Preparation process of fire-resistant hollow sphere

Through the rolling technology of making core pellets and alumina fine powder, combined with the mold pressing and sintering process, the problem of the spherical surface of the refractory hollow sphere being not smooth and the wall thickness being difficult to control is solved, and precise control of the spherical surface smoothness and wall thickness is achieved, reducing the Reduce production costs and improve product quality.

CN118754685APending Publication Date: 2024-10-11ZHEJIANG CHUANG THERMAL CONDUCTIVE MATERIAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410791542.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The spherical surface of existing refractory hollow balls is easily not smooth, and the wall thickness and size are difficult to control, which limits their application in industrial production.

Method used

Using the method of making core pills, organic resin and alumina fine powder are used through the roller drum rolling technology, combined with the mold pressing and drying and sintering processes, to control the diameter and wall thickness of the hollow ball and improve the smoothness and compactness of the spherical surface.

Benefits of technology

It achieves the improvement of the spherical smoothness of the hollow sphere and the precise control of the wall thickness, reduces the production cost, reduces the generation and waste of harmful substances, and ensures the quality and fire resistance of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a preparation process of a fire-resistant hollow sphere, which mainly comprises the following preparation steps: S1, preparing a core pellet: confirming the hollow diameter of the fire-resistant hollow sphere, and preparing a small sphere with a corresponding diameter from organic resin as the core pellet; s2, adhering a shell: changing the blended alumina fine powder into a moisture-containing state, then putting the core ball into a rotating wheel cylinder filled with the moisture-containing alumina fine powder, and enabling the alumina fine powder to be continuously adhered to the core ball until the core ball is rolled into a large ball; s3, placing the large ball into a plurality of molds meeting the diameter requirements of the fire-resistant hollow ball, trimming, pressing and forming, and then drying a fire-resistant hollow ball green body subjected to pressing and forming; and S4, burning loss of the core pellets: sintering the dried fire-resistant hollow ball blank at a high temperature, burning loss and volatilization of the core pellets made of the organic resin, and sintering the left shells to obtain the fire-resistant hollow ball. The hollow ball has the beneficial effects that the smoothness of the spherical surface of the hollow ball is improved, and the wall thickness and size are convenient to control.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field related to the production of refractory hollow balls, in particular to a preparation process of refractory hollow balls. Background Art

[0002] There are two main types of refractory hollow balls: zirconia hollow balls and alumina hollow balls. There are two methods for preparing alumina hollow balls: rolling ball firing and melt blowing. Melt blowing is more commonly used, while rolling ball firing is not widely used in industrial production because the surface of the hollow balls produced by it is not smooth and the wall thickness and size are difficult to control. Summary of the invention

[0003] The present invention aims to overcome the shortcomings of the prior art that the surface of hollow balls is not smooth and the wall thickness and size are not easy to control, and provides a preparation process for refractory hollow balls with improved surface smoothness and convenient control of wall thickness and size.

[0004] In order to achieve the above object, the present invention adopts the following technical solutions: A preparation process of a refractory hollow ball mainly comprises the following preparation steps: S1. Making core pellets: confirm the hollow diameter of the refractory hollow ball, and make small balls of corresponding diameter from organic resin as core pellets; S2, sticking the shell: the blended alumina fine powder is changed to a state containing water, and then the core ball prepared in step S1 is placed in a rotating drum containing the alumina fine powder containing water, and the alumina fine powder is continuously adhered to the core ball until it is rolled into a large ball; S3, placing the large spheres prepared in step S2 into a mold having multiple diameters that meet the requirements of the refractory hollow spheres, trimming and pressing them, and then drying the pressed refractory hollow sphere blanks; S4. Burning out of core pellets: The dried refractory hollow ball blank is placed under high temperature for firing. The core pellets made of organic resin are burned out and volatilized, and the remaining shell is sintered to complete the refractory hollow ball.

[0005] Making the core balls by yourself makes it convenient to control the hollow diameter of the refractory hollow balls. Then using hydrated alumina fine powder makes it easier to wrap the core balls with alumina fine powder. Using molds to press and trim is convenient and accurate, and can also improve the compactness of the hollow balls. Then, the melting point difference between organic resin and alumina fine powder is used to achieve the purpose of making the refractory hollow balls hollow, thereby achieving the purpose of improving the smoothness of the hollow ball surface and facilitating the control of wall thickness and size.

