Low-heat-loss composite brick for active lime rotary kiln
Through the use of alumina clinker and aluminum dihydrogen phosphate solution, the problem of large heat loss in the construction of active lime rotary kiln has been solved, the thermal insulation effect and service life of composite bricks have been improved, and the temperature of the kiln skin has been significantly reduced. .
Patent Information
- Application Number
- CN202410915404.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-11
AI Technical Summary
The refractory bricks built in the existing active lime rotary kiln have no insulation. The rotary kiln skin has high temperature and large heat loss. The insulation material of the composite brick has low strength, low load softening temperature and short service life.
Alumina clinker rotary kiln ring material is used to make the insulation part of the composite brick. Through crushing, fine grinding and the combination of aluminum dihydrogen phosphate solution, the material strength and load softening temperature are improved, and low-temperature composite bricks are prepared through high-pressure molding and baking processes. Heat Loss Composite Brick.
It significantly reduces the temperature of the rotary kiln skin, improves the thermal insulation effect, and extends the service life of the composite bricks. The material has high strength, high load softening temperature, and obvious thermal insulation effect.
Smart Images

Figure CN118754628A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite bricks, in particular to an active lime rotary kiln low heat loss composite brick. Background Art
[0002] At present, the refractory bricks used in the active lime rotary kiln have no insulation, the temperature of the rotary kiln skin is high, the heat loss is large, the insulation part of the composite bricks used in the kiln has low material strength, low load softening temperature, short service life, high temperature of the rotary kiln skin, and large heat loss.
[0003] In order to overcome the shortcomings of the existing composite bricks, such as short service life, high rotary kiln skin temperature and large heat loss, the present invention utilizes alumina clinker rotary kiln ring material to make the insulation part of the composite brick. The material has high strength and high load softening temperature. The composite brick significantly reduces the rotary kiln skin temperature and has obvious thermal insulation effect. Summary of the invention
[0004] The purpose of the present invention is to solve at least one of the technical problems existing in the prior art and to provide a low heat loss composite brick for an active lime rotary kiln. The present invention utilizes alumina clinker rotary kiln ring material to make the insulation part of the composite brick. The material has high strength and a high load softening temperature. The composite brick significantly reduces the temperature of the rotary kiln skin and has obvious thermal insulation effect.
[0005] The present invention also provides the above-mentioned active lime rotary kiln low heat loss composite brick, comprising: the active lime rotary kiln low heat loss composite brick is composited by heat insulation material and heavy material;
[0006] The active lime rotary kiln low heat loss composite brick comprises the following preparation steps:
[0007] S1, thermal insulation material preparation, including the following steps:
[0008] 1) Crushing and classifying the alumina clinker rotary kiln ring material into multiple grades of aggregate;
[0009] 2) crush and grind the alumina clinker rotary kiln ring material into fine powder;
[0010] 3) crush the combined clay and grind it into fine powder;
[0011] 4) Mix aluminum dihydrogen phosphate and water in proportion to form an aluminum dihydrogen phosphate solution;
[0012] 5) Determine the following ratios by measuring the strength, load softening temperature, and thermal insulation effect of the insulation material:
[0013] Alumina clinker ring material
[0014] aggregate
[0015]
[0016] Aluminum dihydrogen phosphate solution is added at 7%;
[0017] 6) Add the aggregate into the mixer according to the ratio in 5), mix and grind for 2 minutes, add 4% aluminum dihydrogen phosphate solution, mix and grind for 3 minutes, and add fine powder.
