A soil water-retaining agent and preparation method thereof

Through the graft reaction of carboxymethyl cellulose and polymerized phosphorus tailings biochar composite, an efficient water absorber is formed, which solves the problem of insufficient service life and water absorption effect of soil water retention agent, and has achieved improved water absorption performance and loose soil structure, avoiding Soil slab effect.

CN118755019BActive Publication Date: 2024-11-22SHANDONG YINGLAIWANG AGRI TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411244180.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-22
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

The existing soil water retention agents have shortcomings in service life and water absorption effect, and the graft of cellulose derivatives leads to soil slab problems.

Method used

Carboxymethylcellulose and polymerized phosphorus tailings biochar composites are used to graft acrylic acid and acrylamide. Through specific chemical treatment and pyrolysis steps, a water retention agent with high water absorption capacity and porous structure is formed to reduce soil viscosity.

Benefits of technology

It significantly improves the water absorption rate and water absorption rate of the soil water retention agent, extends the service life, and improves the soil structure, reduces the soil hardness, and avoids the slab-setting problem.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention provides a soil water retainer and a preparation method thereof, belonging to the technical field of soil conditioning materials. The preparation method comprises preparing a polymerized phosphate tailings biochar composite material and a grafting reaction; in the grafting reaction, carboxymethyl cellulose and the polymerized phosphate tailings biochar composite material are added to deionized water, stirred evenly at 80-90°C, and acrylic acid, acrylamide, initiator ammonium persulfate, and crosslinking agent N, N′-methylenebisacrylamide are added in a nitrogen environment at a temperature of 60-70°C, reacted for 1.5-2.5h, and then the reaction product is dried and crushed to obtain a water retainer. The water retainer prepared by the present invention has a high water absorption rate of 549.87-561.37g / g; the water retainer of the present invention has a fast water absorption rate, the water absorption rate reaches 78.55-80.20g / (g·min), and the soil hardness is 4.86-4.95kg / cm².
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of soil conditioning materials, and in particular relates to a soil water retaining agent and a preparation method thereof. Background Art

[0002] Soil water-retaining agent is a high-molecular polymer containing hydrophilic groups such as hydroxyl and carboxyl. It can absorb a large amount of water, improve the water retention capacity of the soil, and slowly release it when there is a shortage of water, thus achieving a water-saving effect.

[0003] Cellulose has multiple hydrophilic groups such as carboxyl and hydroxyl groups, and is a common material used to prepare water-retaining agents. Currently, there are two common methods for preparing water-retaining agents from cellulose;

[0004] One method of preparing a water retainer is to extract cellulose from crop straw, plant rhizomes, fruit peels, etc., and then graft hydrophilic monomers. However, due to structural reasons, cellulose has small pores, resulting in poor water absorption. The water absorption effect can be improved by grafting hydrophilic monomers with other grafts and cellulose. For example, CN117164780A discloses a cellulose-humic acid composite water retainer and a preparation method thereof. The water retainer is prepared by grafting cellulose and humic acid with acrylic acid and acrylamide. Although the addition of humic acid can improve the water and salt absorption effects of the water retainer and is environmentally friendly, humic acid is easily degraded, which will reduce the service life of the water retainer.

[0005] Another method for preparing a water-retaining agent is to graft a hydrophilic monomer onto a cellulose derivative. For example, CN114478926A discloses a water hyacinth carboxymethyl cellulose salt-resistant-super absorbent resin and a preparation method thereof. The super absorbent resin is prepared by grafting carboxymethyl cellulose onto acrylic acid. Although the super absorbent resin has a long service life and good water-retaining effect, carboxymethyl cellulose has a strong polarity. After grafting with acrylic acid, the number of carboxyl groups in the hydrophilic group increases, resulting in a stronger polarity of the super absorbent resin. After being applied to the soil, the soil viscosity will increase, causing soil compaction. Summary of the invention

[0006] In view of the problems existing in the prior art, the present invention provides a soil water-retaining agent and a preparation method thereof, so as to achieve the following invention objectives: prolong the service life of the water-retaining agent, improve the water-retaining effect, and improve the problem of soil compaction.