[0006] Preferably, in step S1, the organic resin needs to be able to melt and shape at 100-250° C. Organic resin has a low melting point and is easy to shape so as to produce core pellets of different diameters.

[0007] Preferably, in step S1, the organic resin needs to be easily gasified and not easily adhered to alumina. The organic resin needs to be easily gasified and not easily adhered to the refractory solid ball so as not to affect its secondary utilization and reduce the generation of harmful substances in actual use.

[0008] Preferably, in step S2, the composition ratio of the alumina fine powder is 88-99 parts of alumina, 11.8-0.2 parts of silicon oxide, and 0.2-0.4 parts of iron oxide. The presence of other ingredients, and the low content of other ingredients, can reduce production costs and increase the refractory temperature.

[0009] Preferably, in step S2, the aluminum oxide fine powder absorbs water by continuous stirring under steam spraying. The aluminum oxide fine powder absorbs water by continuous stirring under steam spraying, so that the aluminum oxide fine powder can absorb water quickly and evenly and is not easy to stick.

[0010] Preferably, in step S2, before the core pellets are put into the rotating drum for rolling, the outer surface of the core pellets needs to be evenly coated with a binder, which can increase the viscosity of the alumina fine powder.

[0011] Preferably, in step S2, during the rolling of the core pellets in the rotary drum, the water-containing alumina fine powder is added in small amounts and multiple times, and the diameter of the rolled sphere needs to be larger than the diameter of the actually required hollow sphere. Adding alumina fine powder in small amounts and multiple times facilitates a more uniform coating thickness, and the diameter of the rolled sphere needs to be larger than the diameter of the actually required hollow sphere to facilitate later pressing and trimming.

[0012] Preferably, when the core pellets cannot be well bonded after rolling with alumina fine powder in small amounts for multiple times, the core pellets are taken out of the rotating drum for secondary coating with a bonding agent, which is used to improve the bonding degree.

[0013] Preferably, in step S3, the excess alumina fine powder after trimming and pressing of the refractory hollow sphere blank can be used for secondary coating of the core balls after being crushed and sieved. The secondary use of alumina fine powder can reduce waste and cost.

[0014] Preferably, in step S4, the burnout temperature of the refractory hollow ball blank is 1600-1800°C, and then the blank is cooled to remove slag, and finally qualified products are screened. The slag removal and screening after burnout can ensure that the product is qualified and reduce mutual contamination.

[0015] The beneficial effects of the present invention are as follows: the smoothness of the spherical surface of the hollow ball is improved and the wall thickness and size are conveniently controlled; the organic resin has a low melting point and is easy to shape so that core balls of different diameters can be made; the organic resin needs to be easy to gasify and not easy to stick to make a refractory solid ball so that its secondary utilization is not affected and the generation of harmful substances in actual use is reduced; there are other ingredients, and the other ingredients are not high, which is convenient to reduce production costs and improve the refractory temperature; the alumina fine powder absorbs moisture by continuous stirring under steam spraying, so that the alumina fine powder can quickly and evenly absorb moisture and is not easy to stick; the binder can increase the viscosity of the alumina fine powder; adding alumina fine powder in small amounts and multiple times can make the coating thickness more uniform, and the diameter of the rolled sphere needs to be larger than the actual required diameter of the hollow ball to facilitate later pressing and trimming; the secondary coating binder is used to improve the bonding degree; the secondary utilization of the alumina fine powder reduces waste and reduces costs; the slag removal and screening after burnout can ensure that the product is qualified and reduce mutual pollution. DETAILED DESCRIPTION