[0018] Mix and grind for 10 minutes, release, and trap the material for 24 hours;
[0019] S2. Preparation of heavy materials, comprising the following steps:
[0020] 1) Crush and grade 85 bauxite clinker into multiple grades of aggregates and remove iron;
[0021] 2) Crush the 85 bauxite clinker into fine powder and remove iron;
[0022] 3) Crush the combined clay into fine powder and remove iron;
[0023] 4) Mix aluminum dihydrogen phosphate and water in proportion to form an aluminum dihydrogen phosphate solution;
[0024] 5) Mix according to the following ratio:
[0025] 85 alumina clinker
[0026] aggregate
[0027]
[0028]
[0029] Aluminum dihydrogen phosphate solution is added at 6%;
[0030] 6) Put the aggregate into the mixer according to the proportion in 5), mix and grind for 2 minutes, add 4% aluminum dihydrogen phosphate solution, mix and grind for 3 minutes, add fine powder, mix and grind for 10 minutes, release, and trap the material for 24 hours;
[0031] S3, the thermal insulation part material and the heavy part material are compounded, including the following steps:
[0032] 1) Add the heat preservation material after being trapped for 24 hours into the mixer and grind for 3 minutes, add 3% aluminum dihydrogen phosphate solution and grind for 10 minutes, and set aside for use;
[0033] 2) Add the heavy material trapped for 24 hours into the mixer, mix and grind for 3 minutes, add 2% aluminum dihydrogen phosphate solution, mix and grind for 10 minutes, and set aside for use;
[0034] 3) Insert a baffle plate 100mm away from the large end face baffle plate in the press die, put the measured insulation material between the baffle plate and the large end face baffle plate, put the measured heavy material between the baffle plate and the small end face baffle plate, take out the baffle plate, and perform high pressure molding to make a composite brick semi-finished product;
[0035] S4, baking the semi-finished composite bricks, putting the semi-finished composite bricks into an oven, baking at 100℃-300℃ for 48 hours, and cooling to obtain the finished products;
[0036] S5. Monitoring of thermal insulation of composite bricks. Place the composite brick sideways into the furnace mouth of the electric furnace, with the heavy part facing inward and the insulating part facing outward. Wrap the heavy part with alumina fiber to the upper top, lower bottom and side walls of the furnace mouth of the electric furnace. Wrap the insulating part with aluminum silicate fiber cotton to the upper top, lower bottom, side walls and exposed part of the furnace mouth of the electric furnace. Place a 24mm steel plate that is smaller than the large end face of the composite brick close to the exposed large end face of the insulating part. Support the steel plate with a bracket underneath. The steel plate represents the wall of the rotary kiln. The temperature of the steel plate surface represents the temperature of the rotary kiln skin. Heat up and keep warm for five hours, and monitor with an infrared thermometer.
[0037] According to the active lime rotary kiln low heat loss composite brick provided by the present invention, the aluminum oxide content in the alumina clinker rotary kiln ring material in S1 is 72.12%.
[0038] According to the active lime rotary kiln low heat loss composite brick provided by the present invention, the crushing and fine grinding of the alumina clinker rotary kiln ring material and the crushing and fine grinding of the combined clay in S1 are specifically crushed and finely ground into 100 mesh fine powder.
[0039] According to the active lime rotary kiln low heat loss composite brick provided by the present invention, the content of aluminum oxide combined with clay in S1 is 25%.
[0040] According to the active lime rotary kiln low heat loss composite brick provided by the present invention, the multi-grade aggregate in S1 is specifically a bauxite clinker rotary kiln ring material that is crushed and graded into 0-5mm, 5-8mm, and 8-15mm aggregates.
[0041] According to the active lime rotary kiln low heat loss composite brick provided by the present invention, the content of aluminum oxide in the 85 alumina clinker in S2 is 85%, and the content of aluminum oxide in the combined clay in S2 is 25%.
[0042] According to the active lime rotary kiln low heat loss composite brick provided by the present invention, the multi-grade aggregate in S2 is specifically 0-1mm, 1-3mm, 3-5mm, and 5-8mm aggregate.
[0043] According to the active lime rotary kiln low heat loss composite brick provided by the present invention, the crushing in S2 is specifically crushing and grinding into 180 mesh fine powder.
[0044] According to the active lime rotary kiln low heat loss composite brick provided by the present invention, the mixing in proportion in S1 and S2 is specifically mixing aluminum dihydrogen phosphate and water in a ratio of 2:1.
