials in parts by weight:
[0013] PII52.5 cement 60~100 parts
[0014] Silica fume 15-25 parts;
[0015] 90~130 parts of quartz sand;
[0016] Silicon nitride nanofiber@ZIF-8 composite material 2-6 parts;
[0017] 0.5~1.5 parts of polyvinyl alcohol fiber;
[0018] 4-12 parts of acrylic emulsion;
[0019] 1~3 parts of water reducing agent;
[0020] 3~5 parts of expansion agent;
[0021] 2~4 parts of defoaming agent;
[0022] 80~160 parts of water.
[0023] Preferably, the particle size of the silica fume is 100-300 μm; the particle size of the quartz sand is 300-700 μm.
[0024] Preferably, the silicon nitride nanofibers are 2-6 mm in diameter and have an aspect ratio of 100-300:1.
[0025] Preferably, the length of the polyvinyl alcohol fiber is 1-3 mm, and the aspect ratio is 50-100:1; the solid content of the acrylic emulsion is 55 wt%.
[0026] Preferably, the water reducing agent is a polycarboxylic acid-based water reducing agent; the swelling agent is a calcium sulfoaluminate swelling agent; and the defoaming agent is a mineral oil-based defoaming agent.
[0027] In the present invention, a preferred technical solution is that the method for preparing the silicon nitride nanofiber@ZIF-8 composite material comprises the following steps:
[0028] (1) Silicon nitride nanofibers are ultrasonically dispersed in a nitric acid solution, treated in a water bath, cooled to room temperature, filtered, washed, and dried at a certain temperature to a constant weight to obtain acid-modified silicon nitride nanofibers;
[0029] (2) Add the acid-modified silicon nitride nanofibers and zinc salt obtained in step (1) to DMF, ultrasonically disperse for a certain period of time, then add 2-dimethylimidazole, continue ultrasonication for a certain period of time, solvent thermal reaction, filter, wash, and dry to obtain a silicon nitride nanofiber@ZIF-8 composite material.
[0030] Preferably, in step (1), the concentration of the nitric acid solution is 1 to 3 mol / L; and the drying temperature is 60 to 80°C.
[0031] Preferably, in step (1), the water bath treatment is carried out at 60 to 80° C. for 6 to 10 hours.
[0032] Preferably, in step (2), the ultrasonic dispersion time is 20 to 40 minutes; and the continued ultrasonication time is 20 to 40 minutes.
[0033] Preferably, in step (2), the solvent thermal reaction is a solvent thermal reaction at 130-170° C. for 10-16 h; the drying is drying at 80-120° C. for 10-14 h; acid-modified silicon nitride nanofibers, zinc salt, 2-dimethylimidazole: 20 g: 1 mol: 1-2 mol; the zinc salt is at least one of zinc nitrate, zinc chloride or zinc acetate.
[0034] The present invention has the following beneficial effects:
[0035] The present invention can fully fill the cement-based grouting material by adding silicon nitride nanofiber @ZIF-8 composite material, reduce the number and size of voids, and form a denser structure. In addition, the silicon nitride nanofiber itself has high mechanical strength and stability, which can improve the strength of the cement grouting material. The polyvinyl alcohol (PVA) fiber has the advantages of good affinity and adhesion with cement and other base materials, which can significantly increase the toughness of the grouting material matrix and improve the energy consumption capacity of the connector and the connection node. The acrylic emulsion can promote complexation with cement and improve the comprehensive performance of the grouting material. Through the mutual coordination of the above components, the comprehensive performance of the grouting material is significantly improved, and the grouting material has a good application prospect. DETAILED DESCRIPTION
[0036] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0037] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0038] Example 1
[0039] A high-damping grouting material for railway engineering, comprising the following raw materials in parts by weight:
[0040] PII52.5 cement 80 parts;
[0041] 20 parts of silica fume; the particle size of the silica fume is 200 μm;
[0042] 110 parts of quartz sand; the particle size of the quartz sand is 500 μm;
[0043] 4 parts of silicon nitride nanofiber@ZIF-8 composite material; the silicon nitride nanofiber is 4 mm and has an aspect ratio of 200:1;
[0044] 1 part of polyvinyl alcohol fiber; the polyvinyl alcohol fiber has a length of 2 mm and an aspect ratio of 80:1;
[0045] 8 parts of acrylic emulsion; the solid content of the acrylic emulsion is 55wt%;
[0046] 2 parts of water reducing agent; the water reducing agent is H-4005 polycarboxylic acid water reducing agent;
[0047] 4 parts of expansion agent; the expansion agent is a calcium sulphoaluminate expansion agent;
[0048] 3 parts of defoamer; the defoamer is mineral oil defoamer F-111.
