Colorful or patterned mobile phone shell capable of reducing radiation and preparation method thereof
The base body of the mobile phone case is surface treated through anodizing and molten salt electrochemical methods to form an amorphous metal oxide layer, which solves the problems of cumbersome processes and lack of radiation protection in the existing technology, and achieves the dual effects of color and radiation protection. .
Patent Information
- Application Number
- CN202410565814.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-24
- Publication Date
- 2024-10-11
AI Technical Summary
The existing method of manufacturing colored mobile phone cases is cumbersome and lacks radiation protection function, making it difficult to achieve rich colors and simplify the process at the same time.
Use anodizing and/or molten salt electrochemical methods to surface-treat mobile phone case substrates made of tantalum, niobium, tantalum-niobium alloy, titanium and other materials to form an amorphous metal oxide layer or lithium-containing compound layer to achieve color and radiation protection Effect.
The colorful mobile phone case is realized with rich colors, simplified process, and has the function of reducing mobile phone radiation, and is easy to repair and change the color.
Smart Images

Figure CN118756286A_ABST
Abstract
Description
[0001] This application is a divisional application of the patent application with application number 202180007232.8, application date September 24, 2021, and invention name “A colorful or patterned mobile phone case that can reduce radiation and preparation method”. Technical Field
[0002] The invention relates to a method for manufacturing a colored product, in particular to a method for manufacturing a colored mobile phone shell, and a colored product manufactured by the method, in particular to a colored mobile phone shell. Background Art
[0003] Colored products are often favored by people, especially mobile phones with beautiful appearance. With the rapid development of the mobile phone industry, the functions of mobile phones are becoming more and more powerful. At the same time, the appearance of mobile phones is also receiving more and more attention, especially the color of mobile phone shells. In addition, since mobile phones have certain radiation, the manufacture of mobile phone shells with anti-radiation function is also receiving more and more attention.
[0004] CN106067911A describes a method for preparing a plastic mobile phone case, comprising the following steps: (1) mixing a plastic substrate, a fluorescent powder and a dye in proportion, and putting the mixture into an injection molding machine to squeeze the mixture into a mobile phone case mold for forming; (2) spraying a primer and a color paint in sequence, and then vacuum coating; (3) removing the vacuum coating from the area on the vacuum coating layer where the color paint layer is to be displayed by laser engraving; and (4) sequentially forming a middle paint layer and a UV top paint layer on the coating surface after vacuum coating.
[0005] The method described in this patent has complicated processing steps, and the plastic mobile phone case does not have radiation protection function.
[0006] CN105970270A describes a process for processing two aluminum anodizing colors on an aluminum metal mobile phone case, characterized in that it includes the following steps:
[0007] Step 1: Processing the aluminum casing: Using CNC cutting to process the aluminum casing;
[0008] Step 2, injection molding of PPS plastic: injection molding of PPS plastic at the corresponding position of the aluminum casing prepared in step 1;
[0009] Step 3: First anodizing and coloring of aluminum: After completing step 2 of injection molding of PPS plastic, the entire aluminum casing is anodized and colored for the first time;
[0010] Step 4: Processing high-gloss edges: After completing the first aluminum anodizing coloring in step 3, use CNC to cut and process high-gloss edges of equal width on the edge of the aluminum casing;
[0011] Step 5: Use photosensitive protective ink to cover part of the bright edge: Apply photosensitive protective ink on the surface of part of the bright edge, and then bake it at a certain temperature for a certain time and then expose it;
[0012] Step 6, second aluminum anodizing coloring: a second aluminum anodizing coloring is performed on the part of the bright edge that is not shielded by the photosensitive protective ink; wherein the color of the second aluminum anodizing coloring is the same as the color of the first aluminum anodizing coloring;
[0013] Step 7, cleaning the photosensitive protective ink: using a cleaning solution to clean the photosensitive protective ink after exposure in step 5 to reveal the high gloss edge;
[0014] Step eight, third aluminum anodizing coloring: perform a third aluminum anodizing coloring on the bright edges exposed after cleaning the exposed photosensitive protective ink in step seven, wherein the color of the third aluminum anodizing coloring is different from the color of the first aluminum anodizing coloring, thus completing the process of processing two aluminum anodizing colors on the aluminum metal mobile phone case.
[0015] The method described in this patent also has complicated processing steps.
[0016] CN107567217A describes a method for preparing a shell, which includes: (1) providing a metal substrate, and performing hard anodizing treatment on the metal substrate to obtain a metal substrate having a metal hard anodized shell; (2) forming a resin film layer on one surface of the metal substrate obtained in step (1); (3) performing alkaline etching on the substrate obtained in step (2) to remove the metal hard anodized shell on the surface of the substrate where the resin film layer is not formed; (4) performing acid etching on the substrate obtained in step (3) to remove the remaining metal in the substrate.
[0017] In the patent, the holes and etching formed on the surface can cause the surface color to change. In addition, the method described in the patent also has complicated processing steps.
[0018] Therefore, there is still a need to find a method for manufacturing colored products, especially colored mobile phone shells, which not only has a simple process and can obtain rich colors, but also the manufactured mobile phone shells have radiation protection function. Summary of the invention
[0019] To this end, the present invention provides a method for manufacturing a colored product, which comprises the following steps:
[0020] (1) providing a product substrate; and
[0021] (2) surface treatment of the product substrate is performed by anodizing and / or molten salt electrochemical method,
[0022] The product substrate is made of a material selected from tantalum, niobium, tantalum-niobium alloy, titanium and titanium alloy. Preferably, the product substrate is made of a material selected from tantalum, niobium, tantalum-niobium alloy and titanium. More preferably, the product substrate is made of a material selected from tantalum, niobium and tantalum-niobium alloy.
[0023] The present invention also provides a method for manufacturing a colored shell, which comprises the following steps:
[0024] (1) providing a shell substrate; and
[0025] (2) surface treating the shell substrate by anodizing and / or molten salt electrochemical method,
[0026] The shell matrix is made of a material selected from tantalum, niobium, tantalum-niobium alloy, titanium and titanium alloy, preferably the shell matrix is made of a material selected from tantalum, niobium, tantalum-niobium alloy and titanium, and more preferably the shell matrix is made of a material selected from tantalum, niobium and tantalum-niobium alloy.
[0027] The present invention further provides a method for manufacturing a colored mobile phone case, which comprises the following steps:
[0028] (1) providing a mobile phone case base; and
[0029] (2) surface treatment of the mobile phone case substrate is performed by anodizing and / or molten salt electrochemical method,
[0030] The mobile phone case substrate is made of a material selected from tantalum, niobium, tantalum-niobium alloy, titanium and titanium alloy. Preferably, the mobile phone case substrate is made of a material selected from tantalum, niobium, tantalum-niobium alloy and titanium. More preferably, the mobile phone case substrate is made of a material selected from tantalum, niobium and tantalum-niobium alloy.
[0031] The present invention also provides a colored product manufactured by the above method, comprising:
[0032] (1) Product matrix; and
[0033] (2) an amorphous metal oxide layer and / or a lithium compound layer formed on the surface of the product substrate,
[0034] The product substrate is made of a material selected from tantalum, niobium, tantalum-niobium alloy, titanium and titanium alloy. Preferably, the product substrate is made of a material selected from tantalum, niobium, tantalum-niobium alloy and titanium. More preferably, the product substrate is made of a material selected from tantalum, niobium and tantalum-niobium alloy.
[0035] The present invention also provides a colored housing manufactured by the above method, comprising:
[0036] (1) Shell base; and
[0037] (2) an amorphous metal oxide layer and / or a lithium-containing compound layer formed on the surface of the shell substrate,
[0038] The shell matrix is made of a material selected from tantalum, niobium, tantalum-niobium alloy, titanium and titanium alloy, preferably the shell matrix is made of a material selected from tantalum, niobium, tantalum-niobium alloy and titanium, and more preferably the shell matrix is made of a material selected from tantalum, niobium and tantalum-niobium alloy.
[0039] The present invention also provides a colored mobile phone case manufactured by the above method, comprising:
[0040] (1) a mobile phone case base; and
[0041] (2) an amorphous metal oxide layer and / or a lithium compound layer formed on the surface of the mobile phone case substrate,
[0042] The mobile phone case substrate is made of a material selected from tantalum, niobium, tantalum-niobium alloy, titanium and titanium alloy. Preferably, the mobile phone case substrate is made of a material selected from tantalum, niobium, tantalum-niobium alloy and titanium. More preferably, the mobile phone case substrate is made of a material selected from tantalum, niobium and tantalum-niobium alloy.
[0043] The method for manufacturing a colored product, especially a mobile phone shell, of the present invention has one or more of the following beneficial effects:
[0044] (1) Products with rich colors, especially mobile phone cases, can be obtained; (2) the obtained colorful mobile phone cases have the effect of reducing mobile phone radiation; (3) the production process is simple, and (4) the color can be easily repaired and changed. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 The colored tantalum foil is prepared under different process conditions according to an embodiment of the present invention, which shows the colored foil generated on a tantalum foil with a thickness of 0.28 mm by applying different anodizing voltages and constant pressure for 30 minutes in a 0.05 wt % H3PO4 aqueous solution at 25°C.
[0046] Figure 2 The colored tantalum mobile phone case is prepared under different process conditions according to an embodiment of the present invention, which shows the colored mobile phone case generated on the tantalum mobile phone case of different thicknesses at 25° C. in a 0.05 wt % H 3 PO 4 aqueous solution by applying different anodizing voltages and constant pressure for 40 minutes.
[0047] Figure 3 The colored niobium foils are prepared under different process conditions according to an embodiment of the present invention, which show the colored foils generated on a niobium foil with a thickness of 0.03 mm by applying different anodizing voltages and constant pressure for 40 minutes in a 0.05 wt % H 3 PO 4 aqueous solution at 25° C.
[0048] Figure 4 The colored tantalum-niobium alloy foil is prepared under different process conditions according to an embodiment of the present invention, which shows the colored foil generated on tantalum-niobium alloy foils of different thicknesses (weight ratio of 6:4) by applying different anodizing voltages and constant pressure for 40 minutes in a 0.05 wt% H3PO4 aqueous solution at 25°C.
[0049] Figure 5 : The colored titanium foil is prepared under different process conditions according to an embodiment of the present invention, which shows the colored foil generated on a titanium foil with a thickness of 0.02 mm by applying different anodizing voltages and constant pressure for 40 minutes in a 0.05 wt % H 3 PO 4 aqueous solution at 25° C.
[0050] Figure 6 A colored titanium mobile phone case is prepared in molten lithium nitrate under different process conditions according to one embodiment of the present invention, which shows a colored mobile phone case obtained by applying different anode voltages and maintaining constant pressure for different times on a titanium mobile phone case with a thickness of 0.02 mm in molten lithium nitrate at different temperatures.