[0016] Embodiment 1, a preparation process of a refractory hollow ball, which mainly comprises the following preparation steps: S1. Making core balls: confirm the hollow diameter of the refractory hollow ball, melt and shape the organic resin which is easy to gasify and not easy to adhere to the alumina at 250°C into small balls of corresponding diameter as core balls; S2, adhesion shell: the fine alumina powder with a composition ratio of 99 parts of aluminum oxide, 0.2 parts of silicon oxide and 0.4 parts of iron oxide is continuously stirred under steam spraying to absorb water and become a state containing water. Before the core ball is added to the rotating drum for rolling, the outer surface of the core ball needs to be evenly coated with a binder, and then the core ball is placed in the rotating drum containing the water-containing fine alumina powder, so that the fine alumina powder is continuously adhered to the core ball. During the rolling of the core ball in the rotating drum, the water-containing fine alumina powder is added in small amounts and multiple times until it is rolled into a large ball and the diameter of the rolled ball needs to be larger than the actual required diameter of the hollow ball. If the rolled alumina fine powder cannot be well adhered, the core ball is taken out of the rotating drum for secondary coating with a binder; S3, shaping and drying: placing the prepared large spheres into a mold having multiple diameters that meet the requirements of the refractory hollow spheres, trimming and pressing the refractory hollow spheres, and then drying the pressed refractory hollow spheres. The excess alumina fine powder of the refractory hollow spheres after trimming and pressing can be used for secondary coating of the sticky core balls after being crushed and sieved; S4. Burning out of core pellets: The dried refractory hollow ball blanks are placed at 1800°C for sintering. The core pellets made of organic resin are burned out and volatilized, and the remaining shell is sintered to complete the refractory hollow ball. The refractory hollow ball is then cooled and slag is removed, and finally qualified products are screened.

[0017] Embodiment 2, a preparation process of a refractory hollow ball, which mainly comprises the following preparation steps: S1. Making core balls: confirm the hollow diameter of the refractory hollow ball, melt and shape the organic resin which is easy to gasify and not easy to adhere to the alumina at 100°C into small balls of corresponding diameter as core balls; S2, adhesion shell: the fine alumina powder with a composition ratio of 88 parts of aluminum oxide, 11.8 parts of silicon oxide and 0.2 parts of iron oxide is continuously stirred under steam spraying to absorb water and become a state containing water. Before the core ball is added to the rotating drum and rolled, the outer surface of the core ball needs to be evenly coated with a binder, and then the core ball is placed in the rotating drum with the water-containing fine alumina powder, so that the fine alumina powder is continuously adhered to the core ball. During the rolling of the core ball in the rotating drum, the water-containing fine alumina powder is added in small amounts and multiple times until it is rolled into a large ball and the diameter of the rolled ball needs to be larger than the actual required diameter of the hollow ball. If the rolled alumina fine powder cannot be well bonded, the core ball is taken out of the rotating drum for a second coating with a binder; S3, shaping and drying: placing the prepared large spheres into a mold having multiple diameters that meet the requirements of the refractory hollow spheres, trimming and pressing the refractory hollow spheres, and then drying the pressed refractory hollow spheres. The excess alumina fine powder of the refractory hollow spheres after trimming and pressing can be used for secondary coating of the sticky core balls after being crushed and sieved; S4. Burning out of core pellets: The dried refractory hollow ball blanks are placed at 1600°C for sintering. The core pellets made of organic resin are burned out and volatilized, and the remaining shell is sintered to complete the refractory hollow ball. The refractory hollow ball is then cooled and slag is removed, and finally qualified products are screened.

[0018] Comparative Example 1, a preparation process of a refractory hollow ball, which mainly includes the following preparation steps: S1. Making core pellets: confirm the hollow diameter of the refractory hollow ball, melt and shape the organic resin at 100°C into small balls of corresponding diameter as core pellets; S2, adhesion shell: the fine alumina powder with a composition ratio of 88 parts of aluminum oxide, 11.8 parts of silicon oxide and 0.2 parts of iron oxide is used to absorb water under steam spraying to become a state containing water. Before the core ball is added to the rotating drum for rolling, the outer surface of the core ball needs to be evenly coated with a binder, and then the core ball is placed in the rotating drum containing the water-containing fine alumina powder, so that the fine alumina powder is continuously adhered to the core ball. If the rolled alumina fine powder cannot be well adhered, the core ball is taken out of the rotating drum for a second coating with a binder; S3. Burning out of core pellets: The dried refractory hollow ball blanks are placed at 1600°C for sintering. The core pellets made of organic resin are burned out and volatilized, and the remaining shell is sintered to complete the refractory hollow ball. The refractory hollow ball is then cooled and finally qualified products are screened.