[0049] 120 parts of water.
[0050] The preparation method of the silicon nitride nanofiber@ZIF-8 composite material comprises the following steps:
[0051] (1) 100 g of silicon nitride nanofibers were ultrasonically dispersed in 150 mL of 2 mol / L nitric acid solution and treated in a water bath at 70 °C for 8 h; cooled to room temperature, filtered, washed, and dried at 70 °C to constant weight to obtain acid-modified silicon nitride nanofibers;
[0052] (2) Add 20 g of the acid-modified silicon nitride nanofibers obtained in step (1) and 1 mol of zinc nitrate to 250 mL of DMF, and ultrasonically disperse for 30 min. Then add 1.5 mol of 2-dimethylimidazole and continue ultrasonicating for 30 min. Then, solvent thermally react at 150 °C for 14 h, filter, wash, and dry at 100 °C for 12 h to obtain a silicon nitride nanofiber@ZIF-8 composite material.
[0053] Example 2
[0054] The difference between Example 2 and Example 1 is that: a high-damping grouting material for railway engineering, including the following raw materials in parts by weight:
[0055] PII52.5 cement 100 parts;
[0056] Silica fume 15 parts;
[0057] 130 parts of quartz sand;
[0058] 2 parts of silicon nitride nanofiber@ZIF-8 composite material;
[0059] 1.5 parts of polyvinyl alcohol fiber;
[0060] 4 parts of acrylic emulsion;
[0061] 3 parts of water reducing agent;
[0062] 3 parts of expansion agent;
[0063] 4 parts of defoamer;
[0064] 160 parts of water.
[0065] Example 3
[0066] The difference between Example 3 and Example 1 is that: a high-damping grouting material for railway engineering includes the following raw materials in parts by weight:
[0067] PII52.5 cement 60 parts;
[0068] Silica fume 25 parts;
[0069] 90 parts of quartz sand;
[0070] Silicon nitride nanofiber@ZIF-8 composite material 6 parts;
[0071] 0.5 parts of polyvinyl alcohol fiber;
[0072] Acrylate emulsion 12 parts;
[0073] 1 part of water reducing agent;
[0074] 5 parts of expansion agent;
[0075] 2 parts of defoaming agent;
[0076] 80 parts of water.
[0077] Comparative Example 1
[0078] The difference between Control Example 1 and Example 1 is that an equal amount of acid-modified silicon nitride nanofibers is used to replace the silicon nitride nanofiber@ZIF-8 composite material.
[0079] The method for preparing the acid-modified silicon nitride nanofibers comprises the following steps:
[0080] (1) 100 g of silicon nitride nanofibers were ultrasonically dispersed in 150 mL of 2 mol / L nitric acid solution and treated in a water bath at 70 °C for 8 h; cooled to room temperature, filtered, washed, and dried at 70 °C to constant weight to obtain acid-modified silicon nitride nanofibers.
[0081] Comparative Example 2
[0082] The difference between Control Example 2 and Example 1 is that an equal amount of silicon nitride nanofibers is used to replace the silicon nitride nanofiber@ZIF-8 composite material.
[0083] Comparative Example 3
[0084] The difference between Control Example 3 and Example 1 is that 5 parts of silicon nitride nanofiber @ ZIF-8 composite material are used to replace 4 parts of silicon nitride nanofiber @ ZIF-8 composite material and 1 part of polyvinyl alcohol fiber.
[0085] Comparative Example 4
[0086] The difference between Control Example 4 and Example 1 is that 9 parts of acrylic emulsion are used to replace 1 part of polyvinyl alcohol fiber and 8 parts of acrylic emulsion.
[0087] Comparative Example 5
[0088] The difference between Control Example 5 and Example 1 is that CNTs (Flotube 9000, Jiangsu Tiannai Technology Co., Ltd.) are used to replace silicon nitride nanofibers.
[0089] The performance data of test examples 1-3 and control examples 1-5 are shown in Table 1 for specific test results.
