Polyester resin for low-temperature curing high-transparency powder and preparation method
By designing a polyester resin with short linear segments and high degree of branching, and adding appropriate catalysts and accelerators in the esterification reaction, the problems of high softening point and low light transmittance of polyester resin in the TGIC curing system are solved. Achieve low-temperature curing and high-transparency coating effects.
Patent Information
- Application Number
- CN202411109138.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-10-11
AI Technical Summary
The polyester resin in the existing TGIC curing system has a high degree of linear polymerization, resulting in a high softening point, insufficient fluidity at low temperatures, making it difficult to cure, and the light transmittance deteriorates, making it difficult to reach 92% or above.
Triethanolamine, isobutyric acid, terephthalic acid, 2-ethyl-1,3-hexanediol, and glycerol triglycidyl ether are used for polymerization to design a polyester with short linear segments and high degree of branching. Resin, and add esterification reaction catalyst, antioxidant and low-temperature curing accelerator to the esterification reaction to achieve low-temperature curing through specific process steps.
The polyester resin is fully cured at low temperature, with a flat and smooth surface, good impact resistance and gloss. The cured coating film has excellent leveling and light transmittance, which is much higher than that of ordinary polyester resin, reaching more than 92% transmittance. light rate.
Smart Images

Figure BDA0004991663210000021 
Figure BDA0004991663210000041 
Figure BDA0004991663210000051
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of powder coatings, and in particular relates to a polyester resin for low-temperature curing high-transparency powder and a preparation method thereof, as well as application in a TGIC curing system. Background Art
[0002] Powder coating is a solid powdered synthetic resin coating composed of solid resin, pigment, filler and additives. Different from ordinary solvent-based coating and water-based coating, its dispersion medium is not solvent and water, but air. It has the characteristics of no solvent pollution, 100% film formation and low energy consumption. The full name of TGIC is triglycidyl isocyanurate. TGIC powder coating has relatively excellent comprehensive performance and is used in large quantities. In recent years, with the improvement of the decorative properties of powder coatings, transparent powder coatings have also been widely used. For example, they are used on mirror surfaces, instruments and equipment with high surface transparency, photovoltaic panels and other surfaces. However, in ordinary polyester resin powder coatings, due to the high linear polymerization degree and large molecular weight of polyester resin, there are often the following deficiencies: (1) The high linear polymerization degree leads to a high softening point of polyester resin, which is generally 115°C or above, resulting in insufficient fluidity at low temperatures, difficulty in curing at low temperatures, and poor surface leveling; (2) The high linear polymerization degree will also lead to an increase in the crystallinity of the polyester resin, resulting in a poor transmittance of the final coating film, which is difficult to reach 92% or above. How to solve the above problems existing in the current TGIC curing system polyester resin is a research direction in the industry. Summary of the invention
[0003] In view of the above problems existing in the field of high-transparency powder coatings of the current TGIC curing system, the present invention provides a polyester resin for low-temperature curing high-transparency powder coatings, which is obtained by polymerization of triethanolamine, isobutyric acid, terephthalic acid, 2-ethyl-1,3-hexanediol, adipic acid, and propylene glycol triglycidyl ether. Through the design of the above scheme, the polyester resin molecules finally obtained have many advantages such as short linear segments, high branching degree, and low softening point of the product. They can be fully cured with TGIC curing agent at low temperatures, have a smooth surface, good impact resistance and gloss, and the cured coating has excellent leveling grade and light transmittance, which are much higher than ordinary polyester resins, thus having good performance.
[0004] A polyester resin for low temperature curing high transparency powder coating, the polyester resin comprising the following raw materials in molar parts:
[0005]
[0006] The raw materials also include esterification catalyst and antioxidant; the amount of esterification catalyst is 0.05-0.1% of the total mass of the raw materials; the amount of antioxidant is 0.3-0.5% of the total mass of the raw materials; the amount of low-temperature curing accelerator is 0.1-0.15% of the mass of triethanolamine.
[0007] Preferably, the esterification catalyst is tetrabutyl titanate; preferably, the antioxidant is antioxidant 1010, i.e. pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate; preferably, the low-temperature curing accelerator is triphenylethylphosphine chloride.