[0051] Figure 7 The present invention is a colored titanium mobile phone case prepared in molten lithium nitrate under different process conditions according to another embodiment of the present invention, which shows a colored mobile phone case obtained by applying an anode voltage of 10 V and maintaining constant pressure for different times on a titanium mobile phone case with a thickness of 0.02 mm in molten lithium nitrate at 460° C.
[0052] Figure 8 Gray and white tantalum foil, niobium foil and tantalum-niobium alloy foil prepared in molten lithium nitrate according to an embodiment of the present invention are shown, which show the colored and white mobile phone shells obtained by tantalum in molten lithium nitrate at different temperatures, voltages and constant pressure times.
[0053] Fig. 9 It is a titanium mobile phone case with colorful patterns prepared according to an embodiment of the present invention, which shows a colorful mobile phone case made of titanium foil in lithium nitrate at 268°C.
[0054] Fig.10 It is a tantalum mobile phone case with colorful patterns prepared in a 0.05 wt % H3PO4 aqueous solution according to an embodiment of the present invention, which shows a colorful mobile phone case made by anodic oxidation of tantalum foil in a 0.05 wt % H3PO4 aqueous solution.
[0055] Fig.11 The niobium mobile phone case with colorful patterns prepared in a 0.05 wt % H3PO4 aqueous solution according to an embodiment of the present invention shows a colorful mobile phone case made by anodizing niobium foil in a 0.05 wt % H3PO4 aqueous solution.
[0056] Fig.12The colored tantalum, niobium and tantalum-niobium alloy foils are prepared in lithium nitrate:potassium nitrate (weight ratio 1:1) according to an embodiment of the present invention, which shows the colored foils of tantalum foil, tantalum-niobium alloy foil (1:1) and niobium foil generated under different conditions in a mixed molten liquid of lithium nitrate:potassium nitrate (1:1). DETAILED DESCRIPTION
[0057] The method for manufacturing a colored product (such as a mobile phone case) of the present invention can adopt an anodic oxidation method and / or a molten salt electrochemical method. In particular, for tantalum, niobium and tantalum-niobium alloys, either an anodic oxidation method alone or a combination of an anodic oxidation method and a molten salt electrochemical method can be used to prepare colored products, including colored mobile phone cases, while for titanium and titanium alloys, an anodic oxidation method is preferably used to prepare colored products, and a molten salt anodization method is more preferably used to prepare colored products, including colored mobile phone cases.
[0058] Anodic oxidation
[0059] In an oxygen-containing electrolyte solution, at an appropriate temperature, tantalum, niobium, tantalum-niobium alloy, titanium and titanium alloy products such as mobile phone cases are used as anodes, nickel or stainless steel or other metals that are stable to oxygen-containing electrolyte solutions are used as cathodes, and a suitable anode voltage is applied and maintained at a constant voltage for an appropriate time for anodic oxidation.
[0060] In one embodiment, the method of making a colored article of the present invention comprises the following steps:
[0061] (1) providing a product substrate; and
[0062] (2) surface treatment of the product substrate is performed by anodizing,
[0063] The product substrate is made of a material selected from tantalum, niobium, tantalum-niobium alloy, titanium and titanium alloy. Preferably, the product substrate is made of a material selected from tantalum, niobium, tantalum-niobium alloy and titanium. More preferably, the product substrate is made of a material selected from tantalum, niobium and tantalum-niobium alloy. It is also preferred that the product substrate is made of a material selected from titanium and titanium alloy.
[0064] In one embodiment, the method for making a colored shell of the present invention comprises the following steps:
[0065] (1) providing a shell substrate; and
[0066] (2) surface treatment of the shell substrate is performed by anodizing,
[0067] The shell matrix is made of a material selected from tantalum, niobium, tantalum-niobium alloy, titanium and titanium alloy, preferably the shell matrix is made of a material selected from tantalum, niobium, tantalum-niobium alloy and titanium, more preferably the shell matrix is made of a material selected from tantalum, niobium and tantalum-niobium alloy, and further preferably the shell matrix is made of a material selected from titanium and titanium alloy.
[0068] In one embodiment, the method for manufacturing a colored mobile phone case of the present invention comprises the following steps:
[0069] (1) providing a mobile phone case base; and
[0070] (2) surface treatment of the mobile phone case substrate is performed by anodizing,
[0071] The mobile phone case substrate is made of a material selected from tantalum, niobium, tantalum-niobium alloy, titanium and titanium alloy. Preferably, the mobile phone case substrate is made of a material selected from tantalum, niobium, tantalum-niobium alloy and titanium. More preferably, the mobile phone case substrate is made of a material selected from tantalum, niobium and tantalum-niobium alloy. Also preferably, the mobile phone case substrate is made of a material selected from titanium and titanium alloy.
[0072] In a preferred embodiment, the substrate, such as a housing substrate and a mobile phone housing substrate, is made of tantalum.
[0073] In a preferred embodiment, the substrate, such as the housing substrate and the mobile phone housing substrate, is made of niobium.
[0074] In a preferred embodiment, the substrate, such as a shell substrate and a mobile phone shell substrate, is made of a tantalum-niobium alloy.
[0075] In a preferred embodiment, the base body, such as the housing base body and the mobile phone housing base body, is made of titanium.
[0076] In a preferred embodiment, the substrate, such as the housing substrate and the mobile phone housing substrate, is made of a titanium alloy.
[0077] Preferably, the anodization method is carried out under the following conditions: the electrolyte solution temperature is 20°C-600°C, the anode voltage is 1V-800V, the constant voltage time is 0.01-2 hours, and the boost current density is 1-200mA / cm 2 , to form an amorphous metal oxide layer on the surface of a substrate such as a shell substrate and a mobile phone shell substrate.
[0078] The electrolyte solution includes an aqueous solution, a mixture of an aqueous solution and an organic compound, and a non-aqueous solution.
[0079] In one embodiment, the aqueous solution comprises an aqueous solution of an acid, a base or a salt, preferably an aqueous phosphoric acid solution. Preferably, the concentration of the aqueous phosphoric acid solution is 0.01-1 wt %, preferably 0.01-0.1 wt %, more preferably 0.01-0.05 wt %.
[0080] In one embodiment, in the mixture of an aqueous solution and an organic compound, the aqueous solution comprises an aqueous solution of an acid, a base or a salt, and the organic compound comprises an alcohol organic compound, such as ethanol, ethylene glycol, n-butanol or any combination thereof.
[0081] In a preferred embodiment, the mixture of the aqueous solution and the organic compound comprises a mixture of an aqueous phosphoric acid solution having a concentration of 0.01-0.05 wt% and an alcohol, such as ethylene glycol, in a volume ratio of 1:1 to 1:3, preferably 1:1 to 2:1, more preferably 2:1. Preferably, the mixture of the aqueous solution and the organic compound comprises a mixture of an aqueous phosphoric acid solution having a concentration of 0.05 wt% and ethylene glycol in a weight ratio of 2:1.
[0082] Preferably, the non-aqueous solution comprises anhydrous concentrated sulfuric acid, a molten salt, and a mixture of a molten salt and an alkali substance. Preferably, the molten salt comprises molten lithium nitrate, molten sodium nitrate, molten potassium nitrate, and any combination thereof. Preferably, the alkali substance comprises lithium hydroxide, sodium hydroxide, potassium hydroxide, and any combination thereof.
[0083] In one embodiment, the anodization method can be carried out by placing a substrate such as a shell substrate or a mobile phone shell substrate in an aqueous electrolyte solution or a mixed solution of an aqueous electrolyte solution and an organic compound. Preferably, the solution temperature is 1-99°C, preferably 10-95°C, more preferably room temperature to 90°C, the anode voltage is 5-300V, the constant voltage time is 0.5-1.5 hours, and the boost current density is 5-25mA / cm 2 .
[0084] The solution temperature is preferably controlled at room temperature to 95°C. If the temperature is too high, the water evaporates too quickly. A higher solution temperature, a higher anode voltage, and a longer constant voltage time easily lead to the crystallization of the amorphous metal oxide layer. The crystallized metal oxide layer does not refract or transmit light, and thus does not change color with changes in film thickness (generally gray or off-white).
[0085] In one embodiment, the method for manufacturing a colored mobile phone case comprises the following steps:
[0086] (1) providing a mobile phone case base; and
[0087] (2) surface treatment of the mobile phone case substrate is performed in an aqueous solution by an anodic oxidation method,
[0088] The mobile phone case base is made of tantalum.
[0089] The aqueous solution is preferably an aqueous phosphoric acid solution, more preferably an aqueous phosphoric acid solution with a concentration of 0.01-0.05 wt %.
[0090] In a preferred embodiment, a tantalum mobile phone case with a thickness of 0.01-0.3 mm is prepared, and the tantalum mobile phone case is preferably subjected to an anodic oxidation method at room temperature (25° C.) in a 0.01-0.05 wt % H3PO4 aqueous solution and an anode voltage of 28-32 V is applied and constant pressure is maintained for 0.5-1.5 hours to obtain a blue mobile phone case.
[0091] In a preferred embodiment, a tantalum mobile phone case with a thickness of 0.01-0.3 mm is prepared, and the tantalum mobile phone case is preferably subjected to an anodic oxidation method at room temperature (25° C.) in a 0.01-0.05 wt % H3PO4 aqueous solution and subjected to a constant voltage of 72-84 V for 0.5-1.5 hours to obtain a golden mobile phone case.
[0092] In a preferred embodiment, a tantalum mobile phone case with a thickness of 0.01-0.3 mm is prepared, and the tantalum mobile phone case is preferably subjected to an anodic oxidation method at room temperature (25° C.) in a 0.01-0.05 wt % H3PO4 aqueous solution and an anode voltage of 91-103 V is applied and constant pressure is maintained for 0.5-1.5 hours to obtain a bluish purple mobile phone case.
[0093] In a preferred embodiment, a tantalum mobile phone case with a thickness of 0.01-0.3 mm is prepared, and the tantalum mobile phone case is preferably subjected to an anodic oxidation method at room temperature (25° C.) in a 0.01-0.05 wt % H3PO4 aqueous solution and an anode voltage of 150-160 V is applied and constant pressure is applied for 0.5-1.5 hours to obtain a pink mobile phone case.
[0094] In a preferred embodiment, a tantalum mobile phone case with a thickness of 0.01-0.3 mm is prepared, and the tantalum mobile phone case is preferably subjected to an anodic oxidation method at room temperature (25° C.) in a 0.01-0.05 wt % H 3 PO 4 aqueous solution and an anode voltage of 203-210 V is applied and constant pressure is maintained for 0.5-1.5 hours to obtain a green mobile phone case.
[0095] In another embodiment, the method for manufacturing a colored mobile phone case comprises the following steps:
[0096] (1) providing a mobile phone case base; and
[0097] (2) surface treatment of the mobile phone case substrate is performed in an aqueous solution by an anodic oxidation method,
[0098] The mobile phone case substrate is made of niobium.