[0045] Compared with the prior art, the active lime rotary kiln low heat loss composite brick of the present invention utilizes alumina clinker rotary kiln ring material to make the insulation part of the composite brick. The material has high strength and high load softening temperature. The composite brick significantly reduces the temperature of the rotary kiln skin and has obvious thermal insulation effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] The present invention is further described below in conjunction with the accompanying drawings and embodiments;
[0047] Figure 1 The present invention is a flow chart for preparing low heat loss composite bricks for active lime rotary kiln. DETAILED DESCRIPTION
[0048] This section will describe in detail the specific embodiments of the present invention. The preferred embodiments of the present invention are shown in the accompanying drawings. The purpose of the accompanying drawings is to supplement the description of the text part of the specification with graphics, so that people can intuitively and vividly understand each technical feature and the overall technical solution of the present invention, but it cannot be understood as a limitation on the scope of protection of the present invention.
[0049] Reference Figure 1 , an embodiment of the present invention provides an active lime rotary kiln low heat loss composite brick, which includes: an active lime rotary kiln low heat loss composite brick is composited by a heat preservation material and a heavy material;
[0050] Active lime rotary kiln low heat loss composite bricks include the following preparation steps:
[0051] S1, thermal insulation material preparation, including the following steps:
[0052] 1) Crushing and classifying the alumina clinker rotary kiln ring material with 72.12% aluminum oxide content into 0-5mm, 5-8mm, and 8-15mm aggregates;
[0053] 2) crush and grind the alumina clinker rotary kiln ring material with an aluminum oxide content of 72.12% into 100 mesh fine powder;
[0054] 3) crush and grind the combined clay with 25% aluminum oxide content into 100 mesh fine powder;
[0055] 4) Mix aluminum dihydrogen phosphate and water in a ratio of 2:1 to form an aluminum dihydrogen phosphate solution;
[0056] 5) Since the alumina clinker rotary kiln ring material has many pores, it is necessary to consider the strength and load softening temperature of the insulation material, and more importantly, the insulation effect. Therefore, the proportion should use as much aggregate as possible. According to this principle, the test was carried out and the following raw material proportion was finally determined:
[0057] Alumina clinker ring material
[0058] aggregate
[0059]
[0060] Aluminum dihydrogen phosphate solution is added at 7%;
[0061] 6) Add the aggregates to the mixer according to the ratio in 5). Add the aggregates to the mixer according to the above ratio. Mix and grind for 2 minutes and add 4% aluminum dihydrogen phosphate solution. Mix and grind for 3 minutes and add fine powder. Mix and grind for 10 minutes and release. Trapped material for 24 hours;
[0062] S2. Preparation of heavy materials, comprising the following steps:
[0063] 1) Crush and grade 85 alumina clinker into 0-1mm, 1-3mm, 3-5mm, 5-8mm aggregates, and remove iron;
[0064] 2) Crush the 85 bauxite clinker into 180 mesh fine powder and remove iron;
[0065] 3) Crush the combined clay into 180 mesh fine powder and remove iron;
[0066] 4) Mix aluminum dihydrogen phosphate and water in a ratio of 2:1 to form an aluminum dihydrogen phosphate solution;
[0067] 5) Mix according to the following ratio:
[0068] 85 alumina clinker
[0069] aggregate
[0070]
[0071] Aluminum dihydrogen phosphate solution is added at 6%;
[0072] 6) Put the aggregate into the mixer according to the proportion in 5), mix and grind for 2 minutes, add 4% aluminum dihydrogen phosphate solution, mix and grind for 3 minutes, add fine powder, mix and grind for 10 minutes, release, and trap the material for 24 hours;
[0073] S3, the thermal insulation part material and the heavy part material are compounded, including the following steps:
[0074] 1) Add the heat preservation material after being trapped for 24 hours into the mixer and grind for 3 minutes, add 3% aluminum dihydrogen phosphate solution and grind for 10 minutes, and set aside for use;
[0075] 2) Add the heavy material trapped for 24 hours into the mixer, mix and grind for 3 minutes, add 2% aluminum dihydrogen phosphate solution, mix and grind for 10 minutes, and set aside for use;
[0076] 3) Insert a baffle plate 100mm away from the large end face baffle plate in the press die, put the measured insulation material between the baffle plate and the large end face baffle plate, put the measured heavy material between the baffle plate and the small end face baffle plate, take out the baffle plate, and high pressure molding to make a composite brick semi-finished product with a size of 250×200×93 / 80mm;
[0077] S4, baking the semi-finished composite bricks, putting the semi-finished composite bricks into an oven, baking at 100℃-300℃ for 48 hours, and cooling to obtain the finished products;
[0078] S5. Monitoring of thermal insulation of composite bricks. Put the composite brick sideways into the furnace mouth of the electric furnace, with the heavy part facing inward and the insulating part facing outward. The heavy part is wrapped with alumina fiber to the upper top, lower bottom and side walls of the furnace mouth of the electric furnace, and the insulating part is wrapped with aluminum silicate fiber cotton to the upper top, lower bottom, side walls and exposed part of the furnace mouth of the electric furnace. Put a 24mm thick steel plate that is smaller than the large end face of the composite brick close to the exposed large end face of the insulating part, and support it with a bracket underneath. The steel plate represents the wall of the rotary kiln, and the temperature of the steel plate surface represents the temperature of the rotary kiln skin. Heat up and keep warm for five hours, and monitor with an infrared thermometer.