[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0008] A method for preparing a soil water-retaining agent comprises the following steps:

[0009] 1. Preparation of carboxymethyl cellulose

[0010] Rinse the corn stalks with deionized water, cut them into small pieces of 0.5-3 cm, dry them to a moisture content of 7-9%, and then crush them into stalk particles with a particle size of 0.1-0.5 mm. Add the stalk particles to a 23-28 wt% NaOH solution, place them at room temperature for 0.5-2 hours, then drip chloroacetic acid solution into them, and control the dripping rate at 1-2 mL / min. During the dripping process, keep the reaction temperature at 60-70 ° C. After the dripping is completed, cool to room temperature, and then adjust the pH value to 7.5-8.5 with NaOH solution. After continuing the reaction for 2.5-3.5 hours, adjust the pH value to 2.8-3.2 with dilute HCl, then filter, wash the filter cake with distilled water until it is neutral, and then dry it in a drying oven at 75-85 ° C to constant weight to obtain carboxymethyl cellulose;

[0011] The mass ratio of the corn stalk to the 25wt% NaOH solution is 0.8-1.2:0.5-1.5;

[0012] The mass fraction of chloroacetic acid in the chloroacetic acid solution is 28-32%;

[0013] The mass ratio of chloroacetic acid to straw particles is 19-21:6-8;

[0014] The carboxymethyl cellulose, i.e., cellulose whose hydroxyl groups are replaced by carboxymethyl groups, has a stronger water absorption capacity than cellulose.

[0015] 2. Preparation of polymerized phosphate tailings

[0016] Put the phosphate tailings into the phosphoric acid solution and start stirring at the same time. After reacting at room temperature until no gas is generated, place the slurry after the reaction in a muffle furnace and heat it to 180-220°C at a rate of 5-15°C / min, calcine and dry for 0.8-1.3h, then heat it to 500-600°C at the same rate, continue heating for 2.7-3.3h, take out the product after cooling, grind it into a particle size of 0.03-0.09mm, and obtain the polymerized phosphate tailings for standby use;

[0017] The phosphate tailings include the following components by mass fraction: P2O5: 7.07%, MgO: 16.2%, Al2O3: 0.24%, CaO: 35.11%, Fe2O3: 0.24%;

[0018] The stirring speed is 25-35 r / min;

[0019] The mass fraction of phosphoric acid in the phosphoric acid solution is 16 to 24%;

[0020] The mass ratio of the phosphate tailings to the phosphoric acid solution is 1.7-2.3:4-6;

[0021] The polymerized phosphate tailings have a spherical structure. During the polymerization process, the water in the slurry and the water released between molecules escape from the inside of the sphere to form irregular pores, thereby increasing the specific surface area.

[0022] 3. Preparation of polymerized phosphate tailings biochar composites

[0023] Cut the corn stalks into small pieces of 0.5 to 3 cm, and then dry them in a drying oven at 75 to 85°C to constant weight. Add the polymerized phosphate tailings and dried corn stalks into deionized water and ultrasonically disperse them for 1.5 to 2.5 hours, and then stir the mixed slurry at 78 to 82°C for 0.5 to 1.5 hours. After the reaction is completed, filter, collect the filter cake, and place it in a muffle furnace. Under a N2 environment, heat to 430 to 470°C at a rate of 15 to 25°C / min, and maintain the current temperature for pyrolysis for 1.8 to 2.2 hours. After the pyrolysis is completed, wash the collected black solid product with anhydrous ethanol and deionized water several times until the washing liquid is neutral. Finally, dry the product in a drying oven at 75 to 85°C to constant weight, and the obtained product is a polymerized phosphate tailings biochar composite material;

[0024] The stirring speed is 140-160 r / min;

[0025] The mass ratio of the dried corn stalks, polymerized phosphate tailings, and deionized water is 4-6:0.5-2:6-8;

[0026] The polymerized phosphate tailings biochar composite material, in which biochar is composited with polymerized phosphate tailings, will increase the pores of the biochar, enrich the functional groups (such as −COOH, −OH), and enhance the adsorption effect.

