Broadband near-infrared laser crystal of ytterbium-doped silicate mixed crystal as well as preparation method and application of broadband near-infrared laser crystal
By using different concentrations of Ca2+ ions to replace Mg2+ ions in the Y2Mg3(SiO4)3 laser crystal, and adjusting the matrix structure to enhance the non-uniform broadening of Yb3+ ions, the gap in the research on the luminescence performance of the Yb:Y2Mg3-yCay(SiO4)3 laser crystal is solved. , achieving broadband emission and efficient laser coupling, suitable for high-power laser applications.
Patent Information
- Application Number
- CN202410861277.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-11
AI Technical Summary
So far, no research on the luminescence performance of Yb:Y2Mg3-yCay(SiO4)3 laser crystal has been found, and there is a lack of new laser gain medium materials with excellent performance.
Y2Mg3(SiO4)3 is used as the laser crystal matrix. Ca2+ ions of different concentrations are used to replace Mg2+ ions, and the matrix structure is adjusted to enhance the non-uniform broadening of Yb3+ ions and form broadband emission.
An ultra-wide emission cross-section at ~1μm is achieved, which is beneficial to the generation of tuned lasers and ultrafast lasers, and Yb3+ is effectively coupled to InGaAs LD, making it suitable for high-power laser applications.
Smart Images

Figure CN118756339A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of laser crystal gain materials, and in particular to a broadband near-infrared laser crystal of ytterbium-doped silicate mixed crystal, a preparation method and application thereof. Background Art
[0002] Among rare earth ions, ytterbium (Yb 3+ ) laser crystal has become a hot topic in current research. 3+ The advantages of doped crystals are as follows: Yb 3+ There is an absorption peak at ~976nm, which can be effectively coupled with InGaAs semiconductor lasers (900~980nm), and is close to the emission center wavelength of the crystal (~1μm), with high quantum efficiency, which can reduce heat load and contribute to high-power operation. 3+ Ions have a simple energy level structure, with only two energy levels, namely the ground state energy level 2 F 7 / 2 and excited state energy level 2 F 5 / 2 There are no other excited states, nor are there excited state absorption and multi-phonon absorption, so the energy dissipation caused by adverse effects such as excited state absorption, upconversion and cross relaxation caused by concentration quenching is avoided, and high concentration doping can be achieved. Due to its special energy level structure and long excited state lifetime, it is often used as a sensitization center. Yb 3+ It is more affected by the crystal field than other trivalent rare earth ions. This is because the lanthanide series shrinks and Yb is behind the rare earth ions. 3+ The outer electron shielding effect is weaker, and under the action of crystal field electro-acoustic coupling, the two energy levels produce Stark splitting, which makes it have a wider absorption and fluorescence spectrum and forms a quasi-three-level system. 3+ The wide emission band produced by the interaction with the ligand enables laser amplification to occur in a wider spectral region, which is beneficial to laser pulse compression and thus produces ultrashort pulses in the fs range.
[0003] Y2Mg3(SiO4)3(YMS) is a cubic crystal system. Space group. The composition of YMS is flexible and diverse. 3+ and Mg 2+ Two valence cations can accommodate chemical substitutions with ions of different radii and valences. The addition of different elements will change the lattice parameters, further making some lattice-sensitive luminescence centers (such as Yb 3+ions) in this type of matrix become more flexible. The lower symmetry of the YMS matrix crystal structure is conducive to the splitting of the Starks energy level of the doped ions to enrich the spectrum, broaden the spectrum, and remove the parity ban to achieve the output of polarized lasers, and even use mode locking to obtain ultrashort pulses of ps or even fs lasers. Therefore, Y2Mg 3-y Ca y The twisted ligands in (SiO4)3(YMCS) bring about a strong crystal field, which can greatly broaden the spectral width and affect the spectral performance.
[0004] However, no Yb:Y2Mg has been found so far. 3-y Ca y Research on the luminescence properties of (SiO4)3 laser crystals. Therefore, in order to explore new laser gain medium materials with excellent performance, it is of great significance to study ytterbium ion-doped near-infrared laser crystals YMCS. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a broadband near-infrared laser crystal of ytterbium-doped silicate mixed crystal and its preparation method and application. The present invention uses Y2Mg3(SiO4)3 as the laser crystal matrix and uses different concentrations of Ca 2+ Ion replacement for Mg 2+ ions to adjust the matrix structure, thereby enhancing the Yb 3+ The inhomogeneous broadening of the ions results in broadband emission.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] The present invention provides a broadband near-infrared laser crystal of ytterbium-doped silicate mixed crystal, wherein the chemical formula of the broadband near-infrared laser crystal is Yb x Y 2-x Mg y Ca 3-y (SiO4)3, wherein x=0.001~0.20, y=0~3.
