Flame retardant heat-insulating and sound-insulating coating and preparation method thereof
By modifying the cross-linking reaction of coral mucus with acrylic monomer and glutaraldehyde, combined with hollow glass microbeads and other materials, the problems of incompatibility and environmental risks of substrate and additives in the prior art are solved, and high-performance Flame-retardant thermal insulation coating improves the durability and sound insulation performance of the coating.
Patent Information
- Application Number
- CN202411225829.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-03
AI Technical Summary
The physical and chemical incompatibility of substrates and functional additives in existing flame retardant insulation coatings leads to insufficient adhesion, easy layering, cracking and poor durability. Traditional acrylic emulsions may release harmful gases during combustion, which poses environmental risks. .
Modified coral mucus is used as the substrate, and a cross-linking network is formed by reaction with acrylic monomer and glutaraldehyde to enhance the film formation and mechanical strength of the coating. At the same time, hollow glass microbeads, talc powder, and aluminum hydroxide are added. and other materials to form high-performance flame retardant, thermal insulation coatings.
It significantly improves the wear resistance, impact resistance, flame retardant effect and sound insulation properties of the coating, extends the service life, reduces the possibility of cracking and peeling of the coating, and effectively prevents oxygen and heat transfer at high temperatures, reducing heat conduction Coefficient improves the insulation effect.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the field of coating materials, and in particular relates to a flame retardant, heat-insulating and sound-insulating coating and a preparation method thereof. Background Art
[0002] With the continuous development of modern construction technology, the performance requirements of building materials are getting higher and higher. Not only do they need to have basic structural strength and durability, but they also need to meet multiple requirements such as fire prevention, safety, thermal insulation, sound insulation and environmental protection. The flame-retardant, thermal insulation and sound insulation coatings currently on the market usually use water-based acrylic emulsions as the base material, supplemented by various functional additives (such as flame retardants, thermal insulation materials and sound insulation materials) to achieve the goal of multifunctional coatings. However, the physical and chemical incompatibility between the base material and these functional additives in the existing coating system leads to a series of defects in the coating in practical applications, such as insufficient adhesion, easy delamination, cracking, poor durability and other problems.
[0003] The core problem of existing flame-retardant, thermal insulation and sound insulation coatings lies in the poor compatibility between the base emulsion and the functional additives. Although water-based acrylic emulsions have good film-forming properties and mechanical strength, when combined with flame retardants, thermal insulation and sound insulation materials, due to the differences in the physical and chemical properties of the components, problems such as material delamination, coating cracking and insufficient adhesion are prone to occur, especially in long-term use or in extreme environments. The performance of the coating deteriorates more significantly. In addition, some flame retardants may release harmful gases during the combustion process when combined with acrylic emulsions, posing certain environmental risks. In addition, organic coatings are prone to release harmful gases, which are harmful to human health and are not suitable for the needs of interior decoration.
[0004] Coral mucus is a natural biomaterial that comes from nature and does not contain harmful chemicals. This makes it significantly environmentally friendly and meets the requirements of green buildings and sustainable development. Due to its natural ingredients, coral mucus is relatively safe for human health during application and is suitable for indoor environments with high health requirements, such as hospitals and schools. In addition, coral mucus itself has strong adhesion and can provide good adhesion when applied, making it easy to combine with the surface of the substrate and reduce the possibility of peeling or falling off. Coral mucus also contains a variety of active ingredients with antibacterial and antioxidant effects, which can inhibit the growth of microorganisms and reduce the growth of mold or bacteria on the coating surface.
[0005] Although modified coral mucus has shown superiority in solving the compatibility problem between basic emulsion and functional additives, it still faces some technical challenges: the chemical composition of coral mucus is mainly composed of organic substances such as polysaccharides and proteins, which usually do not have the ability to form high-strength and durable coatings. Due to its natural organic composition, it is easily affected by the environment, such as humidity, high temperature or microbial invasion, which leads to the degradation of the coating. Summary of the invention
[0006] In view of the deficiencies in the prior art, the present invention provides a flame retardant, heat-insulating and sound-insulating coating and a preparation method thereof.
[0007] The present invention provides a flame retardant heat-insulating and sound-insulating coating, which is composed of the following components in parts by mass:
[0008] 50-60 parts modified coral mucus;
[0009] 10-15 parts of hollow glass microspheres;
[0010] 10-20 parts of talcum powder;
[0011] 3-5 parts of titanium dioxide;
[0012] 5-10 parts of aluminum hydroxide;
[0013] 0.5-1 part dispersant;
[0014] 0.2-0.5 parts of defoamer;
[0015] 0.3-0.7 parts thickener.