[0027] 4. Grafting reaction

[0028] Add carboxymethyl cellulose and polymerized phosphate tailings biochar composite material into deionized water, stir for 25 to 35 minutes to make it evenly dispersed, and keep the stirring process at 80 to 90°C. Add acrylic acid, acrylamide, initiator ammonium persulfate, and crosslinking agent N, N′-methylenebisacrylamide in a nitrogen environment at a temperature of 60 to 70°C, and react for 1.5 to 2.5 hours. After the solution becomes viscous and climbs the rod, take out the reaction product, dry it in a drying oven at 70 to 90°C for 3 to 5 hours, and finally crush it into particles with a diameter of 1 to 4 mm to obtain finished water-retaining agent particles;

[0029] The stirring speed is 50-70 r / min;

[0030] The mass ratio of the carboxymethyl cellulose, the polymerized phosphate tailings biochar composite material, deionized water, acrylic acid, acrylamide, the initiator, and the crosslinking agent is 1-3: 0.3-0.7: 4-6: 15-17: 6-10: 0.13-0.17: 0.01-0.03;

[0031] The water retaining agent, carboxymethyl cellulose and polymerized phosphate tailings biochar composite material are jointly grafted with acrylic acid and acrylamide, so that the obtained water retaining agent has more porous structures while ensuring the water absorption capacity. After being applied to the soil, the problem of soil compaction can be effectively solved.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] The water-retaining agent prepared by the invention has a high water absorption rate of 549.87-561.37 g / g (NY∕T 886-2016); the water-retaining agent of the invention has a fast water absorption rate of 78.55-80.20 g / (g·min); and the soil hardness after the water-retaining agent is applied for 30 days is 4.86-4.95 kg / cm². DETAILED DESCRIPTION

[0034] Example 1

[0035] 1. Preparation of carboxymethyl cellulose

[0036] Rinse the corn stalks with deionized water, cut them into small pieces of 1-2 cm, dry them to 8% moisture content, and then crush them into stalk particles with a particle size of 0.3-0.4 mm. Add the stalk particles to a 25wt% NaOH solution, place them at room temperature for 1 hour, then drip chloroacetic acid solution into them, and control the dripping rate at 1.5mL / min. During the dripping process, keep the reaction temperature at 65°C. After the dripping is completed, cool it to room temperature, and then adjust the pH value to 8 with NaOH solution. After continuing the reaction for 3 hours, adjust the pH value to 3 with dilute HCl, then filter, wash the filter cake with distilled water until it is neutral, and then dry it in a drying oven at 80°C to constant weight to obtain carboxymethyl cellulose;

[0037] The mass ratio of the corn stalk to the 25wt% NaOH solution is 1:1;

[0038] The mass fraction of chloroacetic acid in the chloroacetic acid solution is 30%;

[0039] The mass ratio of the chloroacetic acid to the straw particles is 20:7.

[0040] 2. Preparation of polymerized phosphate tailings

[0041] Put the phosphate tailings into the phosphoric acid solution and start stirring at the same time. After reacting at room temperature until no gas is generated, place the slurry after the reaction in a muffle furnace and heat it to 200°C at a rate of 10°C / min, calcine and dry for 1 hour, then heat it to 550°C at the same rate, continue heating for 3 hours, take out the product after cooling, grind it into a particle size of 0.05-0.07 mm, and obtain the polymerized phosphate tailings for standby use;

[0042] The stirring speed is 30r / min;

[0043] The mass fraction of phosphoric acid in the phosphoric acid solution is 20%;

[0044] The mass ratio of the phosphate tailings to the phosphoric acid solution is 2:5.

[0045] 3. Preparation of polymerized phosphate tailings biochar composites

[0046] Cut the corn stalks into small pieces of 1 to 2 cm, and then dry them in a drying oven at 80°C to constant weight. Add the polymerized phosphate tailings and dried corn stalks into deionized water and ultrasonically disperse them for 2 hours, and then stir the mixed slurry at 80°C for 1 hour. After the reaction is completed, filter, collect the filter cake, and place it in a muffle furnace. Under a N2 environment, heat to 450°C at a rate of 20°C / min, and maintain the current temperature for pyrolysis for 2 hours. After the pyrolysis is completed, wash the collected black solid product with anhydrous ethanol and deionized water several times until the washing liquid is neutral. Finally, dry the product in a drying oven at 80°C to constant weight, and the obtained product is a polymerized phosphate tailings biochar composite material;

[0047] The stirring speed is 150r / min;

[0048] The mass ratio of the dried corn stalks, polymerized phosphate tailings and deionized water is 5:1:7.