[0008] The present invention also provides a method for preparing the broadband near-infrared laser crystal described in the above technical solution, comprising the following steps:
[0009] 1) Yb2O3, Y2O3, MgO, CaCO3 and SiO2 are used as raw materials, and the ingredients are prepared and mixed according to the following chemical formula to obtain a mixed material;
[0010] 0.5xYb2O3+yMgO+(3-y)CaCO3+0.5(2-x)Y2O3+3SiO2→Yb x Y 2-x Mg y Ca 3-y(SiO4)3+(3-y)CO2↑, where x=0.001~0.20, y=0~3;
[0011] 2) pressing and calcining the mixed material obtained in step 1) to obtain a calcined material;
[0012] 3) The calcined material obtained in step 2) is subjected to crystal growth by a melt method to obtain a broadband near-infrared laser crystal.
[0013] Preferably, the calcination conditions in step 2) include: a temperature of 1250 to 1400° C. and a time of 10 to 15 hours.
[0014] Preferably, the calcination conditions include: temperature of 1300° C. and time of 12 h.
[0015] Preferably, the step 3) melt method comprises: heating to 50-60°C above the melting point, the pulling speed during crystal growth is 1.5-2 mm / h, and the rotation speed is 8-12 rpm;
[0016] After the crystal growth is completed, cool at 15-20℃ / h.
[0017] The present invention also provides a method for preparing the broadband near-infrared laser crystal described in the above technical solution, comprising the following steps:
[0018] A. Yb2O3, Y2O3, MgO, CaCO3 and SiO2 are used as raw materials, and the ingredients are prepared and mixed according to the following chemical formula to obtain a mixed material;
[0019] 0.5xYb2O3+yMgO+(3-y)CaCO3+0.5(2-x)Y2O3+3SiO2→Yb x Y 2-x Mg y Ca 3-y (SiO4)3+(3-y)CO2↑, where x=0.001~0.20, y=0~3;
[0020] B. Pressing and calcining the mixed material obtained in step A to obtain a calcined material;
[0021] C. The calcined material obtained in step B is subjected to crystal growth by a melt method to obtain a broadband near-infrared laser crystal.
[0022] Preferably, the calcination conditions in step B include: temperature of 1280-1380° C. and time of 9-20 hours.
[0023] Preferably, after the calcination, the step B further comprises: grinding, screening and pressing the calcined material, and then calcining to obtain a calcined material;
[0024] The grinding conditions include: grinding in an agate mortar for 20 to 60 minutes;
[0025] The screening conditions include: using a standard sorting sieve with a particle size of 20 to 200 meshes to screen the ground powder, and pressing the sieve-down material.
[0026] Preferably, the melt method in step C comprises any one of a Czochralski method, a laser base heating method, a guided mold method, a pyrolysis method and a heat exchange method.
[0027] The present invention also provides the application of the broadband near-infrared laser crystal described in the above technical solution in one or more of spectroscopy, communication sensing, medical treatment and military defense.
[0028] Beneficial effects of the present invention:
[0029] Using Y2Mg3(SiO4)3 as the laser crystal matrix, different concentrations of Ca 2+ Ion replacement for Mg 2+ ions to adjust the matrix structure, thereby enhancing the Yb 3+ The inhomogeneous broadening of the ions forms broadband emission with an ultra-wide emission cross section at ~1μm, which is conducive to the generation of tunable lasers and ultrafast lasers.
[0030] The grown crystals were optically polished, and the absorption spectrum of the medium was measured from 800 to 1050 nm by a UV-visible-near infrared spectrometer with a resolution of 1 nanometer. Figure 2 The absorption spectrum is shown. Figure 2 In the absorption spectrum shown in the figure, samples 0#-6# correspond to gradually increasing Ca 2+ It can be seen that the absorption bandwidth increases with the co-doping concentration of Ca 2+ The increase of Ca 2+ The high absorption coefficient (α) at 976nm indicates the high absorption capacity of the sample for incident light in this band, indicating that Yb 3+ Can be effectively coupled with InGaAs LD pump source. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required to be used in the embodiments are briefly introduced below.
[0032] Figure 1 Yb x Y 2-x Mg y Ca 3-yA simplified diagram of the energy level transition of (SiO4)3 crystal, where x = 0.001 ~ 0.20, y = 0 ~ 3;
[0033] Figure 2 Yb 0.001 Y 1.999 Mg 0.5 Ca 2.5 Absorption spectrum of (SiO4)3 crystal at 800-1500nm;
[0034] Figure 3 Yb 0.05 Y 1.995 Absorption spectrum of Mg1Ca2(SiO4)3 crystal at 800-1500nm;
[0035] Figure 4 Yb 0.15 Y 1.85 Absorption spectrum of Mg2Ca1(SiO4)3 crystal at 800-1500nm;
[0036] Figure 5 Yb 0.01 Y 1.99 Mg 1.5 Ca 1.5 Absorption spectrum of (SiO4)3 crystal at 800-1500nm;
[0037] Figure 6 Yb 0.2 Y 1.8 Mg 2.5 Ca 0.5 Absorption spectrum of (SiO4)3 crystal at 800-1500nm;
[0038] Figure 7 Yb 0.08 Y 0.92 Absorption spectrum of Mg3Ca0(SiO4)3 crystals at 800-1500nm. DETAILED DESCRIPTION
[0039] The present invention provides a broadband near-infrared laser crystal of ytterbium-doped silicate mixed crystal, wherein the chemical formula of the broadband near-infrared laser crystal is Yb x Y 2-x Mg y Ca 3-y (SiO4)3, wherein x=0.001~0.20, y=0~3.