[0016] The dispersant is at least one of sodium polyacrylate, polycarboxylate and sulfonate.
[0017] The defoamer is at least one of an organosilicon defoamer, a polyether-modified siloxane defoamer and a mineral oil defoamer.
[0018] The thickener is at least one of hydroxyethyl cellulose, xanthan gum and acrylic thickener.
[0019] The method for preparing the modified coral mucus comprises the following steps:
[0020] S1: Mix coral mucus and acrylate monomer at room temperature, wherein the amount of acrylate monomer added is 10-30% of the mass of coral mucus, and stir at a speed of 300-500 r / min for 30-60 minutes to obtain a precursor solution;
[0021] S2. Add an initiator to the precursor solution obtained in step S1, wherein the amount of the initiator added is 0.5-2% of the mass of the acrylic acid monomer, stir and react at 40-50°C for 30-40 minutes, then gradually increase the temperature to 70°C at a rate of 5°C per 10 minutes and react at this temperature for 3 hours to obtain an acrylic acid / coral mucus polymer;
[0022] S3 cools the acrylic acid / coral mucus polymer obtained in step S2 to 40-50° C. at a rate of 3-6° C. per 8-12 min, adds a cross-linking agent in an amount of 1-5% by weight of the coral mucus, and reacts by stirring for 1-2 hours to obtain a cross-linked acrylic acid / coral mucus polymer;
[0023] S4: cooling the cross-linked acrylic acid / coral mucus polymer obtained in step S3 to room temperature, filtering it through a filter with a pore size of 0.5-1 micron, and drying the filtrate at 40-50° C. and 100-200 Pa pressure for 4-6 hours to obtain the modified coral mucus.
[0024] Step S1: The method for preparing the coral mucus comprises the following steps: taking a piece of living giant syngenea coral, using a 1 kg weight to fall freely from 25 cm above the living giant syngenea coral twice to stimulate the living giant syngenea coral, and then immersing the stimulated living giant syngenea coral in seawater for 80 minutes, and finally taking out and inverting to collect mucus, mixing the obtained mucus and activated carbon particles in a mass ratio of 1:0.05, stirring at a speed of 120 r / min for 8 minutes, and centrifuging to separate the activated carbon to obtain the coral mucus.
[0025] In step S1, the acrylic monomer is at least one of methyl acrylate, ethyl acrylate and butyl acrylate; preferably, the acrylic monomer is a mixture of methyl acrylate, ethyl acrylate and butyl acrylate in a mass ratio of 1:(2-3):(1-2).
[0026] The initiator in step S2 is at least one of ammonium persulfate and azobisisobutyronitrile.
[0027] In step S3, the cross-linking agent is at least one of glutaraldehyde, glutaric anhydride and chitosan; preferably, the cross-linking agent is glutaraldehyde.
[0028] The present invention also provides a method for preparing a flame retardant, heat-insulating and sound-insulating coating, comprising the following steps:
[0029] By mass, 50-60 parts of modified coral mucus, 10-15 parts of hollow glass microspheres, 10-20 parts of talcum powder, 3-5 parts of titanium dioxide, 5-10 parts of aluminum hydroxide, 0.5-1 part of dispersant, 0.2-0.5 part of defoamer, and 0.3-0.7 part of thickener are mixed and stirred evenly to obtain the flame retardant, thermal insulation and sound insulation coating.
[0030] Although traditional acrylic emulsions have excellent film-forming properties, they may produce volatile organic compounds (VOCs) during their production and decomposition, which have certain negative effects on the environment and health. In contrast, coral mucus is a natural biomaterial with excellent environmental performance, low toxicity and biodegradability. In addition, coral mucus contains natural antibacterial and anti-mildew ingredients, which makes the coating have certain antibacterial and anti-mildew functions in application, helping to extend the service life of the coating.
[0031] Therefore, the present invention attempts to replace the traditional acrylic emulsion with coral mucus, but the chemical composition of coral mucus is mainly composed of organic substances such as polysaccharides and proteins, and its film-forming properties and mechanical properties are poorer than those of acrylic emulsion. Therefore, the present invention adopts acrylic acid modification to make coral mucus have the film-forming property of acrylic acid, and can form a tougher and denser coating film, thereby improving the wear resistance and impact resistance of the coating. In addition, acrylic acid modification also improves the surface hardness of the coating and enhances its resistance to physical damage. Further, a three-dimensional cross-linked network is formed by cross-linking with glutaraldehyde, further improving the mechanical strength and durability of the coating. The cross-linked structure allows the coating to remain stable during long-term use, reducing the possibility of cracking, peeling and deformation. The cross-linked structure forms a stable carbonized layer at high temperature, and can also effectively prevent the transfer of oxygen and heat, delaying the combustion process. Acrylic acid modification also helps to form a more stable coating, showing better fire resistance and flame retardant effect in fire.