[0099] The aqueous solution is preferably an aqueous phosphoric acid solution, more preferably an aqueous phosphoric acid solution with a concentration of 0.01-0.05 wt %.
[0100] In a preferred embodiment, a niobium mobile phone case with a thickness of 0.01-0.3 mm is prepared, and the niobium mobile phone case is preferably subjected to an anodic oxidation method at room temperature (25° C.) in a 0.01-0.05 wt % H 3 PO 4 aqueous solution and an anodic voltage of 21-29 V is applied and constant pressure is applied for 0.5-1.5 hours to obtain a blue mobile phone case.
[0101] In a preferred embodiment, a niobium mobile phone case with a thickness of 0.01-0.3 mm is prepared, and the niobium mobile phone case is preferably subjected to an anodic oxidation method at room temperature (25° C.) in a 0.01-0.05 wt % H 3 PO 4 aqueous solution and an anodic voltage of 31-38 V is applied and constant pressure is applied for 0.5-1.5 hours to obtain a silvery white mobile phone case.
[0102] In a preferred embodiment, a niobium mobile phone case with a thickness of 0.01-0.3 mm is prepared, and the niobium mobile phone case is preferably subjected to an anodic oxidation method at room temperature (25° C.) in a 0.01-0.05 wt % H 3 PO 4 aqueous solution and an anodic voltage of 40-48 V is applied and constant pressure is applied for 0.5-1.5 hours to obtain a golden mobile phone case.
[0103] In a preferred embodiment, a niobium mobile phone case with a thickness of 0.01-0.3 mm is prepared, and the niobium mobile phone case is preferably anodized at room temperature (25° C.) in a 0.01-0.05 wt % H 3 PO 4 aqueous solution and an anode voltage of 71-78 V is applied and constant pressure is applied for 0.5-1.5 hours to obtain a green mobile phone case.
[0104] In a preferred embodiment, a niobium mobile phone case with a thickness of 0.01-0.3 mm is prepared, and the niobium mobile phone case is preferably subjected to an anodic oxidation method at room temperature (25° C.) in a 0.01-0.05 wt % H 3 PO 4 aqueous solution and an anode voltage of 105-113 V is applied and constant pressure is applied for 0.5-1.5 hours to obtain a purple mobile phone case.
[0105] In yet another embodiment, the method for manufacturing a colored mobile phone case comprises the following steps:
[0106] (1) providing a mobile phone case base; and
[0107] (2) surface treatment of the mobile phone case substrate is performed in an aqueous solution by an anodic oxidation method,
[0108] The mobile phone shell substrate is made of tantalum-niobium alloy.
[0109] The aqueous solution is preferably an aqueous phosphoric acid solution, more preferably an aqueous phosphoric acid solution with a concentration of 0.01-0.05 wt %.
[0110] In a preferred embodiment, a tantalum-niobium alloy mobile phone case with a thickness of 0.01-0.3 mm is prepared, and the tantalum-niobium alloy mobile phone case is preferably anodized by applying an anode voltage of 8-18 V in a 0.01-0.05 wt. % H3PO4 aqueous solution at room temperature (25°C) and maintaining a constant voltage for 0.5-1.5 hours to obtain a chocolate-colored mobile phone case.
[0111] In a preferred embodiment, a tantalum-niobium alloy mobile phone case with a thickness of 0.01-0.3 mm is prepared, and the tantalum-niobium alloy mobile phone case is preferably anodized at room temperature (25° C.) in a 0.01-0.05 wt % H3PO4 aqueous solution and an anode voltage of 27-28 V is applied and constant pressure is applied for 0.5-1.5 hours to obtain a sky blue mobile phone case.
[0112] In a preferred embodiment, a tantalum-niobium alloy mobile phone case with a thickness of 0.01-0.3 mm is prepared, and the tantalum-niobium alloy mobile phone case is preferably anodized at room temperature (25° C.) in a 0.01-0.05 wt % H3PO4 aqueous solution and an anode voltage of 38-46 V is applied and constant pressure is applied for 0.5-1.5 hours to obtain a silver-gray mobile phone case.
[0113] In a preferred embodiment, a tantalum-niobium alloy mobile phone case with a thickness of 0.01-0.3 mm is prepared, and the tantalum-niobium alloy mobile phone case is preferably anodized at room temperature (25° C.) in a 0.01-0.05 wt % H3PO4 aqueous solution and an anode voltage of 97-102 V is applied and constant pressure is applied for 0.5-1.5 hours to obtain a marine green mobile phone case.
[0114] In a preferred embodiment, a tantalum-niobium alloy mobile phone case with a thickness of 0.01-0.3 mm is prepared, and the tantalum-niobium alloy mobile phone case is preferably anodized at room temperature (25° C.) in a 0.01-0.05 wt % H 3 PO 4 aqueous solution and an anode voltage of 138-145 V is applied and constant pressure is applied for 0.5-1.5 hours to obtain a violet mobile phone case.
[0115] In a preferred embodiment, a tantalum-niobium alloy mobile phone case with a thickness of 0.01-0.3 mm is prepared, and the tantalum-niobium alloy mobile phone case is preferably anodized at room temperature (25° C.) in a 0.01-0.05 wt % H3PO4 aqueous solution and an anode voltage of 246-251 V is applied and constant pressure is maintained for 0.5-1.5 hours to obtain a dark brown mobile phone case.
[0116] In one embodiment, the method for manufacturing a colored mobile phone case comprises the following steps:
[0117] (1) providing a mobile phone case base; and
[0118] (2) surface treatment of the mobile phone case substrate is performed in an aqueous solution by an anodic oxidation method,
[0119] The mobile phone case base is made of titanium.
[0120] The aqueous solution is preferably an aqueous phosphoric acid solution, more preferably an aqueous phosphoric acid solution with a concentration of 0.01-0.05 wt %.
[0121] In a preferred embodiment, a titanium mobile phone case with a thickness of 0.01-0.3 mm is prepared, and the titanium mobile phone case is preferably subjected to an anodic oxidation method at room temperature (25° C.) in a 0.01-0.05 wt % H3PO4 aqueous solution and an anodic voltage of 44-54 V is applied and constant pressure is applied for 0.5-1.5 hours to obtain a white-green mobile phone case.
[0122] In a preferred embodiment, a titanium mobile phone case with a thickness of 0.01-0.3 mm is prepared, and the titanium mobile phone case is preferably subjected to an anodic oxidation method at room temperature (25° C.) in a 0.01-0.05 wt % H3PO4 aqueous solution and an anodic voltage of 72-84 V is applied and constant pressure is applied for 0.5-1.5 hours to obtain a golden mobile phone case.
[0123] In a preferred embodiment, a titanium mobile phone case with a thickness of 0.01-0.3 mm is prepared, and the titanium mobile phone case is preferably subjected to an anodic oxidation method at room temperature (25° C.) in a 0.01-0.05 wt % H 3 PO 4 aqueous solution and subjected to a constant voltage of 92-109 V for 0.5-1.5 hours to obtain a purple mobile phone case.
[0124] In a preferred embodiment, a titanium mobile phone case with a thickness of 0.01-0.3 mm is prepared, and the titanium mobile phone case is preferably subjected to an anodic oxidation method at room temperature (25° C.) in a 0.01-0.05 wt % H 3 PO 4 aqueous solution and a constant voltage of 121-133 V is applied for 0.5-1.5 hours to obtain a green mobile phone case.
[0125] In a preferred embodiment, a titanium mobile phone case with a thickness of 0.01-0.3 mm is prepared, and the titanium mobile phone case is preferably subjected to an anodic oxidation method at room temperature (25° C.) in a 0.01-0.05 wt % H 3 PO 4 aqueous solution and an anodic voltage of 159-180 V is applied and constant pressure is applied for 0.5-1.5 hours to obtain a brown-gray mobile phone case.
[0126] The anodization method can also be carried out by placing the shell substrate in a non-aqueous electrolyte solution. The electrolyte solution temperature is the melting point of the electrolyte solution material to 500°C, the anode voltage is 3V-66V, and the constant voltage time is 0.1-80 minutes. Preferably, the electrolyte solution temperature is 250-380°C, the anode voltage is 10-40V, and the constant voltage time is 3 seconds-40 minutes.
[0127] In one embodiment, the method for manufacturing a colored shell, especially a mobile phone shell, comprises the following steps:
[0128] (1) providing a shell substrate; and
[0129] (2) treating the shell substrate surface in a non-aqueous solution by an anodic oxidation method,
[0130] The shell matrix is made of a material selected from tantalum, niobium, tantalum-niobium alloy, titanium and titanium alloy.
[0131] The oxide film formed in the non-aqueous solution is porous, and its thickness, that is, color, during the oxide film formation process is not only related to the temperature and the anode voltage, but also to the constant voltage time. However, for the anode oxidation in the aqueous solution, it has nothing to do with the constant voltage time.
[0132] The non-aqueous solution includes anhydrous concentrated sulfuric acid, molten salt, and a mixture of molten salt and alkaline substances. Preferably, the molten salt includes molten lithium nitrate, molten sodium nitrate, molten potassium nitrate and any combination thereof. Preferably, the alkaline substance includes lithium hydroxide, sodium hydroxide, potassium hydroxide and any combination thereof.
[0133] The non-aqueous solution is preferably a molten salt, including molten potassium nitrate, molten sodium nitrate, molten lithium nitrate and any combination thereof. Preferably, the molten salt is molten lithium nitrate.
[0134] In one embodiment, the method for manufacturing a colored shell, especially a mobile phone shell, comprises the following steps:
[0135] (1) providing a shell substrate; and
[0136] (2) treating the shell substrate surface in a non-aqueous solution by an anodic oxidation method,
[0137] The shell base body is made of titanium.
[0138] like Figure 6 and Figure 7 As shown, in a preferred embodiment, the shell substrate made of titanium is anodized in lithium nitrate at 460° C. at a voltage of 10 V for 5 minutes to obtain a golden shell.
[0139] In a preferred embodiment, a shell substrate made of titanium is anodized in lithium nitrate at 482° C. at a voltage of 12 V for 10 minutes to obtain a purple shell.
[0140] In a preferred embodiment, the shell substrate made of titanium is anodized in lithium nitrate at 460° C. at a voltage of 10 V for 60 minutes to obtain a royal blue shell.
[0141] In a preferred embodiment, the shell substrate made of titanium is anodized in lithium nitrate at 300-350° C. at a voltage of 10 V for 2 minutes to obtain a sky blue shell.
[0142] In a preferred embodiment, a shell substrate made of titanium is anodized in lithium nitrate at 482° C. at a voltage of 12 V for 10 minutes to obtain a purple shell.
[0143] In one embodiment, the present invention provides a method for preparing a colored product having a plurality of color patterns, especially a colored mobile phone case, comprising the following steps:
[0144] (1) forming a color pattern on a product substrate according to a predetermined pattern by anodizing and / or molten salt electrochemical method; and
[0145] (2) The formed color pattern is masked, and then another color pattern is formed by an anodic oxidation method and / or a molten salt electrochemical method.