[0019] Comparative Example 2, a preparation process of a refractory hollow ball, which mainly includes the following preparation steps: S1. Making core pellets: using organic resin balls as core pellets; S2. Adhesion to the shell: The fine alumina powder with a composition ratio of 99 parts of aluminum oxide, 0.2 parts of silicon oxide and 0.4 parts of iron oxide absorbs water to become a state containing water. Before the core ball is added to the rotating drum, the outer surface of the core ball needs to be evenly coated with a binder, and then the core ball is placed in the rotating drum containing the water-containing fine alumina powder, so that the fine alumina powder continues to adhere to the core ball; S4. Burning out of core pellets: The dried refractory hollow ball blanks are placed at 1800°C for sintering. The core pellets made of organic resin are burned out and volatilized, and the remaining shell is sintered to complete the refractory hollow ball. Finally, qualified products are screened.

[0020] Table 1 below shows the analysis results of the natural bulk density and intact rate of Examples 1 to 2 of the present invention and Comparative Examples 1 to 2.

[0021] Table 1

Claims

1. A process for preparing refractory hollow balls, characterized in that: The method mainly includes the following preparation steps: S1. Making core pellets: confirm the hollow diameter of the refractory hollow ball, and make small balls of corresponding diameter from organic resin as core pellets; S2, sticking the shell: the blended alumina fine powder is changed to a state containing water, and then the core ball prepared in step S1 is placed in a rotating drum containing the alumina fine powder containing water, and the alumina fine powder is continuously adhered to the core ball until it is rolled into a large ball; S3, shaping and drying: placing the large spheres prepared in step S2 into a mold having multiple diameters that meet the requirements of the refractory hollow spheres, trimming and pressing them, and then drying the pressed refractory hollow sphere blanks; S4. Burning out of core pellets: The dried refractory hollow ball blank is placed under high temperature for firing. The core pellets made of organic resin are burned out and volatilized, and the remaining shell is sintered to complete the refractory hollow ball.

2. The process for preparing a refractory hollow ball according to claim 1, characterized in that: In step S1, the organic resin needs to be able to be melted and shaped at 100-250°C.

3. The process for preparing a refractory hollow ball according to claim 1, characterized in that: In step S1, the organic resin needs to be easily vaporized and not easily adhered to the alumina.

4. The process for preparing a refractory hollow ball according to claim 1, characterized in that: In step S2, the composition ratio of the aluminum oxide fine powder is 88-99 parts of aluminum oxide, 11.8-0.2 parts of silicon oxide, and 0.2-0.4 parts of iron oxide.

5. The process for preparing a refractory hollow ball according to claim 1, characterized in that: In step S2, the aluminum oxide fine powder absorbs water by continuous stirring under steam spraying.

6. The process for preparing a refractory hollow ball according to claim 1, characterized in that: In step S2, before the core balls are put into the rolling process of the rotary drum, the outer surface of the core balls needs to be evenly coated with a binder.

7. The process for preparing refractory hollow spheres according to claim 6, characterized in that: In step S2, during the rolling process of the core balls in the rotary drum, the water-containing alumina fine powder is added in small amounts and multiple times, and the diameter of the rolled spheres needs to be larger than the diameter of the actually required hollow spheres.

8. The process for preparing refractory hollow spheres according to claim 7, characterized in that: When the core pellets cannot be well bonded after being rolled with alumina fine powder in small amounts for multiple times, the core pellets are taken out of the rotating drum and coated with a binder for a second time.

9. The process for preparing a refractory hollow ball according to claim 1, characterized in that: In step S3, the excess alumina fine powder of the refractory hollow sphere blank after trimming and pressing can be crushed and sieved and then used for secondary coating of the core ball.

10. The process for preparing refractory hollow spheres according to claim 1, characterized in that: In step S4, the burnout temperature of the refractory hollow ball blank is 1600-1800°C, and then the blank is cooled to remove slag, and finally qualified products are screened.

Citation Information

Patent Citations

  • High-strength and low-density ceramic hollow ball and preparation method thereof

    CN102557594A

  • Preparation method of fused quartz hollow spheres

    CN102701573A

  • Preparation method for alumina hollow spheres

    CN103274672A

  • Refractory heat-isolating hollow ball and its preparation

    CN1184088A

  • Thick-wall tabular corundum hollow ball

    CN203582747U