[0032] In addition, acrylic modification gives the coating a denser structure, effectively blocking the propagation of sound. Glutaraldehyde cross-linking further enhances the structural stability and density of the coating, making it more difficult for sound waves to pass through the coating, significantly improving the sound insulation performance. Modified coral mucus combined with insulating materials such as hollow glass microspheres forms a coating with low thermal conductivity. Glutaraldehyde cross-linking increases the density of the coating and reduces the heat conduction path, thereby further reducing the thermal conductivity of the coating and improving the insulation effect.
[0033] Beneficial effects of the present invention:
[0034] The present invention replaces the traditional acrylic emulsion with more environmentally friendly and healthy coral mucus, modifies the coral mucus with acrylic acid, and cross-links the modified coral mucus with glutaraldehyde, thereby greatly improving the film-forming property and mechanical strength of the coral mucus, and further improving its flame retardant, sound insulation and heat insulation properties. After adding hollow glass microspheres, titanium dioxide and aluminum hydroxide, a flame retardant, heat-insulating and sound-insulating coating with excellent performance is obtained. DETAILED DESCRIPTION
[0035] The coral mucus used in Examples 1-5 and Comparative Examples 1 and 3 of the present invention is extracted from giant syngenesium in the Qiongzhou Strait area of the South China Sea, Guangdong Province; the preparation method of the coral mucus comprises the following steps: taking a piece of living giant syngenesium, using a 1 kg weight to fall freely from 25 cm above the living giant syngenesium twice to stimulate the living giant syngenesium, and then immersing the stimulated living giant syngenesium in seawater for 80 minutes, and finally taking out and inverting to collect mucus, mixing the obtained mucus and activated carbon particles in a mass ratio of 1:0.05, stirring at a speed of 120 r / min for 8 minutes, and centrifuging to separate the activated carbon to obtain the coral mucus.
[0036] Hollow glass microspheres, item number: 003, Lingshou County Fuda Mineral Products Processing Factory.
[0037] Talc, item number: 03, Lingshou County Huizi Mineral Products Co., Ltd.
[0038] Titanium dioxide, product number: 01, Jinan Mingliang Chemical Co., Ltd.
[0039] Aluminum hydroxide, product number: 01, Guangzhou Changyu Chemical Co., Ltd.
[0040] Sodium polyacrylate, model: AG-22, Guangdong Zhongtai Lianhua New Materials Co., Ltd.
[0041] Polydimethylsiloxane, product number: 10-1, Shandong Xinfeng Chemical Co., Ltd.
[0042] Hydroxyethyl cellulose, model: LH55RR, Shandong Yousuo Chemical Technology Co., Ltd.
[0043] Example 1
[0044] A flame retardant heat-insulating and sound-insulating coating, comprising the following components in parts by mass:
[0045] 55 parts modified coral mucus;
[0046] 10 parts of hollow glass microspheres;
[0047] 15 parts talcum powder;
[0048] 4 parts titanium dioxide;
[0049] 6 parts of aluminum hydroxide;
[0050] 0.8 parts of dispersant;
[0051] 0.3 parts of defoamer;
[0052] 0.6 parts thickener.
[0053] The dispersant is sodium polyacrylate.
[0054] The defoamer is polydimethylsiloxane in the organosilicon defoamer.
[0055] The thickener is hydroxyethyl cellulose.
[0056] The method for preparing the modified coral mucus comprises the following steps:
[0057] S1: coral mucus and acrylate monomer were mixed at room temperature, the amount of acrylate monomer added was 20% of the mass of coral mucus, and stirred at 400 r / min for 40 minutes to obtain a precursor solution;
[0058] S2. Add an initiator to the precursor solution obtained in step S1, wherein the amount of the initiator added is 1% of the mass of the acrylic acid monomer, and react at 50°C with stirring for 30 minutes, and then gradually increase the temperature to 70°C at a rate of 5°C per 10 minutes and react at a constant temperature for 3 hours to obtain an acrylic acid / coral mucus polymer;
[0059] S3 cools the acrylic acid / coral mucus polymer obtained in step S2 to 50° C. at a rate of 5° C. per 10 minutes, adds a cross-linking agent in an amount of 3% by weight of the coral mucus, and reacts by stirring for 1.5 hours to obtain a cross-linked acrylic acid / coral mucus polymer;
[0060] S4: Cool the cross-linked acrylic acid / coral mucus polymer obtained in step S3 to room temperature, filter it through a filter with a pore size of 0.5 microns, and dry the filtrate at 40° C. and 180 Pa pressure for 5 hours to obtain the modified coral mucus.