[0146] In a preferred embodiment, in the method of preparing a colored product with multiple color patterns, especially a colored mobile phone shell, a portion of the mobile phone shell can be first protected with a tape having a specific pattern, and then the mobile phone shell is anodized to form a color pattern, and then the tape is torn off and the color pattern formed on the mobile phone shell is protected with another tape, and then the mobile phone shell is further anodized to obtain another color pattern. Of course, multiple tapes can be used to protect the mobile phone shell during anodization to obtain a mobile phone shell with multiple colors, such as three or more colors. The tape used is usually a waterproof tape and has tolerance to the anodizing conditions used.
[0147] In a preferred embodiment, the method for preparing a colored article having a plurality of color patterns, especially a colored mobile phone case, comprises:
[0148] (1) Determine the metal material and specific pattern on the mobile phone case;
[0149] (2) Determine the color used for each pattern on the phone case;
[0150] (3) Determine the order of surface treatments to achieve the color of each pattern on the mobile phone housing. The order should comply with the principle of gradually reducing the thickness of the oxide film, that is, the thickness of the film corresponding to the color of the first surface treatment (or anodizing treatment) should be greater than the thickness of the film of the color of the subsequent treatment; and
[0151] (4) Use waterproof and acid-proof tape to protect the part other than the first anodized pattern, and then tear it off after the first oxidation treatment is completed. Then use this tape protection method to perform anodization treatment on the next pattern until all the patterns are processed.
[0152] The waterproof tape should also meet the tolerance of the anodizing conditions used, such as temperature, acid resistance, etc.
[0153] Molten salt electrochemical method
[0154] In one embodiment, the method for manufacturing a colored shell, especially a mobile phone shell, comprises the following steps:
[0155] (1) providing a shell substrate; and
[0156] (2) surface treating the shell substrate by molten salt electrochemical method,
[0157] The shell substrate is made of a material selected from tantalum, niobium and tantalum-niobium alloy.
[0158] Preferably, the molten salt electrochemical method is a molten lithium salt electrochemical method.
[0159] Preferably, the molten salt electrochemical method comprises placing the shell substrate in an oxygen-containing inorganic lithium salt, a mixed melt of an oxygen-containing inorganic lithium salt and lithium hydroxide, a mixed melt of salt and lithium hydroxide, or a mixed melt of a lithium salt and an oxygen-containing salt at 200°C-650°C, applying an anode voltage of 1-66V, and maintaining a constant voltage for 3 seconds-60 hours, for example, 0.1-90 minutes, wherein the boost current density is 1-1000mA / cm 2 , a white or off-white shell is obtained. Preferably, an ultrasonic generator is arranged in the mixed melt or the mixed melt liquid.
[0160] Preferably, the temperature of the mixed melt or the mixed melt is 250°C-520°C, the applied anode voltage is 5-25V, and the boost current density is 5-20mA / cm 2 .
[0161] In a preferred embodiment, the oxygen-containing inorganic lithium salt is LiNO3.
[0162] In a preferred embodiment, the mixed melt of lithium salt and oxygen-containing salt is a mixed melt of LiNO 3 and KNO 3 .
[0163] In a preferred embodiment, the mixed melt of lithium salt and oxygen-containing salt is a mixed melt of LiNO3 and KNO3 in a weight ratio of 1:2 to 2:1, preferably 1:1.
[0164] For the mixed melt or the mixed melt, such as nitrates such as LiNO3, NaNO3 and KNO3, the thickness of the amorphous metal oxide film (layer) generated at a higher temperature increases with the increase of the anodizing time. After reaching a certain thickness, the amorphous metal oxide film will react electrochemically with the nitrate to generate a white or grayish white lithium tantalate film, a lithium niobate film, a film of a mixture of lithium tantalate and lithium niobate, especially at higher temperatures and higher anode voltages.
[0165] In one embodiment, the method for manufacturing a colored shell, especially a mobile phone shell, comprises the following steps:
[0166] (1) providing a shell substrate; and
[0167] (2) surface treating the shell substrate by molten salt electrochemical method,
[0168] The shell base body is made of tantalum.
[0169] In one embodiment, a shell substrate made of tantalum is subjected to constant pressure in lithium nitrate at 440° C. to 650° C. at a voltage of 5 to 50 V for 3 seconds to 5 hours to obtain a white shell.
[0170] In a preferred embodiment, the shell substrate made of tantalum is subjected to constant pressure in lithium nitrate at 570° C. to 585° C. at a voltage of 8-50 V for 2 minutes to 5 hours to obtain a white shell.
[0171] In one embodiment, a shell substrate made of niobium is subjected to constant pressure at a voltage of 5-48 V for 2 seconds to 2 hours in lithium nitrate:potassium nitrate (weight ratio of 1:2 to 2:1, preferably weight ratio of 1:1) at 380° C. to 550° C. to obtain a white shell.
[0172] In a preferred embodiment, the shell substrate made of niobium is subjected to constant pressure at a voltage of 5-28 V for 2-30 minutes in lithium nitrate:potassium nitrate (weight ratio of 1:2 to 2:1, preferably weight ratio of 1:1) at 450° C.-480° C. to obtain a white shell.
[0173] In one embodiment, the method for manufacturing a colored shell, especially a mobile phone shell, comprises the following steps:
[0174] (1) providing a shell substrate; and
[0175] (2) surface treatment of the shell substrate is performed by an anodic oxidation method and a molten salt electrochemical method,
[0176] The shell substrate is made of a material selected from tantalum, niobium and tantalum-niobium alloy.
[0177] In a preferred embodiment, a shell substrate made of a tantalum-niobium alloy is subjected to constant pressure at 135-145 V for 1-2 hours in a 0.01-0.05 wt % H3PO4 aqueous solution, and then subjected to constant pressure at 25-32 V for 1-3 hours in lithium nitrate:potassium nitrate (weight ratio of 1:2 to 2:1, preferably weight ratio of 1:1) at 460-585°C to obtain a white shell.
[0178] A combination of white or other colored patterns can also be formed on a mobile phone case by combining an anodic oxidation method and a molten salt electrochemical method. For example, a mobile phone case made of tantalum, niobium, or tantalum-niobium alloy can be first electrochemically reacted by adding a suitable anode voltage to a molten oxygen-containing lithium salt, such as lithium nitrate, or a mixed melt of lithium nitrate and potassium nitrate or sodium nitrate to generate a corresponding white lithium tantalate film, or a lithium niobate film, or a mixture of lithium tantalate and lithium niobate. If the pattern is desired to be white and the contrasting background is a colored anodic oxide film, the white film outside the pattern can be removed by mechanical polishing or HF acid corrosion until the metal tantalum, niobium, or tantalum-niobium alloy is exposed, and then the designed colored anodic oxide film is generated by anodic oxidation in a dilute aqueous solution or anodic oxidation in a molten salt.
[0179] The colored product manufactured according to the method of the present invention comprises:
[0180] (1) Product matrix; and
[0181] (2) an amorphous metal oxide layer and / or a lithium compound layer formed on the surface of the product substrate, preferably an amorphous metal oxide layer,
[0182] The product matrix is made of a material selected from tantalum, niobium, tantalum-niobium alloy, titanium and titanium alloy, preferably the product matrix is made of a material selected from tantalum, niobium, tantalum-niobium alloy and titanium, preferably the product matrix is made of a material selected from tantalum, niobium and tantalum-niobium alloy.
[0183] The colored shell manufactured according to the method of the present invention comprises:
[0184] (1) a product shell substrate; and
[0185] (2) an amorphous metal oxide layer and / or a lithium compound layer formed on the surface of the shell substrate, preferably an amorphous metal oxide layer,
[0186] The shell matrix is made of a material selected from tantalum, niobium, tantalum-niobium alloy, titanium and titanium alloy, preferably the shell matrix is made of a material selected from tantalum, niobium, tantalum-niobium alloy and titanium, and more preferably the shell matrix is made of a material selected from tantalum, niobium and tantalum-niobium alloy.
[0187] The colored mobile phone case manufactured according to the method of the present invention comprises:
[0188] (1) a finished mobile phone case substrate; and
[0189] (2) an amorphous metal oxide layer and / or a lithium compound layer formed on the surface of the mobile phone case substrate, preferably an amorphous metal oxide layer,
[0190] The mobile phone case substrate is made of a material selected from tantalum, niobium, tantalum-niobium alloy, titanium and titanium alloy. Preferably, the mobile phone case substrate is made of a material selected from tantalum, niobium, tantalum-niobium alloy and titanium. More preferably, the mobile phone case substrate is made of a material selected from tantalum, niobium and tantalum-niobium alloy.
[0191] In one embodiment, the amorphous metal oxide includes amorphous tantalum pentoxide, amorphous niobium pentoxide, amorphous titanium dioxide, and mixtures thereof.
[0192] In a preferred embodiment, the lithium-containing compound includes lithium tantalate, lithium niobate and mixtures thereof.
[0193] In a preferred embodiment, the shell matrix has a thickness of 0.01-0.5 mm, preferably 0.02-0.3 mm.
[0194] The shell matrix of the present invention can be manufactured by techniques known in the art, such as cutting, casting, calendering, etc., without particular limitation.
[0195] In the context of the present invention, the mobile phone case includes a mobile phone body case, a mobile phone decorative case, a mobile phone protective case, etc.
[0196] In the context of the present invention, colored articles include housings, such as mobile phone housings and computer housings, etc.; accessories, such as rings, bracelets, necklaces and watch straps, etc.; pendants, such as human figures and animal figures, etc.
[0197] In one embodiment, a transparent plastic shell can be added to the outside of the mobile phone shell of the present invention to protect the mobile phone from damage when it is accidentally bumped. The mobile phone shell of the present invention can be embedded in the transparent plastic shell to achieve the purpose of anti-scratch and anti-deformation, and the transparent plastic shell allows the bright colors of the colored mobile phone shell to be appreciated. In addition, the mobile phone decorative shell or mobile phone protective shell embedded in the transparent plastic shell can be easily replaced with another color.
[0198] In another embodiment, the mobile phone case of the present invention, such as a mobile phone decorative case or a mobile phone protective case, can be combined with a plastic transparent case as one body, for example, the metal mobile phone case of the present invention is placed in a transparent plastic case, so that it can be better ensured that when the mobile phone plastic case is taken off, the metal mobile phone case will not be scratched, worn or deformed due to careless operation or the like.
[0199] In the context of the present invention, "color" should be understood to include but not limited to red, green, blue, yellow, purple, golden yellow, white, silvery white, gray, etc.
[0200] Unless otherwise indicated, all percentages or proportions herein are by weight.
[0201] Those skilled in the art can more easily understand the present invention according to the following preferred embodiments, but the preferred embodiments are not intended to limit the scope of the present invention.