[0079] Aluminum dihydrogen phosphate indicators:
[0080]
[0081] Physical and chemical indicators of composite brick insulation materials
[0082]
[0083]
[0084] Detection result of step S5
[0085] Furnace temperature (℃) Insulation time (h) Steel plate surface temperature (℃) 800 5 107 900 5 116-120 1000 5 120-125 1100 5 125-130 1200 5 130-135 1300 5 145-155 1400 5 165-175
[0086] Analyze and judge based on the monitoring results and the physical and chemical indicators of the insulation materials
[0087] 1. The compressive strength of the insulation material at room temperature is 25Mpa, which is 2-3 times the flexural strength. The flexural strength of the insulation material is sufficient.
[0088] 2. The load softening temperature of the insulation part material is 1374℃, which is the temperature at which it deforms 0.6% under a constant pressure of 0.2MPa. However, in the production process, the pressure of the lime does not reach 0.2MPa. The insulation part material will not soften when subjected to a flame temperature of 1400℃. The insulation part and the heavy part are well combined and will not break.
[0089] 3. The volume density of the insulation material is 2.65g / cm 3 The alumina content reaches 68.35%, and the insulation part material has good wear resistance and corrosion resistance. After the heavy part is worn out, the insulation part material can continue to be used.
[0090] 4. Use refractory bricks made of heavy parts to build active lime rotary kiln. During the production process, the highest temperature of the kiln skin is 380-400℃. The apparent porosity of the insulation part material is 13.34%, which is low, while the highest kiln skin temperature of the composite brick monitoring result is 175℃. Proof: The reason for the thermal insulation of the composite brick is the role of the alumina clinker rotary kiln ring material.
[0091] The embodiments of the present invention are described in detail above with reference to the accompanying drawings. However, the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in the technical field without departing from the purpose of the present invention.
Claims
1. A low heat loss composite brick for active lime rotary kiln, It is characterized in that include: The active lime rotary kiln low heat loss composite brick is composited with heat-insulating material and heavy material; The thermal insulation material comprises: alumina clinker rotary kiln ring material and bonding clay; The heavy materials include: 85 alumina clinker and combined clay; The active lime rotary kiln low heat loss composite brick comprises the following preparation steps: S1, thermal insulation material preparation, including the following steps: 1) Crushing and classifying the alumina clinker rotary kiln ring material into multiple grades of aggregate; 2) crush and grind the alumina clinker rotary kiln ring material into fine powder; 3) crush the combined clay and grind it into fine powder; 4) Mix aluminum dihydrogen phosphate and water in proportion to form an aluminum dihydrogen phosphate solution; 5) Determine the following ratios by measuring the strength, load softening temperature, and thermal insulation effect of the insulation material: Alumina clinker ring material aggregate Aluminum dihydrogen phosphate solution is added at 7%; 6) Add the aggregates into the mixer according to the proportion in 5), mix and grind for 2 minutes, add 4% aluminum dihydrogen phosphate solution, mix and grind for 3 minutes, add fine powder, mix and grind for 10 minutes, release, and trap the material for 24 hours; S2. Preparation of heavy materials, comprising the following steps: 1) Crush and grade 85 bauxite clinker into multiple grades of aggregates and remove iron; 2) Crush the 85 bauxite clinker into fine powder and remove iron; 3) Crush the combined clay into fine powder and remove iron; 4) Mix aluminum dihydrogen phosphate and water in proportion to form an aluminum dihydrogen phosphate solution; 5) Mix according to the following ratio: 85 alumina clinker aggregate Aluminum dihydrogen phosphate solution is added at 6%; 6) Put the aggregate into the mixer