[0061] The acrylic acid monomer in step S1 is prepared by mixing methyl acrylate, ethyl acrylate and butyl acrylate in a mass ratio of 1:2:1.
[0062] The initiator in step S2 is ammonium persulfate.
[0063] The cross-linking agent in step S3 is glutaraldehyde.
[0064] The method for preparing the flame retardant, heat-insulating and sound-insulating coating comprises the following steps:
[0065] By mass, 55 parts of modified coral mucus, 10 parts of hollow glass microspheres, 15 parts of talcum powder, 4 parts of titanium dioxide, 6 parts of aluminum hydroxide, 0.8 parts of dispersant, 0.3 parts of defoaming agent and 0.6 parts of thickener are mixed and stirred uniformly to obtain the flame retardant, thermal insulation and sound insulation coating.
[0066] Example 2
[0067] A flame retardant heat-insulating and sound-insulating coating, comprising the following components in parts by mass:
[0068] 55 parts modified coral mucus;
[0069] 10 parts of hollow glass microspheres;
[0070] 15 parts talcum powder;
[0071] 4 parts titanium dioxide;
[0072] 6 parts of aluminum hydroxide;
[0073] 0.8 parts of dispersant;
[0074] 0.3 parts of defoamer;
[0075] 0.6 parts thickener.
[0076] The dispersant is sodium polyacrylate.
[0077] The defoamer is polydimethylsiloxane in the organosilicon defoamer.
[0078] The thickener is hydroxyethyl cellulose.
[0079] The method for preparing the modified coral mucus comprises the following steps:
[0080] S1: coral mucus and acrylate monomer were mixed at room temperature, the amount of acrylate monomer added was 20% of the mass of coral mucus, and stirred at 400 r / min for 40 minutes to obtain a precursor solution;
[0081] S2. Add an initiator to the precursor solution obtained in step S1, wherein the amount of the initiator added is 1% of the mass of the acrylic acid monomer, and react at 50°C with stirring for 30 minutes, and then gradually increase the temperature to 70°C at a rate of 5°C per 10 minutes and react at a constant temperature for 3 hours to obtain an acrylic acid / coral mucus polymer;
[0082] S3: Cooling the acrylic acid / coral mucus polymer obtained in step S2 to room temperature, filtering it through a filter with a pore size of 0.5 micrometers, and drying the filtrate at 40° C. and 180 Pa pressure for 5 hours to obtain the modified coral mucus.
[0083] The acrylic acid monomer in step S1 is prepared by mixing methyl acrylate, ethyl acrylate and butyl acrylate in a mass ratio of 1:2:1.
[0084] The initiator in step S2 is ammonium persulfate.
[0085] The method for preparing the flame retardant, heat-insulating and sound-insulating coating comprises the following steps:
[0086] By mass, 55 parts of modified coral mucus, 10 parts of hollow glass microspheres, 15 parts of talcum powder, 4 parts of titanium dioxide, 6 parts of aluminum hydroxide, 0.8 parts of dispersant, 0.3 parts of defoaming agent and 0.6 parts of thickener are mixed and stirred uniformly to obtain the flame retardant, thermal insulation and sound insulation coating.
[0087] Example 3
[0088] A flame retardant heat-insulating and sound-insulating coating, comprising the following components in parts by mass:
[0089] 55 parts modified coral mucus;
[0090] 10 parts of hollow glass microspheres;
[0091] 15 parts talcum powder;
[0092] 4 parts titanium dioxide;
[0093] 6 parts of aluminum hydroxide;
[0094] 0.8 parts of dispersant;
[0095] 0.3 parts of defoamer;
[0096] 0.6 parts thickener.
[0097] The dispersant is sodium polyacrylate.
[0098] The defoamer is polydimethylsiloxane in the organosilicon defoamer.
[0099] The thickener is hydroxyethyl cellulose.