[0202] 1. A method for producing a colored product, comprising the following steps:
[0203] (1) providing a product substrate; and
[0204] (2) The product substrate is surface treated by anodizing and / or molten salt electrochemical method, wherein the product substrate is made of a material selected from tantalum, niobium, tantalum-niobium alloy, titanium and titanium alloy.
[0205] 2. The method according to embodiment 1, comprising the following steps:
[0206] (1) providing a shell substrate; and
[0207] (2) surface treating the shell substrate by anodizing and / or molten salt electrochemical method,
[0208] The shell matrix is made of a material selected from tantalum, niobium, tantalum-niobium alloy, titanium and titanium alloy.
[0209] 3. The method according to embodiment 2, comprising the following steps:
[0210] (1) providing a mobile phone case base; and
[0211] (2) The mobile phone case substrate is surface treated by anodizing and / or molten salt electrochemical method, wherein the mobile phone case substrate is made of a material selected from tantalum, niobium, tantalum-niobium alloy, titanium and titanium alloy.
[0212] 4. The method according to any one of embodiments 1-3, wherein step (2) comprises:
[0213] - forming a color pattern on the substrate according to a predetermined pattern by anodization and / or molten salt electrochemical method; and
[0214] - Masking the formed color pattern, and then forming another color pattern by anodization and / or molten salt electrochemical method.
[0215] 5. The method according to any one of embodiments 1 to 3, wherein the anodization method is carried out under the following conditions: the electrolyte solution temperature is 20°C-600°C, the anode voltage is 1V-800V, the constant voltage time is 3 seconds-5 hours, preferably 30 seconds-1.5 hours, and the boost current density is 1-200 mA / cm 2 , to form an amorphous metal oxide layer and / or a lithium-containing compound layer on the surface of the substrate.
[0216] 6. The method according to embodiment 5, wherein the electrolyte solution includes an aqueous solution, a mixture of an aqueous solution and an organic compound, and a non-aqueous solution.
[0217] 7. The method according to embodiment 6, wherein the aqueous solution comprises an aqueous solution of an acid, a base or a salt, preferably an aqueous phosphoric acid solution, and the concentration of the aqueous phosphoric acid solution is 0.01-1% by weight, preferably 0.01-0.05% by weight.
[0218] 8. The method according to embodiment 6, wherein in the mixture of the aqueous solution and the organic compound, the aqueous solution comprises an aqueous solution of an acid, a base or a salt, and the organic compound comprises an alcohol such as ethanol, ethylene glycol, n-butanol or any combination thereof.
[0219] 9. A method according to embodiment 6, wherein the mixture of the aqueous solution and the organic compound comprises a mixture of an aqueous H3PO4 solution with a concentration of 0.01-0.05 wt% and ethylene glycol in a weight ratio of 1:1 to 3:1, preferably 1:1 to 2:1.
[0220] 10. The method according to embodiment 6, wherein the non-aqueous solution includes anhydrous concentrated sulfuric acid, a molten salt, and a mixture of a molten salt and an alkali substance.
[0221] 11. The method according to embodiment 10, wherein the molten salt comprises molten lithium nitrate, molten sodium nitrate, molten potassium nitrate, and any combination thereof.
[0222] 12. The method according to embodiment 10, wherein the alkaline substance comprises lithium hydroxide, sodium hydroxide, potassium hydroxide and any combination thereof.
[0223] 13. A method according to embodiment 6, wherein when the electrolyte solution is an aqueous solution or a mixture of an aqueous solution and an organic compound, the anodization method is carried out under the following conditions: the electrolyte solution temperature is 1-99°C, the anode voltage is 5V-600V, and the constant voltage time is within 90 minutes; preferably, the electrolyte solution temperature is from room temperature to 95°C, the anode voltage is 10-200V, and the constant voltage time is 30-60 minutes.
[0224] 14. A method according to embodiment 13, wherein a tantalum mobile phone case with a thickness of 0.01-0.3 mm is prepared, and the tantalum mobile phone case is preferably subjected to an anodic oxidation method at room temperature (25° C.) in a 0.01-0.05 wt % H3PO4 aqueous solution and subjected to a constant voltage of 72-84 V for 0.5-1.5 hours to obtain a golden mobile phone case.
[0225] 15 A method according to Embodiment 13, wherein a niobium mobile phone case with a thickness of 0.01-0.3 mm is prepared, and the niobium mobile phone case is preferably subjected to an anodic oxidation method at room temperature (25° C.) in a 0.01-0.05 wt % H3PO4 aqueous solution with an anode voltage of 40-48 V and constant pressure for 0.5-1.5 hours to obtain a golden mobile phone case.
[0226] 16. A method according to embodiment 13, wherein a tantalum-niobium alloy mobile phone case with a thickness of 0.01-0.3 mm is prepared, and the tantalum-niobium alloy mobile phone case is preferably anodized by applying an anode voltage of 27-28 V in a 0.01-0.05 wt. % H3PO4 aqueous solution at room temperature (25°C) and maintaining a constant voltage for 0.5-1.5 hours to obtain a sky blue mobile phone case.
[0227] 17. A method according to embodiment 13, wherein a titanium mobile phone case with a thickness of 0.01-0.3 mm is prepared, and the titanium mobile phone case is preferably subjected to an anodic oxidation method at room temperature (25° C.) in a 0.01-0.05 wt % H3PO4 aqueous solution and subjected to a constant voltage of 72-84 V for 0.5-1.5 hours to obtain a golden mobile phone case.
[0228] 18. A method according to embodiment 6, wherein when the electrolyte solution is a non-aqueous solution, the anodization method is carried out under the following conditions: the electrolyte solution temperature is from the melting point of the electrolyte solution substance to 500°C, the anode voltage is 3V-66V, and the constant voltage time is within 60 minutes; preferably, the electrolyte solution temperature is 250-350°C, the anode voltage is 5-40V, and the constant voltage time is 3-30 minutes.
[0229] 19. The method according to embodiment 18, wherein the shell substrate made of titanium is anodized in lithium nitrate at 460° C. at a voltage of 10 V for 5 minutes to obtain a golden shell.
[0230] 20. A method according to any one of embodiments 1-3, wherein the molten salt electrochemical method comprises placing the substrate in an oxygen-containing inorganic lithium salt, a mixed melt of an oxygen-containing inorganic lithium salt and lithium hydroxide, a mixed melt of salt and lithium hydroxide, or a mixed melt of a lithium salt and an oxygen-containing salt at 250°C-650°C, applying an anode voltage of 1-66V, and maintaining a constant voltage for 0.01-60 hours, wherein the boost current density is 1-1000mA / cm2 , get a white or off-white phone case.
[0231] 21. The method according to embodiment 20, wherein the temperature of the mixed melt or the mixed melt is 300°C-520°C, the applied anode voltage is 5-25V, and the boost current density is 5-20mA / cm 2 .
[0232] 22. The method according to embodiment 20, wherein the oxygen-containing inorganic lithium salt is LiNO3.
[0233] 23. The method according to embodiment 20, wherein the shell substrate made of tantalum is subjected to constant pressure in lithium nitrate at 440-650° C. at a voltage of 8-50 V for 2 minutes to 5 hours to obtain a white shell.
[0234] 24. The method according to embodiment 20, wherein the shell substrate made of niobium is subjected to constant pressure at a voltage of 5-28 V for 2-30 minutes in a lithium nitrate / potassium nitrate mixture with a weight ratio of 1:2 to 2:1, preferably a weight ratio of 1:1, at 380-550°C to obtain a white shell.
[0235] 25. The method according to embodiment 2 or 3, comprising the following steps:
[0236] (1) providing a shell substrate; and
[0237] (2) surface treatment of the shell substrate is performed by an anodic oxidation method and a molten salt electrochemical method,
[0238] The shell substrate is made of a material selected from tantalum, niobium and tantalum-niobium alloy.
[0239] 26. A method according to embodiment 25, wherein the shell substrate made of tantalum-niobium alloy is subjected to constant pressure at 135-145 V for 1-2 hours in an aqueous solution of 0.01-0.05 wt % H3PO4, and then subjected to constant pressure at 25-32 V for 1-3 hours in a mixture of lithium nitrate / potassium nitrate with a weight ratio of 1:2 to 2:1, preferably a weight ratio of 1:1, at 400-585°C to obtain a white shell.
[0240] 27. A colored article made according to any one of embodiments 1 to 26, comprising:
[0241] (1) Product matrix; and
[0242] (2) an amorphous metal oxide layer and / or a lithium compound layer formed on the surface of the product substrate, preferably an amorphous metal oxide layer,
[0243] The product matrix is made of a material selected from tantalum, niobium, tantalum-niobium alloy, titanium and titanium alloy. Preferably, the product matrix is made of a material selected from tantalum, niobium, tantalum-niobium alloy and titanium. More preferably, the product matrix is made of a material selected from tantalum, niobium and tantalum-niobium alloy.
[0244] 28. The colored article of embodiment 27, wherein the amorphous metal oxide comprises amorphous tantalum pentoxide, amorphous niobium pentoxide, amorphous titanium dioxide, and mixtures thereof.
[0245] 29. The colored article of embodiment 27 or 28, wherein the lithium-containing compound comprises lithium tantalate, lithium niobate, and mixtures thereof.
[0246] 30. The colored article according to embodiment 27 or 28, wherein the colored article comprises a shell, such as a mobile phone shell and a computer shell; accessories, such as a ring, a bracelet, a necklace and a watch strap; a pendant such as a human figure and an animal figure.
[0247] 31. The colorful article according to embodiment 30, wherein the mobile phone case comprises a mobile phone body case, a mobile phone decorative case and a mobile phone protective case.
[0248] Example
[0249] Certain exemplary embodiments are described below in conjunction with the accompanying drawings. As will be appreciated by those skilled in the art, the described embodiments may be modified in various ways without departing from the spirit or scope of the present invention. Therefore, the accompanying drawings and descriptions are considered to be exemplary and non-restrictive in nature.
[0250] Example 1
[0251] A tantalum mobile phone shell with a thickness of 0.28 mm was prepared. The tantalum mobile phone shell was subjected to an anodic oxidation method and an anode voltage of 1-286 V was applied to the tantalum mobile phone shell in a 0.05 wt% H3PO4 aqueous solution at room temperature for 40 minutes to obtain a colored tantalum mobile phone shell, wherein a blue tantalum mobile phone shell was obtained at 30 V, a golden tantalum mobile phone shell was obtained at 78 V, a purple tantalum mobile phone shell was obtained at 95 V, a green tantalum mobile phone shell was obtained at 125 V, a yellow tantalum mobile phone shell was obtained at 142 V, and a rose-red tantalum mobile phone shell was obtained at 168 V. Figure 1 shown.