[0049] 4. Grafting reaction

[0050] Add carboxymethyl cellulose and polymerized phosphate tailings biochar composite material into deionized water and stir for 30 minutes to make it evenly dispersed, and keep the stirring process at 85°C. Add acrylic acid, acrylamide, initiator ammonium persulfate, and crosslinking agent N, N′-methylenebisacrylamide in a nitrogen environment at a temperature of 65°C, and react for 2 hours. After the solution becomes viscous and climbs the rod, take out the reaction product, dry it in a drying oven at 80°C for 4 hours, and finally crush it into particles with a diameter of 2 to 3 mm to obtain the finished water retaining agent particles;

[0051] The stirring speed is 60r / min;

[0052] The mass ratio of the carboxymethyl cellulose, the polymerized phosphate tailings biochar composite material, deionized water, acrylic acid, acrylamide, the initiator, and the crosslinking agent is 2:0.5:5:16:8:0.15:0.02.

[0053] Example 2

[0054] 1. Preparation of carboxymethyl cellulose

[0055] Rinse the corn stalks with deionized water, cut them into small pieces of 0.5-1.0 cm, dry them to 7% moisture content, and then crush them into stalk particles with a particle size of 0.1-0.3 mm. Add the stalk particles to a 23wt% NaOH solution, place them at room temperature for 0.5 h, then drip chloroacetic acid solution into them, and control the dripping rate at 1.0 mL / min. During the dripping process, keep the reaction temperature at 60°C, cool to room temperature after the dripping is completed, and then adjust the pH value to 7.5 with NaOH solution. After continuing the reaction for 2.5 h, adjust the pH value to 2.8 with dilute HCl, then filter, wash the filter cake with distilled water until it is neutral, and then dry it in a drying oven at 75°C to constant weight to obtain carboxymethyl cellulose;

[0056] The mass ratio of the corn stalk to the 23wt% NaOH solution is 0.8:0.5;

[0057] The mass fraction of chloroacetic acid in the chloroacetic acid solution is 28%;

[0058] The mass ratio of the chloroacetic acid to the straw particles is 19:6.

[0059] 2. Preparation of polymerized phosphate tailings

[0060] Put the phosphate tailings into the phosphoric acid solution and start stirring at the same time. After reacting at room temperature until no gas is generated, place the slurry after the reaction in a muffle furnace and heat it to 180°C at a rate of 5°C / min, calcine and dry for 0.8h, then heat it to 500°C at the same rate, continue heating for 2.7h, take out the product after cooling, grind it into a particle size of 0.03-0.05mm, and obtain the polymerized phosphate tailings for standby use;

[0061] The stirring speed is 25r / min;

[0062] The mass fraction of phosphoric acid in the phosphoric acid solution is 16%;

[0063] The mass ratio of the phosphate tailings to the phosphoric acid solution is 1.7:4.

[0064] 3. Preparation of polymerized phosphate tailings biochar composites

[0065] Cut the corn stalks into small pieces of 0.5-1 cm, and then dry them in a drying oven at 75°C to constant weight. Add the polymerized phosphate tailings and dried corn stalks into deionized water and ultrasonically disperse them for 1.5 hours, and then stir the mixed slurry at 78°C for 0.5 hours. After the reaction is completed, filter, collect the filter cake, and place it in a muffle furnace. Under a N2 environment, heat to 430°C at a rate of 15°C / min, and maintain the current temperature for pyrolysis for 1.8 hours. After the pyrolysis is completed, wash the collected black solid product with anhydrous ethanol and deionized water several times until the washing liquid is neutral. Finally, dry the product in a drying oven at 75°C to constant weight, and the obtained product is a polymerized phosphate tailings biochar composite material;

[0066] The stirring speed is 140r / min;

[0067] The mass ratio of the dried corn stalks, polymerized phosphate tailings and deionized water is 4:0.5:6.