[0100] The method for preparing the modified coral mucus comprises the following steps:
[0101] S1: coral mucus and acrylate monomer were mixed at room temperature, the amount of acrylate monomer added was 20% of the mass of coral mucus, and stirred at 400 r / min for 40 minutes to obtain a precursor solution;
[0102] S2. Add an initiator to the precursor solution obtained in step S1, wherein the amount of the initiator added is 1% of the mass of the acrylic acid monomer, and react at 50°C with stirring for 30 minutes, and then gradually increase the temperature to 70°C at a rate of 5°C per 10 minutes and react at a constant temperature for 3 hours to obtain an acrylic acid / coral mucus polymer;
[0103] S3 cools the acrylic acid / coral mucus polymer obtained in step S2 to 50° C. at a rate of 5° C. per 10 minutes, adds a cross-linking agent in an amount of 3% by weight of the coral mucus, and reacts by stirring for 1.5 hours to obtain a cross-linked acrylic acid / coral mucus polymer;
[0104] S4: Cool the cross-linked acrylic acid / coral mucus polymer obtained in step S3 to room temperature, filter it through a filter with a pore size of 0.5 microns, and dry the filtrate at 40° C. and 180 Pa pressure for 5 hours to obtain the modified coral mucus.
[0105] The acrylic acid monomer in step S1 is methyl acrylate.
[0106] The initiator in step S2 is ammonium persulfate.
[0107] The cross-linking agent in step S3 is glutaraldehyde.
[0108] The method for preparing the flame retardant, heat-insulating and sound-insulating coating comprises the following steps:
[0109] By mass, 55 parts of modified coral mucus, 10 parts of hollow glass microspheres, 15 parts of talcum powder, 4 parts of titanium dioxide, 6 parts of aluminum hydroxide, 0.8 parts of dispersant, 0.3 parts of defoaming agent and 0.6 parts of thickener are mixed and stirred uniformly to obtain the flame retardant, thermal insulation and sound insulation coating.
[0110] Example 4
[0111] A flame retardant heat-insulating and sound-insulating coating, comprising the following components in parts by mass:
[0112] 55 parts modified coral mucus;
[0113] 10 parts of hollow glass microspheres;
[0114] 15 parts talcum powder;
[0115] 4 parts titanium dioxide;
[0116] 6 parts of aluminum hydroxide;
[0117] 0.8 parts of dispersant;
[0118] 0.3 parts of defoamer;
[0119] 0.6 parts thickener.
[0120] The dispersant is sodium polyacrylate.
[0121] The defoamer is polydimethylsiloxane in the organosilicon defoamer.
[0122] The thickener is hydroxyethyl cellulose.
[0123] The method for preparing the modified coral mucus comprises the following steps:
[0124] S1: coral mucus and acrylate monomer were mixed at room temperature, the amount of acrylate monomer added was 20% of the mass of coral mucus, and stirred at 400 r / min for 40 minutes to obtain a precursor solution;
[0125] S2. Add an initiator to the precursor solution obtained in step S1, wherein the amount of the initiator added is 1% of the mass of the acrylic acid monomer, and react at 50°C with stirring for 30 minutes, and then gradually increase the temperature to 70°C at a rate of 5°C per 10 minutes and react at a constant temperature for 3 hours to obtain an acrylic acid / coral mucus polymer;
[0126] S3 cools the acrylic acid / coral mucus polymer obtained in step S2 to 50° C. at a rate of 5° C. per 10 minutes, adds a cross-linking agent in an amount of 3% by weight of the coral mucus, and reacts by stirring for 1.5 hours to obtain a cross-linked acrylic acid / coral mucus polymer;
[0127] S4: Cool the cross-linked acrylic acid / coral mucus polymer obtained in step S3 to room temperature, filter it through a filter with a pore size of 0.5 microns, and dry the filtrate at 40° C. and 180 Pa pressure for 5 hours to obtain the modified coral mucus.
[0128] The acrylic acid monomer in step S1 is ethyl acrylate.
[0129] The initiator in step S2 is ammonium persulfate.
[0130] The cross-linking agent in step S3 is glutaraldehyde.
[0131] The method for preparing the flame retardant, heat-insulating and sound-insulating coating comprises the following steps:
[0132] By mass, 55 parts of modified coral mucus, 10 parts of hollow glass microspheres, 15 parts of talcum powder, 4 parts of titanium dioxide, 6 parts of aluminum hydroxide, 0.8 parts of dispersant, 0.3 parts of defoaming agent and 0.6 parts of thickener are mixed and stirred uniformly to obtain the flame retardant, thermal insulation and sound insulation coating.
[0133] Example 5
[0134] A flame retardant heat-insulating and sound-insulating coating, comprising the following components in parts by mass:
[0135] 55 parts modified coral mucus;
[0136] 10 parts of hollow glass microspheres;
[0137] 15 parts talcum powder;
[0138] 4 parts titanium dioxide;
[0139] 6 parts of aluminum hydroxide;
[0140] 0.8 parts of dispersant;
[0141] 0.3 parts of defoamer;
[0142] 0.6 parts thickener.