[0252] Example 2
[0253] A tantalum mobile phone case with a thickness of 0.03 mm was prepared by anodizing the tantalum mobile phone case, preferably at room temperature (25° C.) in a 0.05 wt % H3PO4 aqueous solution, applying an anode voltage of 30 V and constant pressure for 40 minutes to obtain a blue tantalum mobile phone case, such as Figure 2 shown.
[0254] Example 3
[0255] A tantalum mobile phone shell with a thickness of 0.03 mm was prepared by anodizing the tantalum mobile phone shell, preferably at room temperature (25° C.) in a 0.05 wt % H3PO4 aqueous solution, applying an anode voltage of 75 V and keeping the voltage constant for 40 minutes to obtain a golden tantalum mobile phone shell, such as Figure 2 shown.
[0256] Example 4
[0257] A tantalum mobile phone case with a thickness of 0.02 mm was prepared by anodizing the tantalum mobile phone case, preferably at room temperature (25° C.) in a 0.05 wt % H3PO4 aqueous solution, applying an anode voltage of 100 V and constant pressure for 40 minutes to obtain a blue-purple tantalum mobile phone case, such as Figure 2 shown.
[0258] Example 5
[0259] A tantalum mobile phone case with a thickness of 0.075 mm was prepared by anodizing the tantalum mobile phone case, preferably at room temperature (25° C.) in a 0.05 wt % H 3 PO 4 aqueous solution, applying an anode voltage of 110 V and constant pressure for 40 minutes to obtain a turquoise tantalum mobile phone case, such as Figure 2 shown.
[0260] Example 6
[0261] A tantalum mobile phone case with a thickness of 0.03 mm was prepared by anodizing the tantalum mobile phone case, preferably at room temperature (25° C.) in a 0.05 wt % H3PO4 aqueous solution, applying an anode voltage of 120 V and constant pressure for 40 minutes to obtain a light green tantalum mobile phone case, such as Figure 2 shown.
[0262] Example 7
[0263] A tantalum mobile phone case with a thickness of 0.05 mm was prepared by anodizing the tantalum mobile phone case, preferably at room temperature (25° C.) in a 0.05 wt % H 3 PO 4 aqueous solution, applying an anode voltage of 154 V and constant pressure for 40 minutes to obtain a light pink tantalum mobile phone case, such as Figure 2 shown.
[0264] Example 8
[0265] A tantalum mobile phone shell with a thickness of 0.1 mm was prepared by anodizing the tantalum mobile phone shell, preferably at room temperature (25° C.) in a 0.05 wt % H 3 PO 4 aqueous solution, applying an anode voltage of 160 V and constant pressure for 40 minutes to obtain a pink tantalum mobile phone shell, such as Figure 2 shown.
[0266] Example 9
[0267] A tantalum mobile phone case with a thickness of 0.03 mm was prepared by anodizing the tantalum mobile phone case, preferably at room temperature (25° C.) in a 0.05 wt % H3PO4 aqueous solution, applying an anode voltage of 178 V and constant pressure for 40 minutes to obtain a purple tantalum mobile phone case, such as Figure 2 shown.
[0268] Example 10
[0269] A tantalum mobile phone case with a thickness of 0.03 mm was prepared by anodizing the tantalum mobile phone case, preferably at room temperature (25° C.) in a 0.05 wt % H 3 PO 4 aqueous solution, applying an anode voltage of 205 V and constant pressure for 40 minutes to obtain a green tantalum mobile phone case, such as Figure 2 shown.
[0270] Embodiment 11
[0271] A niobium mobile phone case with a thickness of 0.03 mm was prepared. The niobium mobile phone case was subjected to an anodic oxidation method at room temperature in a 0.05 wt% H3PO4 aqueous solution and a constant voltage of 1-210 V was applied for 40 minutes to obtain a colored niobium mobile phone case, wherein a blue niobium mobile phone case was obtained at 25 V, a silvery white niobium mobile phone case was obtained at 36 V, a golden yellow niobium mobile phone case was obtained at 44 V, a sapphire green niobium mobile phone case was obtained at 73 V, and a purple-red niobium mobile phone case was obtained at 108 V. Figure 3 shown.
[0272] Example 12
[0273] A tantalum-niobium alloy (weight ratio of 6:4) mobile phone case with a thickness of 0.1 mm or 0.28 mm is prepared. The tantalum-niobium alloy mobile phone case is preferably subjected to an anodic oxidation method at room temperature (25° C.) in a 0.05 wt % H3PO4 aqueous solution and subjected to a constant voltage of 1-260 V for 40 minutes to obtain a colored tantalum-niobium alloy mobile phone case, wherein a sky blue tantalum-niobium alloy mobile phone case is obtained at 0.1 mm and 28 V, a gray tantalum-niobium alloy mobile phone case is obtained at 0.1 mm and 43 V, a marine green tantalum-niobium alloy mobile phone case is obtained at 0.28 mm and 100 V, a violet tantalum-niobium alloy mobile phone case is obtained at 0.1 mm and 141 V, and a dark brown tantalum-niobium alloy mobile phone case is obtained at 0.28 mm and 249 V. Figure 4 shown.
[0274] Embodiment 13
[0275] A titanium mobile phone case with a thickness of 0.02 mm is prepared. The titanium mobile phone case is preferably subjected to an anodic oxidation method at room temperature (25° C.) in a 0.05 wt % H3PO4 aqueous solution and subjected to a constant voltage of 1-197 V for 40 minutes to obtain a colored titanium mobile phone case, wherein a silver-gray niobium mobile phone case is obtained at 16 V, a silvery-white niobium mobile phone case is obtained at 24 V, a golden-yellow niobium mobile phone case is obtained at 82 V, a rose-red niobium mobile phone case is obtained at 98 V, and a rose-brown niobium mobile phone case is obtained at 175 V. Figure 5 shown.
[0276] Embodiment 14
[0277] A titanium mobile phone case with a thickness of 0.02 mm was prepared, and then a 10 V anode voltage was applied to the titanium mobile phone case in a molten lithium nitrate solution at 300 °C and constant pressure was applied for 2 minutes to obtain a blue titanium mobile phone case, such as Figure 6 shown.
[0278] Embodiment 15
[0279] A titanium mobile phone case with a thickness of 0.02 mm was prepared, and then a 10 V anode voltage was applied to the titanium mobile phone case in a molten lithium nitrate solution at 350 ° C and constant pressure was applied for 2 minutes to obtain a sky blue titanium mobile phone case, such as Figure 6 shown.
[0280] Example 16
[0281] A titanium mobile phone case with a thickness of 0.02 mm was prepared, and then a 12 V anode voltage was applied to the titanium mobile phone case in a molten lithium nitrate solution at 482 ° C and constant pressure was applied for 0.5 minutes to obtain a rose red titanium mobile phone case, such as Figure 6 shown.
[0282] Embodiment 17
[0283] A titanium mobile phone case with a thickness of 0.02 mm was prepared, and then a 12 V anode voltage was applied to the titanium mobile phone case in a molten lithium nitrate solution at 482 ° C and constant pressure was applied for 10 minutes to obtain a purple titanium mobile phone case, such as Figure 6 shown.
[0284] Embodiment 18
[0285] A titanium mobile phone case with a thickness of 0.02 mm was prepared, and then a 10 V anode voltage was applied to the titanium mobile phone case in a molten lithium nitrate solution at 460 ° C and constant pressure was applied for 1 minute to obtain a light yellow titanium mobile phone case, such as Figure 7 shown.
[0286] Embodiment 19
[0287] A titanium mobile phone case with a thickness of 0.02 mm was prepared, and then a 10 V anode voltage was applied to the titanium mobile phone case in a molten lithium nitrate solution at 460 ° C and constant pressure was applied for 2 minutes to obtain a light yellow titanium mobile phone case, such as Figure 7 shown.
[0288] Embodiment 20
[0289] A titanium mobile phone case with a thickness of 0.02 mm was prepared, and then a 10 V anode voltage was applied to the titanium mobile phone case in a molten lithium nitrate solution at 460 ° C and constant pressure was applied for 5 minutes to obtain a golden titanium mobile phone case, such as Figure 7 shown.
[0290] Embodiment 21
[0291] A titanium mobile phone case with a thickness of 0.02 mm was prepared, and then a 10 V anode voltage was applied to the titanium mobile phone case in a molten lithium nitrate solution at 460°C and constant pressure was applied for 15 minutes to obtain a purple titanium mobile phone case. Figure 7 shown.
[0292] Embodiment 22
[0293] A titanium mobile phone case with a thickness of 0.02 mm was prepared, and then a 10 V anode voltage was applied to the titanium mobile phone case in a molten lithium nitrate solution at 460 ° C and constant pressure was applied for 20 minutes to obtain a lavender titanium mobile phone case, such as Figure 7 shown.
[0294] Embodiment 23
[0295] A titanium mobile phone case with a thickness of 0.02 mm was prepared, and then a 10 V anode voltage was applied to the titanium mobile phone case in a molten lithium nitrate solution at 460 ° C and constant pressure was applied for 30 minutes to obtain a purple titanium mobile phone case, such as Figure 7 shown.
[0296] Embodiment 24
[0297] A titanium mobile phone case with a thickness of 0.02 mm was prepared, and then a 10 V anode voltage was applied to the titanium mobile phone case in a molten lithium nitrate solution at 460 ° C and constant pressure was applied for 35 minutes to obtain a purple titanium mobile phone case. Figure 7 shown.
[0298] Embodiment 25
[0299] A titanium mobile phone case with a thickness of 0.02 mm was prepared, and then a 10 V anode voltage was applied to the titanium mobile phone case in a molten lithium nitrate solution at 460 ° C and constant pressure was applied for 60 minutes to obtain a sapphire blue titanium mobile phone case, such as Figure 7 shown.
[0300] Embodiment 26
[0301] A tantalum mobile phone case with a thickness of 0.05 mm was prepared. A 10 V anode voltage was applied to the tantalum mobile phone case in molten lithium nitrate at 580 ° C and constant voltage reaction was performed for 3s and 60s to obtain an off-white tantalum mobile phone case, such as Figure 8 shown.
[0302] Embodiment 27
[0303] A mobile phone case with a thickness of 0.28 mm was prepared. A 10 V anode voltage was applied to the tantalum mobile phone case in molten lithium nitrate at 580°C and the reaction was carried out at a constant voltage for 3 seconds to 10 minutes to obtain a gray or white tantalum mobile phone case, such as Figure 8 shown.
[0304] Embodiment 28
[0305] A tantalum-niobium alloy mobile phone case with a thickness of 0.05 mm was prepared by first placing the tantalum-niobium alloy mobile phone case in a 90° C. aqueous solution of 0.05 wt.% H3PO4 at a constant voltage of 143 V for 1.5 hours, and then applying a voltage of 28 V to the tantalum-niobium alloy mobile phone case in a molten lithium nitrate:potassium nitrate (1:1 weight ratio) at 482° C. and performing a constant voltage electrochemical reaction for 3 hours to obtain a white tantalum-niobium alloy mobile phone case, as shown in FIG. Figure 8 shown.