[0008] The method for preparing a polyester resin for low temperature curing and highly transparent powder coating as described above comprises the following steps:
[0009] A. Add the formulated amount of triethanolamine, isobutyric acid and esterification catalyst into a reaction kettle, and heat it to 130-140°C to perform high-temperature esterification dehydration reaction;
[0010] B. Take samples for testing. When the acid value of the esterified product reaches below 2 mgKOH / g, it indicates that the isobutyric acid grafting reaction has been completed. At this time, add the formulated amount of terephthalic acid, then gradually raise the temperature to 190-200°C and keep it warm for polymerization reaction;
[0011] C. Take samples for testing. When the acid value of the polymer reaches 40-50 mgKOH / g, add 2-ethyl-1,3-hexanediol and adipic acid, and heat to 215-220°C for polymerization reaction;
[0012] D. Take samples to test the acid value of the polymer. When the acid value of the polymer reaches 65-75 mgKOH / g, it indicates that the linear segment polymerization is basically completed. At this time, the temperature is lowered to 195-200°C, and trifunctional glycerol triglycidyl ether is added to carry out chain extension polymerization reaction;
[0013] E. Take samples to detect the acid value of the polymer. When the epoxy equivalent reaches 2120-2200 g / mol, it indicates that the three epoxy groups of glycerol triglycidyl ether have basically completed the chain extension reaction. Then add the formulated amount of antioxidant, start the vacuum system, and carry out vacuum polycondensation reaction.
[0014] F. Take samples to test the acid value of the polymer. When the acid value of the polymer reaches the expected value (25-32 mgKOH / g), stop the reaction, add the formulated amount of low-temperature curing accelerator, stir well, discharge the material while hot, cool the polyester resin, and then crush and granulate it to obtain the polyester resin.
[0015] The obtained product has the appearance of colorless and transparent particles, an acid value of 25-32 mgKOH / g, and a softening point of 93-102°C.
[0016] Preferably, in step B, the temperature is gradually increased to 190-200° C. at a heating rate of 15-18° C. / h.
[0017] Preferably, in step E, the vacuum degree is controlled at -0.096 MPa to -0.098 MPa.
[0018] Preferably, in step F, the polyester resin is cooled by a steel belt with condensed water.
[0019] The present invention also relates to the use of the polyester resin for low temperature curing high transparency powder coating as described above or the polyester resin for low temperature curing high transparency powder coating prepared by the preparation method as described above in a TGIC curing system.
[0020] The TGIC curing system, in addition to the polyester resin and TGIC prepared above, may also contain leveling agents, brighteners and other commonly used additives in the art. The coating preparation method is: according to the TGIC curing system powder coating formula, the materials are mixed, extruded, tableted and crushed by a twin-screw extruder, and then the tablets are crushed and sieved to form a powder coating. The powder coating is sprayed on the tinplate substrate after surface treatment by an electrostatic spray gun, and a certain film thickness (for example, about 50 μm) is obtained after curing to obtain a coating.
[0021] Beneficial effects:
[0022] The invention provides a polyester resin for low-temperature curing and highly transparent powder coating. The polyester resin is designed to be finally obtained by polymerization of triethanolamine, isobutyric acid, terephthalic acid, 2-ethyl-1,3-hexanediol, adipic acid and propylene glycol triglycidyl ether. The polyester resin molecules obtained above have short linear segments but high branching degree, and can achieve rapid curing. Since the molecular weight of the linear polyester resin is small, the transparency of the coating after curing with TGIC is relatively high, reaching more than 92%. At the same time, the isobutyrate-esterified triethanolamine is used to introduce the isobutyrate group into the linear segment, further improving the lubricity and leveling ability of the segment and reducing the softening point. The participation of 2-ethyl-1,3-hexanediol further improves the hydrophobicity of the segment and reduces the softening point of the polyester resin. The amino groups introduced into the segment by triethanolamine and the inert hydroxyl groups left in the segment after the ring-opening polymerization of propylene triglycidyl ether will increase the adhesion between the coating and the substrate. The terminal carboxyl group after the linear adipic acid end-capping has small steric hindrance and high activity. After the final coating is fully cured at a low temperature of 155°C / 15min, its leveling grade and transmittance are both high, and the conventional mechanical properties can also meet the application requirements.