[0143] The dispersant is sodium polyacrylate.
[0144] The defoamer is polydimethylsiloxane in the organosilicon defoamer.
[0145] The thickener is hydroxyethyl cellulose.
[0146] The method for preparing the modified coral mucus comprises the following steps:
[0147] S1: coral mucus and acrylate monomer were mixed at room temperature, the amount of acrylate monomer added was 20% of the mass of coral mucus, and stirred at 400 r / min for 40 minutes to obtain a precursor solution;
[0148] S2. Add an initiator to the precursor solution obtained in step S1, wherein the amount of the initiator added is 1% of the mass of the acrylic acid monomer, and react at 50°C with stirring for 30 minutes, and then gradually increase the temperature to 70°C at a rate of 5°C per 10 minutes and react at a constant temperature for 3 hours to obtain an acrylic acid / coral mucus polymer;
[0149] S3 cools the acrylic acid / coral mucus polymer obtained in step S2 to 50° C. at a rate of 5° C. per 10 minutes, adds a cross-linking agent in an amount of 3% by weight of the coral mucus, and reacts by stirring for 1.5 hours to obtain a cross-linked acrylic acid / coral mucus polymer;
[0150] S4: Cool the cross-linked acrylic acid / coral mucus polymer obtained in step S3 to room temperature, filter it through a filter with a pore size of 0.5 microns, and dry the filtrate at 40° C. and 180 Pa pressure for 5 hours to obtain the modified coral mucus.
[0151] The acrylic acid monomer in step S1 is butyl acrylate.
[0152] The initiator in step S2 is ammonium persulfate.
[0153] The cross-linking agent in step S3 is glutaraldehyde.
[0154] The method for preparing the flame retardant, heat-insulating and sound-insulating coating comprises the following steps:
[0155] By mass, 55 parts of modified coral mucus, 10 parts of hollow glass microspheres, 15 parts of talcum powder, 4 parts of titanium dioxide, 6 parts of aluminum hydroxide, 0.8 parts of dispersant, 0.3 parts of defoaming agent and 0.6 parts of thickener are mixed and stirred uniformly to obtain the flame retardant, thermal insulation and sound insulation coating.
[0156] Comparative Example 1
[0157] A flame retardant heat-insulating and sound-insulating coating, comprising the following components in parts by mass:
[0158] 55 parts coral mucus;
[0159] 10 parts of hollow glass microspheres;
[0160] 15 parts talcum powder;
[0161] 4 parts titanium dioxide;
[0162] 6 parts of aluminum hydroxide;
[0163] 0.8 parts of dispersant;
[0164] 0.3 parts of defoamer;
[0165] 0.6 parts thickener.
[0166] The dispersant is sodium polyacrylate.
[0167] The defoamer is polydimethylsiloxane in the organosilicon defoamer.
[0168] The thickener is hydroxyethyl cellulose.
[0169] The method for preparing the flame retardant, heat-insulating and sound-insulating coating comprises the following steps:
[0170] By mass, 55 parts of coral mucus, 10 parts of hollow glass microspheres, 15 parts of talcum powder, 4 parts of titanium dioxide, 6 parts of aluminum hydroxide, 0.8 parts of dispersant, 0.3 parts of defoaming agent and 0.6 parts of thickener are mixed and stirred evenly to obtain the flame retardant, thermal insulation and sound insulation coating.
[0171] Comparative Example 2
[0172] A flame retardant heat-insulating and sound-insulating coating, comprising the following components in parts by mass:
[0173] 55 parts of acrylic emulsion;
[0174] 10 parts of hollow glass microspheres;
[0175] 15 parts talcum powder;
[0176] 4 parts titanium dioxide;
[0177] 6 parts of aluminum hydroxide;
[0178] 0.8 parts of dispersant;
[0179] 0.3 parts of defoamer;
[0180] 0.6 parts thickener.
[0181] The dispersant is sodium polyacrylate.
[0182] The defoamer is polydimethylsiloxane in the organosilicon defoamer.
[0183] The thickener is hydroxyethyl cellulose.
[0184] The acrylic emulsion is an acrylic emulsion stock solution with the brand number E0503 produced by Shenzhen Jitian Chemical Co., Ltd.