[0306] Embodiment 29
[0307] A tantalum-niobium alloy mobile phone case with a thickness of 0.28 mm was prepared by first placing the tantalum-niobium alloy mobile phone case in a 0.05 wt% H3PO4 aqueous solution at 90°C at a constant voltage of 143 V for 1.5 hours, and then applying a voltage of 28 V to the tantalum-niobium alloy mobile phone case in molten lithium nitrate: potassium nitrate (1:1 weight ratio) at 482°C and performing a constant voltage electrochemical reaction for 3 hours to obtain a white tantalum-niobium alloy mobile phone case, as shown in FIG. Figure 8 shown.
[0308] Embodiment 30
[0309] A niobium mobile phone case with a thickness of 0.05 mm was prepared. A voltage of 10 V was applied to the niobium mobile phone case in molten lithium nitrate: potassium nitrate (1:1 weight ratio) at 460°C and the voltage was kept constant for 20 minutes to obtain a white niobium mobile phone case, such as Figure 8 shown.
[0310] Embodiment 31
[0311] A niobium mobile phone case with a thickness of 0.28 mm was prepared. A voltage of 10 V was applied to the niobium mobile phone case in molten lithium nitrate: potassium nitrate (1:1 weight ratio) at 460°C and the voltage was kept constant for 20 minutes to obtain a white niobium mobile phone case, such as Figure 8 shown.
[0312] Embodiment 32
[0313] A titanium foil with a thickness of 0.03 mm was prepared. Under the protection of tape, a voltage of 15 V was applied to the titanium foil in molten lithium nitrate at 268° C. and the voltage was kept constant for 5 minutes to obtain a blue background pattern. The stripe pattern was protected by tape. Then, a voltage of 10 V was applied to the titanium foil in molten lithium nitrate at 268° C. and the voltage was kept constant for 5 minutes to obtain a purple stripe pattern. Fig. 9 As shown in Sample 1.
[0314] Embodiment 33
[0315] A titanium foil with a thickness of 0.03 mm was prepared. Under the protection of tape, a voltage of 10 V was applied to the titanium foil in molten lithium nitrate at 268° C. and the voltage was kept constant for 5 minutes to obtain a purple background pattern. The stripe pattern was protected by tape. Then, a voltage of 5 V was applied to the titanium foil in molten lithium nitrate at 268° C. and the voltage was kept constant for 5 minutes to obtain a golden stripe pattern. Fig. 9 As shown in Sample 2.
[0316] Embodiment 34
[0317] A titanium foil with a thickness of 0.03 mm was prepared. Under the protection of tape, a voltage of 15 V was applied to the titanium foil in molten lithium nitrate at 268° C. and the voltage was kept constant for 5 minutes to obtain a blue background pattern. The Taurus pattern was protected by tape. Then, a voltage of 5 V was applied to the titanium foil in molten lithium nitrate at 268° C. and the voltage was kept constant for 5 minutes to obtain a Taurus pattern. Fig. 9 As shown in sample three.
[0318] Embodiment 35
[0319] Tantalum foils with a thickness of 0.05 mm or 0.075 mm were prepared, and in the case of tape protection, they were placed in a 0.05 wt% H3PO4 aqueous solution at a constant voltage for 30 minutes for each color in the order of the numbers in the figure to obtain tantalum foils with multiple color patterns, such as Fig.10 As shown, in sample one, background 1 is purple, stripe 2 is blue, and stripe 3 is golden; in sample two, the stripe pattern is golden and the background is purple; in sample three, the stripe pattern is golden and the background is blue-purple; in sample four, the cow pattern is golden and the background is blue; in sample five, the cow pattern is golden and the background is purple.
[0320] Embodiment 36
[0321] A niobium foil with a thickness of 0.05 mm was prepared, and under the protection of an adhesive tape, a constant voltage was applied to each color at a corresponding voltage in a 0.05 wt % H3PO4 aqueous solution for 20 minutes in the order of the numbers in the figure to obtain niobium foils each including a plurality of color patterns, such as Fig.11 shown.
[0322] Table 1 below shows the radiation of the mobile phone measured in different directions when the mobile phone is making a call after the mobile phone case of the present invention is installed, as tested by the Electromagnetic Testing Center of Tsinghua University.
[0323] Table 1
[0324]
[0325] The results in Table 1 show that the mobile phone case of the present invention has a certain radiation protection effect. Compared with the mobile phone without the mobile phone case of the present invention, the radiation amount in all directions of the mobile phone when making a call is reduced.
[0326] Although specific embodiments of the present invention are shown and described, it should be understood that other improvements, substitutions and alternatives are known to those skilled in the art. Such improvements, substitutions and alternative embodiments may be made without departing from the spirit and scope of the present invention as determined by the appended claims. Each feature of the present invention is described in the appended claims.
Claims
1. A method for producing a colored product, wherein The following steps are involved: (1) Providing a product substrate; and (2) surface treatment of the product substrate is performed by anodizing and / or molten salt electrochemical method, The product substrate is made of a material selected from tantalum, niobium, tantalum-niobium alloy, titanium and titanium alloy.
2. The method according to claim 1, The following steps are involved: (1) providing a shell substrate; and (2) surface treating the shell substrate by anodizing and / or molten salt electrochemical method, The shell matrix is made of a material selected from tantalum, niobium, tantalum-niobium alloy, titanium and titanium alloy.
3. The method according to claim 2, wherein The following steps are involved: (1) providing a mobile phone case base; and (2) surface treatment of the mobile phone case substrate is performed by anodizing and / or molten salt electrochemical method, The mobile phone case substrate is made of a material selected from tantalum, niobium, tantalum-niobium alloy, titanium and titanium alloy.
4. The method according to any one of claims 1 to 3, wherein step (2) include: - forming a color pattern on the substrate according to a predetermined pattern by anodization and / or molten salt electrochemical method; and - Masking the formed color pattern, and then forming another color pattern by anodization and / or molten salt electrochemical method.
5. The method according to any one of claims 1 to 3, wherein the anodization process is carried out under the following conditions: the electrolyte solution temperature is 20°C-600°C, the anode voltage is 1V-800V, the constant voltage time is 3 seconds-5 hours, preferably 30 seconds-1.5 hours, and the boost current density is 1-200 mA / cm 2 , to form an amorphous metal oxide layer and / or a lithium-containing compound layer on the surface of the substrate. 6 . The method according to claim 5 , wherein the electrolyte solution comprises an aqueous solution, a mixture of an aqueous solution and an organic compound, and a non-aqueous solution.
7. The method according to claim 6, wherein the aqueous solution comprises an aqueous solution of an acid, an alkali or a salt, preferably an aqueous solution of phosphoric acid, and the concentration of the aqueous solution of phosphoric acid is 0.01-1% by weight, preferably 0.01-0.05% by weight.
8. The method according to claim 6, wherein in the mixture of aqueous solution and organic compound, the aqueous solution comprises an aqueous solution of an acid, a base or a salt, and the organic compound comprises an alcohol such as ethanol, ethylene glycol, n-butanol or any combination thereof.
9. The method according to claim 6, wherein the mixture of the aqueous solution and the organic compound comprises a concentration of 0.01-0.05 wt % H 3 PO 4 The weight ratio of the aqueous solution to the ethylene glycol is 1:1 to 3:1, preferably a mixture of 1:1 to 2:
1.
10. The method according to claim 6, wherein the non-aqueous solution comprises anhydrous concentrated sulfuric acid, a molten salt, and a mixture of a molten salt and an alkali substance.
11. The method of claim 10, wherein the molten salt comprises molten lithium nitrate, molten sodium nitrate, molten potassium nitrate, and any combination thereof.
12. The method according to claim 10, wherein the alkaline substance comprises lithium hydroxide, sodium hydroxide, potassium hydroxide and any combination thereof.
13. The method according to claim 6, wherein when the electrolyte solution is an aqueous solution or a mixture of an aqueous solution and an organic compound, the anodization method is carried out under the following conditions: the electrolyte solution temperature is 1-99°C, the anode voltage is 5V-600V, and the constant voltage time is within 90 minutes; preferably, the electrolyte solution temperature is from room temperature to 95°C, the anode voltage is 10-200V, and the constant voltage time is 30-60 minutes.
14. The method according to claim 13, wherein a tantalum mobile phone case having a thickness of 0.01-0.3 mm is prepared by anodizing the tantalum mobile phone case preferably at room temperature (25° C.) at 0.01-0.05 wt % H 3 PO 4 An anode voltage of 28-32 V is applied to the aqueous solution and kept at a constant voltage for 0.5-1.5 hours to obtain a blue mobile phone case.
15. The method according to claim 13, wherein a tantalum mobile phone case having a thickness of 0.01-0.3 mm is prepared by anodizing the tantalum mobile phone case preferably at room temperature (25° C.) at 0.01-0.05 wt % H 3 PO 4 An anode voltage of 72-84 V was applied to the aqueous solution and kept constant for 0.5-1.5 hours to obtain a golden mobile phone case.
16. The method according to claim 13, wherein a tantalum mobile phone case having a thickness of 0.01-0.3 mm is prepared by anodizing the tantalum mobile phone case preferably at room temperature (25° C.) at 0.01-0.05 wt % H 3 PO 4 An anode voltage of 91-103 V was applied to the aqueous solution and kept constant for 0.5-1.5 hours to obtain a blue-purple mobile phone case.
17. The method according to claim 13, wherein a tantalum mobile phone case having a thickness of 0.01-0.3 mm is prepared by anodizing the tantalum mobile phone case preferably at room temperature (25° C.) at 0.01-0.05 wt % H 3 PO 4 An anode voltage of 150-160 V was applied to the aqueous solution and kept constant for 0.5-1.5 hours to obtain a pink mobile phone case.
18. The method according to claim 13, wherein a tantalum mobile phone case having a thickness of 0.01-0.3 mm is prepared by anodizing the tantalum mobile phone case preferably at room temperature (25° C.) in the presence of 0.01-0.05 wt % H 3 PO 4 An anode voltage of 203-210 V was applied to the aqueous solution and kept at a constant voltage for 0.5-1.5 hours to obtain a green mobile phone case.
19. The method according to claim 13, wherein a niobium mobile phone case having a thickness of 0.01-0.3 mm is prepared by anodizing the niobium mobile phone case preferably at room temperature (25°C) in the presence of 0.01-0.05 wt% H 3 PO 4 An anode voltage of 21-29 V is applied to the aqueous solution and maintained at a constant voltage for 0.5-1.5 hours to obtain a blue mobile phone case.
20. The method according to claim 13, wherein a niobium mobile phone case having a thickness of 0.01-0.3 mm is prepared by anodizing the niobium mobile phone case preferably at room temperature (25°C) in the presence of 0.01-0.05 wt% H 3 PO 4 An anode voltage of 31-38 V is applied to the aqueous solution and kept at a constant voltage for 0.5-1.5 hours to obtain a silvery white mobile phone case.