[0023] The present invention has been described in detail above, but the above embodiments are only illustrative in nature and are not intended to limit the present invention. In addition, this article is not limited by any theory described in the above prior art or invention content or the following examples. DETAILED DESCRIPTION
[0024] The present invention is further described below in conjunction with examples. It should be noted that the following examples are provided for illustrative purposes only and do not constitute a limitation on the scope of protection claimed for the present invention.
[0025] Unless otherwise specified, the raw materials, reagents, methods, etc. used in the examples are conventional raw materials, reagents, methods in the art.
[0026] Preparation Example 1
[0027] A polyester resin for low temperature curing high transparency powder coating, the polyester resin comprising the following raw materials in molar parts:
[0028]
[0029] The catalyst for the esterification reaction is tetrabutyl titanate, and the amount used is 0.1% of the total mass of the raw materials;
[0030] The antioxidant is antioxidant 1010, and the dosage is 0.5% of the total weight of the raw materials;
[0031] The low temperature curing accelerator is triphenylethylphosphine chloride, and the dosage is 0.1% of the mass of triethanolamine.
[0032] The method for preparing a polyester resin for low temperature curing and highly transparent powder coating as described above comprises the following steps:
[0033] A. Add the formulated amount of triethanolamine, isobutyric acid and esterification reaction catalyst into a reaction kettle, and heat it to 130° C. to carry out high-temperature esterification dehydration reaction;
[0034] B. Take samples for testing. When the acid value of the esterified product reaches below 2 mgKOH / g, it indicates that the isobutyric acid grafting reaction has been completed. Then, add the formulated amount of terephthalic acid, and then gradually increase the temperature to 190°C at a heating rate of 15°C / h, and keep the temperature to allow polymerization reaction;
[0035] C. Take samples for testing. When the acid value of the polymer reaches 40-50 mgKOH / g, add 2-ethyl-1,3-hexanediol and adipic acid, and heat to 215°C for polymerization reaction;
[0036] D. Take samples to test the acid value of the polymer. When the acid value of the polymer reaches 65-75 mgKOH / g, it indicates that the linear segment polymerization is basically completed. At this time, the temperature is lowered to 195°C, and trifunctional glycerol triglycidyl ether is added to carry out chain extension polymerization reaction;
[0037] E. Take samples to detect the epoxy equivalent of the polymer. When the epoxy equivalent of the polymer reaches 2120-2200 g / mol, it indicates that the three epoxy groups of glycerol triglycidyl ether have basically completed the chain extension reaction. Then add the formulated amount of antioxidant, start the vacuum system, and carry out vacuum polycondensation reaction. The vacuum degree is controlled at -0.098 Mpa.
[0038] F. Take samples to test the acid value of the polymer. When the acid value of the polymer reaches 25-32 mgKOH / g, stop the reaction, add the formulated amount of low-temperature curing accelerator, stir well, discharge the material while hot, cool the polyester resin with a steel belt with condensed water, and then crush and granulate to obtain the polyester resin.
[0039] The obtained product has the appearance of colorless and transparent particles, an acid value of 26 mgKOH / g, and a softening point of 101°C.
[0040] Preparation Example 2
[0041] A polyester resin for low temperature curing high transparency powder coating, the polyester resin comprising the following raw materials in molar parts:
[0042]
[0043] The catalyst for the esterification reaction is tetrabutyl titanate, and the amount used is 0.1% of the total mass of the raw materials;
[0044] The antioxidant is antioxidant 1010, and the dosage is 0.5% of the total weight of the raw materials.
[0045] The low temperature curing accelerator is triphenylethylphosphine chloride, and the dosage is 0.15% of the mass of triethanolamine.
[0046] The preparation method is the same as Example 1.
[0047] The acid value of the obtained product is 28 mgKOH / g and the softening point is 98°C.