[0068] 4. Grafting reaction

[0069] Add carboxymethyl cellulose and polymerized phosphate tailings biochar composite material into deionized water and stir for 25 minutes to make it evenly dispersed. Keep the stirring process at 80°C. Add acrylic acid, acrylamide, initiator ammonium persulfate, and crosslinking agent N, N′-methylenebisacrylamide in a nitrogen environment at 60°C. React for 1.5 hours. After the solution becomes viscous and climbs the rod, take out the reaction product, dry it in a drying oven at 70°C for 3 hours, and finally crush it into particles with a diameter of 1 to 2 mm to obtain finished water retaining agent particles;

[0070] The stirring speed is 50r / min;

[0071] The mass ratio of the carboxymethyl cellulose, the polymerized phosphate tailings biochar composite material, deionized water, acrylic acid, acrylamide, the initiator, and the crosslinking agent is 1:0.3:4:15:6:0.13:0.01.

[0072] Example 3

[0073] 1. Preparation of carboxymethyl cellulose

[0074] Rinse the corn stalks with deionized water, cut them into small pieces of 2 to 3 cm, dry them to 9% moisture content, and then crush them into stalk particles with a particle size of 0.4 to 0.5 mm. Add the stalk particles to a 28wt% NaOH solution, place them at room temperature for 2 hours, then drip chloroacetic acid solution into them, and control the dripping rate at 2mL / min. During the dripping process, keep the reaction temperature at 70°C, cool to room temperature after the dripping is completed, and then adjust the pH value to 8.5 with NaOH solution. After continuing the reaction for 3.5 hours, adjust the pH value to 3.2 with dilute HCl, then filter, wash the filter cake with distilled water until it is neutral, and then dry it in a drying oven at 85°C to constant weight to obtain carboxymethyl cellulose;

[0075] The mass ratio of the corn stalk to the 25wt% NaOH solution is 1.2:1.5;

[0076] The mass fraction of chloroacetic acid in the chloroacetic acid solution is 32%;

[0077] The mass ratio of the chloroacetic acid to the straw particles is 21:8.

[0078] 2. Preparation of polymerized phosphate tailings

[0079] Put the phosphate tailings into the phosphoric acid solution and start stirring at the same time. After reacting at room temperature until no gas is generated, place the slurry after the reaction in a muffle furnace and heat it to 220°C at a rate of 15°C / min, calcine and dry for 1.3h, then heat it to 600°C at the same rate, continue heating for 3.3h, take out the product after cooling, grind it into a particle size of 0.07-0.09mm, and obtain the polymerized phosphate tailings for standby use;

[0080] The stirring speed is 35r / min;

[0081] The mass fraction of phosphoric acid in the phosphoric acid solution is 24%;

[0082] The mass ratio of the phosphate tailings to the phosphoric acid solution is 2.3:6.

[0083] 3. Preparation of polymerized phosphate tailings biochar composites

[0084] Cut the corn stalks into small pieces of 2 to 3 cm, and then dry them in a drying oven at 85°C to constant weight. Add the polymerized phosphate tailings and dried corn stalks into deionized water and ultrasonically disperse them for 2.5 hours, and then stir the mixed slurry at 82°C for 1.5 hours. After the reaction is completed, filter, collect the filter cake, and place it in a muffle furnace. Under a N2 environment, heat to 470°C at a rate of 25°C / min, and maintain the current temperature for pyrolysis for 2.2 hours. After the pyrolysis is completed, wash the collected black solid product with anhydrous ethanol and deionized water several times until the washing liquid is neutral. Finally, dry the product in a drying oven at 85°C to constant weight, and the obtained product is a polymerized phosphate tailings biochar composite material;

[0085] The stirring speed is 160r / min;

[0086] The mass ratio of the dried corn stalks, polymerized phosphate tailings and deionized water is 6:2:8.