[0185] The method for preparing the flame retardant, heat-insulating and sound-insulating coating comprises the following steps:
[0186] By mass, 55 parts of acrylic emulsion, 10 parts of hollow glass microspheres, 15 parts of talcum powder, 4 parts of titanium dioxide, 6 parts of aluminum hydroxide, 0.8 parts of dispersant, 0.3 parts of defoaming agent and 0.6 parts of thickener are mixed and stirred uniformly to obtain the flame retardant thermal insulation and sound insulation coating.
[0187] Comparative Example 3
[0188] A flame retardant heat-insulating and sound-insulating coating, comprising the following components in parts by mass:
[0189] 55 parts modified coral mucus;
[0190] 10 parts of hollow glass microspheres;
[0191] 15 parts talcum powder;
[0192] 4 parts titanium dioxide;
[0193] 6 parts of aluminum hydroxide;
[0194] 0.8 parts of dispersant;
[0195] 0.3 parts of defoamer;
[0196] 0.6 parts thickener.
[0197] The dispersant is sodium polyacrylate.
[0198] The defoamer is polydimethylsiloxane in the organosilicon defoamer.
[0199] The thickener is hydroxyethyl cellulose.
[0200] The method for preparing the modified coral mucus comprises the following steps:
[0201] S1: coral mucus and acrylate monomer were mixed at room temperature, the amount of acrylate monomer added was 20% of the mass of coral mucus, and stirred at 400 r / min for 40 minutes to obtain a precursor solution;
[0202] S2. Add an initiator to the precursor solution obtained in step S1, wherein the amount of the initiator added is 1% of the mass of the acrylic acid monomer, and stir the reaction at 50°C for 30 minutes, then gradually increase the temperature to 70°C at a rate of 5°C per minute and react at this temperature for 3 hours to obtain an acrylic acid / coral mucus polymer;
[0203] S3 cools the acrylic acid / coral mucus polymer obtained in step S2 to 50° C. at a rate of 5° C. per 10 minutes, adds a cross-linking agent in an amount of 3% by weight of the coral mucus, and reacts by stirring for 1.5 hours to obtain a cross-linked acrylic acid / coral mucus polymer;
[0204] S4: Cool the cross-linked acrylic acid / coral mucus polymer obtained in step S3 to room temperature, filter it through a filter with a pore size of 0.5 microns, and dry the filtrate at 40° C. and 180 Pa pressure for 5 hours to obtain the modified coral mucus.
[0205] The acrylic acid monomer in step S1 is prepared by mixing methyl acrylate, ethyl acrylate and butyl acrylate in a mass ratio of 1:2:1.
[0206] The initiator in step S2 is ammonium persulfate.
[0207] The cross-linking agent in step S3 is glutaraldehyde.
[0208] The method for preparing the flame retardant, heat-insulating and sound-insulating coating comprises the following steps:
[0209] By mass, 55 parts of modified coral mucus, 10 parts of hollow glass microspheres, 15 parts of talcum powder, 4 parts of titanium dioxide, 6 parts of aluminum hydroxide, 0.8 parts of dispersant, 0.3 parts of defoaming agent and 0.6 parts of thickener are mixed and stirred uniformly to obtain the flame retardant, thermal insulation and sound insulation coating.
[0210] Test Example 1
[0211] The sound insulation performance of the flame retardant, thermal insulation and sound insulation coatings prepared in each embodiment and comparative example was tested according to GB / T 50121-2005 "Building Sound Insulation Evaluation Standard". The test object was: 9mm thick gypsum wallboard plus 3mm thick flame retardant, thermal insulation and sound insulation coatings prepared in each embodiment and comparative example. The results are shown in Table 1.
[0212] Table 1: Sound insulation test results
[0213]
[0214] Test Example 2
[0215] Thermal insulation performance test: The thermal conductivity was measured in accordance with GB / T 10295-2008 “Determination of steady-state thermal resistance and related properties of thermal insulation materials – heat flow meter method”. The results are shown in Table 2.
[0216] Table 2: Thermal insulation performance test results
[0217]
[0218] Test Example 3
[0219] Adhesion test: refer to GB / T5210-2006 standard for pull-off test, coating thickness is 1mm, the results are shown in Table 3.