[0048] Preparation Example 3
[0049] A polyester resin for low temperature curing high transparency powder coating, the polyester resin comprising the following raw materials in molar parts:
[0050]
[0051] The catalyst for the esterification reaction is tetrabutyl titanate, and the amount used is 0.05% of the total mass of the raw materials;
[0052] The antioxidant is antioxidant 1010, and the dosage is 0.4% of the total weight of the raw materials.
[0053] The low temperature curing accelerator is triphenylethylphosphine chloride, and the dosage is 0.12% of the mass of triethanolamine.
[0054] The preparation method is the same as Example 1.
[0055] The acid value of the obtained product is 31 mgKOH / g and the softening point is 94°C.
[0056] Preparation Example 4
[0057] A polyester resin for low temperature curing high transparency powder coating, the polyester resin comprising the following raw materials in molar parts:
[0058]
[0059] The catalyst for the esterification reaction is tetrabutyl titanate, and the amount used is 0.08% of the total mass of the raw materials;
[0060] The antioxidant is antioxidant 1010, and the dosage is 0.4% of the total weight of the raw materials.
[0061] The low temperature curing accelerator is triphenylethylphosphine chloride, and the dosage is 0.13% of the mass of triethanolamine.
[0062] The preparation method is the same as Example 1.
[0063] The acid value of the obtained product is 29 mgKOH / g and the softening point is 95°C.
[0064] Comparative Preparation Example 1
[0065] Commercially available ordinary polyester resin for TGIC system, acid value: 35 mgKOH / g, softening point 118°C, model SJ4A, purchased from Anhui Shenjian New Materials Co., Ltd.
[0066] Comparative Preparation Example 2
[0067] The other conditions are the same as those in Comparative Example 1, except that the curing conditions are changed from 155°C / 12min to 200°C / 10min.
[0068] Examples 1-4 and Comparative Examples 1 and 2 (polyester resins are obtained by the above corresponding examples or comparative examples)
[0069] The formula of TGIC curing system transparent powder coating is as follows in parts by weight:
[0070]
[0071] The TGIC model is JF-77B, which comes from Huangshan Jinfeng Industrial Co., Ltd.; the leveling agent model is GLP503C, and the brightener model is BLC701, both of which come from Ningbo Nanhai Chemical Co., Ltd.
[0072] Preparation of coating: According to the above TGIC curing system transparent powder coating formula, all materials are mixed, extruded, tableted and crushed by a twin-screw extruder, and then the tablets are crushed and sieved (180-200 mesh) to make powder coating. The powder coating is sprayed on the surface treated tinplate substrate with an electrostatic spray gun, with a film thickness of about 50μm, and cured at 155℃ / 12min to obtain the coating.
[0073] The coating index test is based on GB / T 21776-2008 "Guide to the Testing Standards of Powder Coatings and Their Coatings"; the leveling performance adopts the PCI leveling grade, 1-10, the larger the number, the better the leveling.
[0074] Transmittance test: spray the transparent powder coating on a clean and transparent standard glass plate with residual heat, control the film thickness to about 50μm, and obtain a transparent coating film after curing at 155℃ / 12min. Test the transmittance of the standard glass plate after the sprayed transparent powder coating is cured. Compare the transmittance of the standard glass plate after the sprayed transparent powder coating is cured with the transmittance of the pure standard glass plate. Transmittance of transparent powder coating film = transmittance of test plate / transmittance of standard glass plate*100%.
[0075] Table 1 Performance tests of embodiments and comparative examples
[0076]
[0077]
[0078] As can be seen from Table 1, the polyester resin prepared by the product of the present invention using special raw materials and processes has the advantages of short linear segments and high branching degree. The product has a low softening point and high end group activity. It can be fully cured at 155°C / 15min with TGIC curing agent. The surface is flat and smooth, and the impact resistance and gloss are good. In particular, due to the short polymer chain segment, the cured coating film has excellent leveling grade and light transmittance, with the leveling grade reaching level 7 and the light transmittance being above 92%, which is much higher than the light transmittance of ordinary polyester resin after curing.