21. The method according to claim 13, wherein a niobium mobile phone case having a thickness of 0.01-0.3 mm is prepared by anodizing the niobium mobile phone case preferably at room temperature (25°C) in the presence of 0.01-0.05 wt% H 3 PO 4 An anode voltage of 40-48 V is applied to the aqueous solution and maintained at a constant voltage for 0.5-1.5 hours to obtain a golden mobile phone case.
22. The method according to claim 13, wherein a niobium mobile phone case having a thickness of 0.01-0.3 mm is prepared by anodizing the niobium mobile phone case preferably at room temperature (25° C.) in the presence of 0.01-0.05 wt % H 3 PO 4 An anode voltage of 71-78 V was applied to the aqueous solution and kept at a constant voltage for 0.5-1.5 hours to obtain a green mobile phone case.
23. The method according to claim 13, wherein a niobium mobile phone case having a thickness of 0.01-0.3 mm is prepared by anodizing the niobium mobile phone case preferably at room temperature (25°C) in the presence of 0.01-0.05 wt% H 3 PO 4 An anode voltage of 105-113 V is applied to the aqueous solution and maintained at a constant voltage for 0.5-1.5 hours to obtain a purple-red mobile phone case.
24. The method according to claim 13, wherein the tantalum-niobium alloy mobile phone case with a thickness of 0.01-0.3 mm is prepared by anodizing the tantalum-niobium alloy mobile phone case preferably at room temperature (25° C.) at 0.01-0.05 wt % H 3 PO 4 An anode voltage of 8-18 V was applied to the aqueous solution and kept constant for 0.5-1.5 hours to obtain a chocolate-colored mobile phone case.
25. The method according to claim 13, wherein a tantalum-niobium alloy mobile phone case having a thickness of 0.01-0.3 mm is prepared by anodizing the tantalum-niobium alloy mobile phone case preferably at room temperature (25°C) in the presence of 0.01-0.05 wt.% H 3 PO 4 An anode voltage of 27-28 V was applied to the aqueous solution and kept at a constant voltage for 0.5-1.5 hours to obtain a sky blue mobile phone case.
26. The method according to claim 13, wherein a tantalum-niobium alloy mobile phone case having a thickness of 0.01-0.3 mm is prepared by anodizing the tantalum-niobium alloy mobile phone case preferably at room temperature (25° C.) at 0.01-0.05 wt % H 3 PO 4 An anode voltage of 38-46 V was applied to the aqueous solution and kept at a constant voltage for 0.5-1.5 hours to obtain a silver-grey mobile phone case.
27. The method according to claim 13, wherein a tantalum-niobium alloy mobile phone case having a thickness of 0.01-0.3 mm is prepared by anodizing the tantalum-niobium alloy mobile phone case preferably at room temperature (25° C.) at 0.01-0.05 wt % H 3 PO 4 An anode voltage of 97-102 V was applied to the aqueous solution and kept constant for 0.5-1.5 hours to obtain a mobile phone case in ocean green.
28. The method according to claim 13, wherein the tantalum-niobium alloy mobile phone case with a thickness of 0.01-0.3 mm is prepared by anodizing the tantalum-niobium alloy mobile phone case preferably at room temperature (25° C.) at 0.01-0.05 wt % H 3 PO 4 An anode voltage of 138-145 V was applied to the aqueous solution and kept constant for 0.5-1.5 hours to obtain a violet mobile phone case.
29. The method according to claim 13, wherein the tantalum-niobium alloy mobile phone case with a thickness of 0.01-0.3 mm is prepared by anodizing the tantalum-niobium alloy mobile phone case preferably at room temperature (25° C.) at 0.01-0.05 wt % H 3 PO 4 An anode voltage of 246-251 V was applied to the aqueous solution and kept at a constant voltage for 0.5-1.5 hours to obtain a dark brown mobile phone case.
30. The method according to claim 13, wherein a titanium mobile phone case having a thickness of 0.01-0.3 mm is prepared by anodizing the titanium mobile phone case preferably at room temperature (25° C.) at 0.01-0.05 wt % H 3 PO 4 An anode voltage of 72-84 V was applied to the aqueous solution and kept constant for 0.5-1.5 hours to obtain a golden mobile phone case.
31. The method according to claim 6, wherein when the electrolyte solution is a non-aqueous solution, the anodization method is carried out under the following conditions: the electrolyte solution temperature is from the melting point of the electrolyte solution substance to 500°C, the anode voltage is 3V-66V, and the constant voltage time is within 60 minutes; preferably, the electrolyte solution temperature is 250-350°C, the anode voltage is 5-40V, and the constant voltage time is 3-30 minutes.
32. The method according to claim 31, wherein the shell substrate made of titanium is anodized in lithium nitrate at 460°C at a voltage of 10 V for 5 minutes to obtain a golden shell.
33. The method according to any one of claims 1 to 3, wherein the molten salt electrochemical method comprises placing the substrate in an oxygen-containing inorganic lithium salt, a mixed melt of an oxygen-containing inorganic lithium salt and lithium hydroxide, a mixed melt of salt and lithium hydroxide, or a mixed melt of a lithium salt and an oxygen-containing salt at 250°C to 650°C, applying an anode voltage of 1 to 66V, and maintaining the voltage for 0.01 to 60 hours, wherein the boost current density is 1 to 1000 mA / cm 2 , get a white or off-white phone case.
34. The method according to claim 33, wherein the temperature of the mixed melt or the mixed melt is 300°C-520°C, the applied anode voltage is 5-25V, and the boost current density is 5-20mA / cm 2 .
35. The method according to claim 33, wherein the oxygen-containing inorganic lithium salt is LiNO 3 .
36. The method according to claim 33, wherein the shell substrate made of tantalum is subjected to constant pressure in lithium nitrate at 440-650°C at a voltage of 8-50V for 2 minutes to 5 hours to obtain a white shell.
37. The method according to claim 33, wherein the shell substrate made of niobium is subjected to constant pressure at a voltage of 5-28 V for 2-30 minutes in a lithium nitrate / potassium nitrate mixture with a weight ratio of 1:2 to 2:1, preferably a weight ratio of 1:1, at 380-550°C to obtain a white shell.
38. The method according to claim 2 or 3, wherein The following steps are involved: (1) providing a shell substrate; and (2) surface treatment of the shell substrate is performed by an anodic oxidation method and a molten salt electrochemical method, The shell substrate is made of a material selected from tantalum, niobium and tantalum-niobium alloy.
39. The method according to claim 38, wherein the shell substrate made of tantalum-niobium alloy is 0.01-0.05 wt. % H 3 PO 4 The aqueous solution is subjected to constant pressure at 135-145 V for 1-2 hours, and then in a lithium nitrate / potassium nitrate mixture with a weight ratio of 1:2 to 2:1, preferably a weight ratio of 1:1 at 400-585°C at a voltage of 25-32 V for 1-3 hours to obtain a white shell.
40. The method according to claim 1, wherein a tantalum foil having a thickness of 0.075 mm is prepared and the tantalum foil is protected by a tape and heated to 0.05 wt. % H 3 PO 4 In aqueous solution, a purple background was obtained by constant voltage of 168 V for 30 minutes, and a golden pattern was obtained by constant voltage of 78 V for 30 minutes.
41. The method according to claim 1, wherein a tantalum foil having a thickness of 0.075 mm is prepared and the tantalum foil is coated with 0.05 wt. % H 3 PO 4 In aqueous solution, a blue-purple background was obtained by constant voltage of 96 V for 30 minutes, and a golden pattern was obtained by constant voltage of 78 V for 30 minutes.
42. The method according to claim 1, wherein a tantalum foil having a thickness of 0.05 mm is prepared and protected by a tape in an atmosphere of 0.05 wt. % H 3 PO 4 In aqueous solution, a blue background was obtained by constant voltage of 106 V for 30 minutes, and a golden cow pattern was obtained by constant voltage of 75 V for 30 minutes.
43. The method according to claim 1, wherein a tantalum foil having a thickness of 0.05 mm is prepared and protected by a tape in an atmosphere of 0.05 wt. % H 3 PO 4 In aqueous solution, a purple background was obtained by constant voltage of 95 V for 30 minutes, and a golden cow pattern was obtained by constant voltage of 75 V for 30 minutes.
44. The method according to claim 1, wherein a niobium foil having a thickness of 0.05 mm is prepared and the niobium foil is coated with 0.05 wt. % H 3 PO 4 In aqueous solution, a sapphire blue background was obtained by constant voltage of 66 V for 20 minutes, and a golden pattern was obtained by constant voltage of 46 V for 20 minutes.
45. The method according to claim 1, wherein a niobium foil having a thickness of 0.05 mm is prepared and the niobium foil is coated with 0.05 wt. % H 3 PO 4 In aqueous solution, a grass green background was obtained by constant voltage of 78 V for 20 minutes, and a golden pattern was obtained by constant voltage of 46 V for 20 minutes.
46. The method according to claim 1, wherein a niobium foil having a thickness of 0.05 mm is prepared and the niobium foil is coated with 0.05 wt. % H 3 PO 4 In aqueous solution, a constant voltage of 100 V was applied for 20 minutes to obtain the background, and a constant voltage of 46 V was applied for 20 minutes to obtain the Taurus pattern.
47. The method according to claim 1, wherein a niobium foil having a thickness of 0.05 mm is prepared and protected by a tape in an atmosphere of 0.05 wt. % H 3 PO 4 In aqueous solution, a constant voltage of 66 V was applied for 20 minutes to obtain the background, and a constant voltage of 46 V was applied for 20 minutes to obtain the Taurus pattern.
48. A colored article produced according to any one of claims 1 to 47, wherein include: (1) Product substrate; and (2) an amorphous metal oxide layer and / or a lithium compound layer formed on the surface of the product substrate, preferably an amorphous metal oxide layer, The product matrix is made of a material selected from tantalum, niobium, tantalum-niobium alloy, titanium and titanium alloy. Preferably, the product matrix is made of a material selected from tantalum, niobium, tantalum-niobium alloy and titanium. More preferably, the product matrix is made of a material selected from tantalum, niobium and tantalum-niobium alloy.
49. The colored article of claim 48, wherein the amorphous metal oxide comprises amorphous tantalum pentoxide, amorphous niobium pentoxide, amorphous titanium dioxide, and mixtures thereof.
50. The colored article of claim 48 or 49, wherein the lithium-containing compound comprises lithium tantalate, lithium niobate, and mixtures thereof.
51. The colored article according to claim 48 or 49, wherein the colored article comprises a housing, such as a mobile phone housing and a computer housing; accessories, such as a ring, a bracelet, a necklace and a watch strap; and pendants such as figures and animal figures.
52. The colorful article according to claim 51, wherein the mobile phone case comprises a mobile phone body case, a mobile phone decorative case and a mobile phone protective case.