[0220] Table 3: Adhesion
[0221]
[0222] It can be seen from Table 1, Table 2 and Table 3 that Examples 1-5 all have good sound insulation, heat insulation and adhesion, and the flame retardant heat insulation and sound insulation coating prepared in Example 1 has the best performance. Example 2 does not use glutaraldehyde for cross-linking, and its performance is significantly lower than that of Example 1, which shows that the cross-linking reaction has a significant improvement in the sound insulation, heat insulation and adhesion performance of coral mucus. Examples 3-5 use methyl acrylate, ethyl acrylate and butyl acrylate as modified monomers, respectively, and their effects are slightly lower than those of Example 1, which shows that the structure of the acrylic monomer also has a certain influence on the performance of the modified coral mucus. Comparison with Comparative Examples 1 and 2 can further show that compared with unmodified coral mucus and traditional acrylic emulsion, the modified coral mucus has significantly improved performance and has a more obvious advantage. Comparison with Comparative Example 3 shows that in the modification scheme of the present invention, the heating rate has a greater influence on the reaction process of acrylic monomer and coral mucus. A faster heating process is not conducive to the reaction of acrylic monomer and coral mucus, and generates a substance with higher sound insulation, heat insulation and excellent adhesion.
Claims
1. A flame retardant, heat-insulating and sound-insulating coating, characterized in that: By mass, it is composed of the following components: 50-60 parts modified coral mucus; 10-15 parts of hollow glass microspheres; 10-20 parts of talcum powder; 3-5 parts of titanium dioxide; 5-10 parts of aluminum hydroxide; 0.5-1 part dispersant; 0.2-0.5 parts of defoamer; 0.3-0.7 parts thickener; The method for preparing the modified coral mucus comprises the following steps: S1: Mix coral mucus with acrylate monomer at room temperature, wherein the amount of acrylate monomer added is 10-30% of the mass of coral mucus, and stir at 300-500 r / min for 30-60 min to obtain a precursor solution; S2. Add an initiator to the precursor solution obtained in step S1, wherein the amount of the initiator added is 0.5-2% of the mass of the acrylic acid monomer, stir and react at 40-50°C for 30-40 minutes, then gradually increase the temperature to 70°C at a rate of 5°C per 10 minutes and react at this temperature for 3 hours to obtain an acrylic acid / coral mucus polymer; S3 cools the acrylic acid / coral mucus polymer obtained in step S2 to 40-50° C. at a rate of 3-6° C. per 8-12 min, adds a cross-linking agent in an amount of 1-5% by weight of the coral mucus, and reacts by stirring for 1-2 hours to obtain a cross-linked acrylic acid / coral mucus polymer; S4: cooling the cross-linked acrylic acid / coral mucus polymer obtained in step S3 to room temperature, filtering it through a filter with a pore size of 0.5-1 micron, and drying the filtrate at 40-50° C. and 100-200 Pa pressure for 4-6 hours to obtain the modified coral mucus; Step S1: The method for preparing the coral mucus comprises the following steps: taking a piece of living giant syngenesium, using a 1 kg weight to fall freely from 25 cm above the living giant syngenesium twice to stimulate the living giant syngenesium, and then immersing the stimulated living giant syngenesium in seawater for 80 minutes, and finally taking out and inverting to collect mucus, mixing the obtained mucus and activated carbon particles at a mass ratio of 1:0.05, stirring at a speed of 120 r / min for 8 minutes, and centrifuging to separate the activated carbon to obtain the coral mucus; The acrylic monomer in step S1 is at least one of methyl acrylate, ethyl acrylate and butyl acrylate.
2. The flame retardant, heat-insulating and sound-insulating coating according to claim 1, characterized in that: The dispersant is at least one of sodium polyacrylate, polycarboxylate and sulfonate.
3. The flame retardant, heat-insulating and sound-insulating coating according to claim 1, characterized in that: The defoamer is at least one of an organosilicon defoamer, a polyether-modified siloxane defoamer and a mineral oil defoamer.
4. The flame retardant, heat-insulating and sound-insulating coating according to claim 1, characterized in that: The thickener is at least one of hydroxyethyl cellulose, xanthan gum and acrylic thickener.
5. The flame retardant, heat-insulating and sound-insulating coating according to claim 1, characterized in that: The initiator in step S2 is at least one of ammonium persulfate and azobisisobutyronitrile.
6. The flame retardant, heat-insulating and sound-insulating coating according to claim 1, characterized in that: In step S3, the cross-linking agent is at least one of glutaraldehyde, glutaric anhydride and chitosan.
7. A method for preparing the flame retardant, heat-insulating and sound-insulating coating according to any one of claims 1 to 6, characterized in that: The following steps are involved: By mass, 50-60 parts of modified coral mucus, 10-15 parts of hollow glass microspheres, 10-20 parts of talcum powder, 3-5 parts of titanium dioxide, 5-10 parts of aluminum hydroxide, 0.5-1 part of dispersant, 0.2-0.5 part of defoamer, and 0.3-0.7 part of thickener are mixed and stirred evenly to obtain the flame retardant, thermal insulation and sound insulation coating.