[0079] Since the comparative example 1 is not fully cured, its appearance, gloss and impact resistance are all poor; while the comparative example 2 can achieve full curing after the curing temperature is raised to 200°C, and the appearance, impact resistance and gloss of the cured coating film are relatively good, but the leveling property is average, with a leveling grade of 5, and the light transmittance of the coating film is also average, which can only reach 88.6%, which is lower than the polyester resin of the product of the present invention.
[0080] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents, without departing from the spirit and essence of the claims of the present invention; and these modifications or replacements are still within the scope defined by the claims of the present invention.
Claims
1. A polyester resin for low temperature curing and highly transparent powder coating, It is characterized in that The polyester resin comprises the following raw materials in molar proportions: The raw materials also include esterification catalyst, antioxidant and low temperature curing accelerator; the amount of esterification catalyst is 0.05-0.1% of the total mass of the raw materials; the amount of antioxidant is 0.3-0.5% of the total mass of the raw materials; the amount of low temperature curing accelerator is 0.1-0.15% of the mass of triethanolamine.
2. A polyester resin for low temperature curing and highly transparent powder coating as claimed in claim 1, further characterized in that the esterification reaction catalyst is tetrabutyl titanate.
3. A polyester resin for low temperature curing high transparency powder coating as claimed in claim 1, further characterized in that the antioxidant is antioxidant 1010; and the low temperature curing accelerator is triphenylethylphosphine chloride.
4. A method for preparing a polyester resin for low temperature curing and highly transparent powder coating according to any one of claims 1 to 3, It is characterized in that The following steps are involved: A. Add the formulated amount of triethanolamine, isobutyric acid and esterification catalyst into a reaction kettle, and heat it to 130-140°C to perform high-temperature esterification dehydration reaction; B. Take samples for testing. When the acid value of the esterified product reaches below 2 mgKOH / g, it indicates that the isobutyric acid grafting reaction has been completed. At this time, add the formulated amount of terephthalic acid, then gradually raise the temperature to 190-200°C and keep it warm for polymerization reaction; C. Take samples for testing. When the acid value of the polymer reaches 40-50 mgKOH / g, add 2-ethyl-1,3-hexanediol and adipic acid, and heat to 215-220°C for polymerization reaction; D. Take samples to test the acid value of the polymer. When the acid value of the polymer reaches 65-75 mgKOH / g, it indicates that the linear segment polymerization is basically completed. At this time, the temperature is lowered to 195-200°C, and trifunctional glycerol triglycidyl ether is added to carry out chain extension polymerization reaction; E. Take samples to detect the epoxy equivalent of the polymer. When the epoxy equivalent of the polymer reaches 2120-2200 g / mol, it indicates that the three epoxy groups of glycerol triglycidyl ether have basically completed the chain extension reaction; then add the formulated amount of antioxidant, start the vacuum system, and carry out vacuum polycondensation reaction; F. Take samples to test the acid value of the polymer. When the acid value of the polymer reaches 25-32 mgKOH / g, stop the reaction, add the formulated amount of low-temperature curing accelerator, stir well, discharge the material while hot, cool the polyester resin, and then crush and granulate it to obtain the polyester resin.
5. The method for preparing a polyester resin for low-temperature curing and highly transparent powder coating according to claim 4, further characterized in that in step B, the temperature is gradually increased to 190-200°C at a heating rate of 15-18°C / h.
6. The method for preparing a polyester resin for low-temperature curing and highly transparent powder coating according to claim 4, further characterized in that in step E, the vacuum degree is controlled at -0.096 MPa to -0.098 MPa.
7. The method for preparing a polyester resin for low-temperature curing and highly transparent powder coating according to claim 4, further characterized in that in step F, the polyester resin is cooled by a steel belt with condensed water.
8. Use of the polyester resin for low temperature curing and highly transparent powder coating according to any one of claims 1 to 3 or the polyester resin for low temperature curing and highly transparent powder coating prepared by the preparation method according to any one of claims 4 to 8 in a TGIC curing system.
Citation Information
Cited By
Low-temperature curing polyester resin powder coating and preparation method thereof
CN119955384A
Polyester resin for low-temperature curing powder coating as well as preparation method and application of polyester resin
CN121736245A