[0090] Among them, the preparation method of high damping grouting material for railway engineering is as follows:
[0091] Silicon nitride nanofiber @ ZIF-8 composite material and polyvinyl alcohol fiber were dispersed in water and stirred at 260 rpm for 20 min, then PII52.5 cement, silica fume, quartz sand, acrylic emulsion, water reducer, expansion agent and defoamer were added, and stirring was continued for 10 min to obtain high damping grouting material for railway engineering.
[0092] The test standards are as follows:
[0093] Compressive strength: GB / T 17671-2021;
[0094] Vertical expansion rate: GB50448-2015.
[0095] The damping ratio is used to characterize the damping performance of concrete (the grouting material is cured to 28 days and the performance after curing is tested)
[0096] Table 1
[0097]
[0098] As can be seen from Table 1, by comparing Examples 1-3 with Control Examples 1-5, it can be seen that the present invention can significantly improve the compressive properties of the grouting material by adding the modified component, thereby showing a more excellent performance.
[0099] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A high damping grouting material for railway engineering, characterized in that: By weight, it includes the following raw materials: PII52.5 cement 60~100 parts Silica fume 15-25 parts; 90~130 parts of quartz sand; Silicon nitride nanofiber@ZIF-8 composite material 2-6 parts; 0.5~1.5 parts of polyvinyl alcohol fiber; 4-12 parts of acrylic emulsion; 1~3 parts of water reducing agent; 3~5 parts of expansion agent; 2~4 parts of defoaming agent; 80~160 parts of water; The preparation method of the silicon nitride nanofiber@ZIF-8 composite material comprises the following steps: (1) Silicon nitride nanofibers are ultrasonically dispersed in a nitric acid solution, treated in a water bath, cooled to room temperature, filtered, washed, and dried at a certain temperature to a constant weight to obtain acid-modified silicon nitride nanofibers; (2) Add the acid-modified silicon nitride nanofibers and zinc salt obtained in step (1) to DMF, ultrasonically disperse for a certain period of time, then add 2-dimethylimidazole, continue ultrasonication for a certain period of time, solvent thermal reaction, filter, wash, and dry to obtain a silicon nitride nanofiber@ZIF-8 composite material; acid-modified silicon nitride nanofibers, zinc salt, 2-dimethylimidazole: 20 g: 1 mol: 1~2 mol.
2. The high-damping grouting material for railway engineering according to claim 1, characterized in that: The particle size of the silica fume is 100-300 μm; the particle size of the quartz sand is 300-700 μm.
3. The high damping grouting material for railway engineering according to claim 1, characterized in that: The silicon nitride nanofibers are 2-6 mm in diameter and have an aspect ratio of 100-300:
1.
4. The high damping grouting material for railway engineering according to claim 1, characterized in that: The length of the polyvinyl alcohol fiber is 1-3 mm, and the aspect ratio is 50-100:1; the solid content of the acrylic ester emulsion is 55 wt%.
5. The high damping grouting material for railway engineering according to claim 1, characterized in that: The water reducing agent is a polycarboxylic acid-based water reducing agent; the expansion agent is a calcium sulfoaluminate expansion agent; and the defoaming agent is a mineral oil-based defoaming agent.
6. The high-damping grouting material for railway engineering according to claim 1, characterized in that: In step (1), the concentration of the nitric acid solution is 1 to 3 mol / L; and the drying temperature is 60 to 80°C.
7. The high damping grouting material for railway engineering according to claim 1, characterized in that: In step (1), the water bath treatment is carried out at 60 to 80° C. for 6 to 10 hours.
8. The high damping grouting material for railway engineering according to claim 1, characterized in that: In step (2), the ultrasonic dispersion time is 20 to 40 minutes; the continued ultrasonic time is 20 to 40 minutes.
9. The high damping grouting material for railway engineering according to claim 1, characterized in that: In step (2), the solvent thermal reaction is a solvent thermal reaction at 130-170° C. for 10-16 hours; the drying is drying at 80-120° C. for 10-14 hours; and the zinc salt is at least one of zinc nitrate, zinc chloride or zinc acetate.
Citation Information
Patent Citations
Early strength cement grouting material with controllable initial setting time and preparation method thereof
CN117776646A
Ternary early strength grouting material, preparation method and application thereof
CN117865584A
High-performance cement-based early-strength grouting material and preparation method thereof
CN117985988A
High-strength grouting material for mounting foundation base of high-power wind turbine generator and preparation method of high-strength grouting material
CN118005341A
High-strength cement-based damping grouting material
CN102234189A