[0087] 4. Grafting reaction

[0088] Add carboxymethyl cellulose and polymerized phosphate tailings biochar composite material into deionized water and stir for 35 minutes to make it evenly dispersed. Keep the stirring process at 90°C. Add acrylic acid, acrylamide, initiator ammonium persulfate, and crosslinking agent N, N′-methylenebisacrylamide in a nitrogen environment at 70°C. React for 2.5 hours. After the solution becomes viscous and climbs the rod, take out the reaction product, dry it in a drying oven at 90°C for 5 hours, and finally crush it into particles with a diameter of 3 to 5 mm to obtain the finished water retaining agent particles;

[0089] The stirring speed is 70r / min;

[0090] The mass ratio of the carboxymethyl cellulose, the polymerized phosphate tailings biochar composite material, deionized water, acrylic acid, acrylamide, the initiator, and the cross-linking agent is 3:0.7:6:17:10:0.17:0.03.

[0091] Comparative Example 1

[0092] In order to verify the effect of the polymerized phosphate tailings biochar composite material, the same soil water retaining agent and preparation method as in Example 1 were used, except that the addition of the polymerized phosphate tailings biochar composite material was omitted in step 4.

[0093] Comparative Example 2

[0094] In order to verify the effect of biochar, the same soil water retaining agent and preparation method as in Example 1 were used, except that the addition of polymerized phosphate tailings powder was omitted in step 3 to finally prepare biochar, and the polymerized phosphate tailings biochar composite material was replaced with biochar in step 4.

[0095] Test example

[0096] The water absorption ratio, water absorption rate and soil hardness of the soil water retaining agents prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were tested, and the test results are as follows:

[0097]

[0098] Test Method

[0099] (1) Determination of water absorption ratio: Weigh 1g of soil water retaining agent of Examples 1 to 3 and Comparative Examples 1 to 2 (mass is recorded as m1) and mix with 1000mL of water for 30min to allow the water retaining agent to fully absorb water and swell. Pour the water retaining agent gel into a sieve with a pore size of 0.18mm, filter and weigh (mass is recorded as m2). The calculation formula of water absorption ratio Q (g / g) is as follows;

[0100]

[0101] (2) Determination of water absorption rate: Weigh 1g of soil water retaining agent of Examples 1 to 3 and Comparative Examples 1 to 2 (mass is recorded as m1) and 1000mL of water, mix and stir for 7min to obtain water retaining agent gel, pour the water retaining agent gel into a sieve with a pore size of 0.18mm, filter and weigh (mass is recorded as m2). The water absorption rate V (g / (g·min)) is calculated as follows:

[0102]

[0103] The water absorption rate is the average rate of the soil water retaining agent within 7 minutes.

[0104] (3) Determination of soil hardness: The soil water retaining agents of Examples 1 to 3 and Comparative Examples 1 to 2 were mixed with fine dry soil in a mass ratio of 1:10, and evenly sprinkled on the surface of the test soil. The mixture was then turned into a soil layer about 5 to 10 cm deep and then watered thoroughly. The hardness of the test soil was measured using a soil hardness meter after 15 days and 30 days.

[0105] The specific determination method is to use a Yamanaka-type soil hardness tester to measure points on the surface of the test soil to be tested. The interval between points is 20 cm, the number of points is 30, and the average value of the measurement results is finally taken.

[0106] It can be seen from the above results that the water absorption rate of Example 1 is slightly higher than that of Comparative Example 1, and the soil hardness is significantly lower than that of Comparative Example 1. This shows that the polymerized phosphate tailings biochar composite material has a certain water absorption effect, and its unique porous structure will make the soil loose and reduce the soil hardness after being applied to the soil; it can be seen from Example 1 and Comparative Example 2 that the composite of biochar and polymerized phosphate tailings will increase the porosity of biochar, strengthen the adsorption effect, and improve the soil hardness.

[0107] Furthermore, after carboxymethyl cellulose is grafted with acrylic acid and acrylamide on the polymerized phosphate tailings biochar composite material, the polymerized phosphate tailings biochar composite material can enlarge the gaps in the carboxymethyl cellulose network structure, increase the distance between the carboxyl groups therein, and reduce the polarity of the water retaining agent, thereby reducing soil viscosity, that is, reducing soil hardness.