according to the proportion in 5), mix and grind for 2 minutes, add 4% aluminum dihydrogen phosphate solution, mix and grind for 3 minutes, add fine powder, mix and grind for 10 minutes, release, and trap the material for 24 hours; S3, the thermal insulation part material and the heavy part material are compounded, including the following steps: 1) Add the heat preservation material after being trapped for 24 hours into the mixer and grind for 3 minutes, add 3% aluminum dihydrogen phosphate solution and grind for 10 minutes, and set aside for use; 2) Add the heavy material trapped for 24 hours into the mixer, mix and grind for 3 minutes, add 2% aluminum dihydrogen phosphate solution, mix and grind for 10 minutes, and set aside for use; 3) Insert a baffle plate 100mm away from the large end face baffle plate in the press die, put the measured insulation material between the baffle plate and the large end face baffle plate, put the measured heavy material between the baffle plate and the small end face baffle plate, take out the baffle plate, and perform high pressure molding to make a composite brick semi-finished product; S4, baking the semi-finished composite bricks, putting the semi-finished composite bricks into an oven, baking at 100℃-300℃ for 48 hours, and cooling to obtain the finished products; S5. Monitoring of thermal insulation of composite bricks. Put the composite brick sideways into the furnace mouth of the electric furnace, with the heavy part facing inward and the insulating part facing outward. The heavy part is wrapped with alumina fiber to the upper top, lower bottom and side walls of the furnace mouth of the electric furnace, and the insulating part is wrapped with aluminum silicate fiber cotton to the upper top, lower bottom, side walls and exposed part of the furnace mouth of the electric furnace. Put a 24mm thick steel plate that is smaller than the large end face of the composite brick close to the exposed large end face of the insulating part, and support it with a bracket underneath. The steel plate represents the wall of the rotary kiln, and the temperature of the steel plate surface represents the temperature of the rotary kiln skin. Heat up and keep warm for five hours, and monitor with an infrared thermometer.
2. The active lime rotary kiln low heat loss composite brick according to claim 1, It is characterized in that The aluminum oxide content in the alumina clinker rotary kiln ring material in S1 is 72.12%.
3. The low heat loss composite brick for active lime rotary kiln according to claim 1, It is characterized in that The crushing and fine grinding of the alumina clinker rotary kiln ring material and the crushing and fine grinding of the combined clay in S1 are specifically crushing and fine grinding into 100 mesh fine powder.
4. The active lime rotary kiln low heat loss composite brick according to claim 1, It is characterized in that The content of aluminum oxide combined with clay in the S1 is 25%.
5. The low heat loss composite brick for active lime rotary kiln according to claim 1, It is characterized in that The multi-grade aggregate in S1 is specifically the alumina clinker rotary kiln ring material crushed and graded into 0-5mm, 5-8mm, and 8-15mm aggregates.
6. The low heat loss composite brick for active lime rotary kiln according to claim 1, It is characterized in that The content of aluminum oxide in the 85 alumina clinker in the S2 is 85%, and the content of aluminum oxide in the combined clay in the S2 is 25%.
7. The low heat loss composite brick for active lime rotary kiln according to claim 1, It is characterized in that The multi-grade aggregates in S2 are specifically 0-1mm, 1-3mm, 3-5mm, and 5-8mm aggregates.
8. The low heat loss composite brick for active lime rotary kiln according to claim 1, It is characterized in that The pulverizing in S2 is specifically pulverizing and grinding into 180 mesh fine powder.
9. The active lime rotary kiln low heat loss composite brick according to claim 1, wherein the mixing in proportion in S1 and S2 is specifically mixing aluminum dihydrogen phosphate and water in a ratio of 2:1.