Claims

1. A method for preparing a soil water-retaining agent, characterized in that: The preparation method comprises preparing a polymerized phosphorus tailings biochar composite material and a grafting reaction; The method for preparing the polymerized phosphate tailings biochar composite material comprises adding the polymerized phosphate tailings and dried corn stalks into deionized water and ultrasonically dispersing them, then stirring the mixed slurry at a temperature of 78 to 82° C. for 0.5 to 1.5 hours, collecting the filter cake after filtering, heating the mixture to 430 to 470° C. at a rate of 15 to 25° C. / min in a N2 environment, pyrolyzing the mixture for 1.8 to 2.2 hours, and washing and drying the mixture to obtain the polymerized phosphate tailings biochar composite material; The preparation method of the polymerized phosphate tailings comprises the following steps: placing the phosphate tailings into a phosphoric acid solution, stirring the solution at the same time, reacting at room temperature until no gas is generated, heating the slurry after the reaction to 180-220° C. at a rate of 5-15° C. / min, calcining and drying the slurry for 0.8-1.3 h, then heating the slurry to 500-600° C. at the same rate, continuing to heat the slurry for 2.7-3.3 h, cooling the slurry, taking out the slurry, grinding the slurry to a particle size of 0.03-0.09 mm, and obtaining the polymerized phosphate tailings; In the grafting reaction, carboxymethyl cellulose and polymerized phosphate tailings biochar composite material are added into deionized water, stirred evenly at 80-90° C., acrylic acid, acrylamide, initiator ammonium persulfate, and crosslinking agent N,N′-methylenebisacrylamide are added in a nitrogen environment at a temperature of 60-70° C., reacted for 1.5-2.5 hours, and then the reaction product is dried and crushed to obtain a water retaining agent.

2. The method for preparing a soil water-retaining agent according to claim 1, characterized in that: In the step of preparing the polymerized phosphate tailings biochar composite material, the mass ratio of the dried corn stalks, polymerized phosphate tailings, and deionized water is 4-6:0.5-2:6-8.

3. The method for preparing a soil water-retaining agent according to claim 1, characterized in that: In the step of preparing the polymerized phosphate tailings biochar composite material, the length of the dried corn stalks is 0.5 to 3 cm.

4. The method for preparing a soil water-retaining agent according to claim 1, characterized in that: In the grafting reaction step, the mass ratio of carboxymethyl cellulose, polymerized phosphate tailings biochar composite material, deionized water, acrylic acid, acrylamide, initiator and crosslinking agent is 1-3: 0.3-0.7: 4-6: 15-17: 6-10: 0.13-0.17: 0.01-0.

03.

5. The method for preparing a soil water-retaining agent according to claim 1, characterized in that: The mass ratio of the phosphate tailings to the phosphoric acid solution is 1.7-2.3:4-6; the mass fraction of phosphoric acid in the phosphoric acid solution is 16-24%.

6. The method for preparing a soil water-retaining agent according to claim 1, characterized in that: The preparation method of the carboxymethyl cellulose comprises the following steps: drying corn stalks, crushing them into stalk particles of 0.1 to 0.5 mm, adding them into a 23 to 28 wt % NaOH solution, placing them at room temperature for 0.5 to 2 hours, dripping chloroacetic acid solution therein, maintaining the reaction temperature at 60 to 70° C. during the dripping process, cooling the reaction mixture to room temperature after the dripping is completed, adjusting the pH value to 7.5 to 8.5, continuing the reaction for 2.5 to 3.5 hours, adjusting the pH value to 2.8 to 3.2, and then washing and drying the mixture to obtain the carboxymethyl cellulose.

7. The method for preparing a soil water-retaining agent according to claim 6, characterized in that: The mass ratio of the corn stalk to the 25wt% NaOH solution is 0.8-1.2:0.5-1.5; the mass fraction of chloroacetic acid in the chloroacetic acid solution is 28-32%; and the mass ratio of chloroacetic acid to the stalk particles is 19-21:6-8.

8. The soil water-retaining agent prepared by the preparation method according to any one of claims 1 to 7.

Citation Information

Cited By

  • Water-absorbing material capable of retaining water for soil and automatically supplying fertilizer as well as preparation method and application of water-absorbing material

    CN121271557A