[0040] The present invention also provides a method for preparing the broadband near-infrared laser crystal described in the above technical solution, comprising the following steps:
[0041] 1) Yb2O3, Y2O3, MgO, CaCO3 and SiO2 are used as raw materials, and the ingredients are prepared and mixed according to the following chemical formula to obtain a mixed material;
[0042] 0.5xYb2O3+yMgO+(3-y)CaCO3+0.5(2-x)Y2O3+3SiO2→Yb x Y 2-x Mg y Ca 3-y (SiO4)3+(3-y)CO2↑, where x=0.001~0.20, y=0~3;
[0043] 2) pressing and calcining the mixed material obtained in step 1) to obtain a calcined material;
[0044] 3) The calcined material obtained in step 2) is subjected to crystal growth by a melt method to obtain a broadband near-infrared laser crystal.
[0045] The present invention uses Yb2O3, Y2O3, MgO, CaCO3, and SiO2 as raw materials, and mixes them according to the following chemical formula to obtain a mixed material;
[0046] 0.5xYb2O3+yMgO+(3-y)CaCO3+0.5(2-x)Y2O3+3SiO2→Yb x Y 2-x Mg y Ca 3-y (SiO4)3+(3-y)CO2↑, where x=0.001-0.20, y=0-3. In the present invention, the purity of the raw materials is 99.999%. In the present invention, the mixing conditions preferably include: putting the weighed raw material powder into a centrifuge tube that has been cleaned in advance, and then placing the centrifuge tube containing the raw material into a sealed box, or directly loading the raw material into the sealed box. Then fix the sealed box on the mixer, and the mixer moves alternately clockwise and counterclockwise for 10-40 hours to ensure uniform mixing.
[0047] The present invention presses and calcines the obtained mixed material to obtain a calcined material. In the present invention, the pressing conditions preferably include: using a mold to press the material to make the raw material into a block. A hydraulic press can be used for initial pressing and then further compacted with an isostatic press after sealing. In the present invention, the calcining conditions preferably include: a temperature of 1250 to 1400°C and a time of 10 to 15 hours. In the present invention, the calcining conditions also preferably include: a temperature of 1300°C and a time of 12 hours.
[0048] The present invention uses a melt method to grow a crystal from the obtained calcined material to obtain a broadband near-infrared laser crystal. In the present invention, the melt method preferably includes: heating to 50-60°C above the melting point, a pulling speed of 1.5-2 mm / h during crystal growth, and a rotation speed of 8-12 rpm; cooling at 15-20°C / h after the crystal growth is completed.
[0049] The present invention also provides a method for preparing the broadband near-infrared laser crystal described in the above technical solution, comprising the following steps:
[0050] A. Yb2O3, Y2O3, MgO, CaCO3 and SiO2 are used as raw materials, and the ingredients are prepared and mixed according to the following chemical formula to obtain a mixed material;
[0051] 0.5xYb2O3+yMgO+(3-y)CaCO3+0.5(2-x)Y2O3+3SiO2→Yb x Y 2-x Mg y Ca 3-y (SiO4)3+(3-y)CO2↑, where x=0.001~0.20, y=0~3;
[0052] B. Pressing and calcining the mixed material obtained in step A to obtain a calcined material;
[0053] C. The calcined material obtained in step B is subjected to crystal growth by a melt method to obtain a broadband near-infrared laser crystal.
[0054] The present invention uses Yb2O3, Y2O3, MgO, CaCO3, and SiO2 as raw materials, and mixes them according to the following chemical formula to obtain a mixed material;
[0055] 0.5xYb2O3+yMgO+(3-y)CaCO3+0.5(2-x)Y2O3+3SiO2→Yb x Y 2-x Mg y Ca 3-y (SiO4)3+(3-y)CO2↑, where x=0.001-0.20, y=0-3. In the present invention, the purity of the raw materials is 99.999%. In the present invention, the mixing conditions preferably include: putting the weighed raw material powder into a centrifuge tube that has been cleaned in advance, and then placing the centrifuge tube containing the raw material into a sealed box, or directly loading the raw material into the sealed box. Then fix the sealed box on the mixer, and the mixer moves alternately clockwise and counterclockwise for 10-40 hours to ensure uniform mixing.
[0056] The present invention presses and calcines the obtained mixed material to obtain a calcined material. In the present invention, the calcination conditions preferably include: a temperature of 1280 to 1380°C and a time of 9 to 20 hours. In the present invention, the calcination preferably includes: grinding, screening and pressing the calcined material, and then calcining to obtain a calcined material. The purpose of the first calcination is to preliminarily synthesize rare earth ion-doped silicate polycrystalline raw materials, which is conducive to crystal growth. Then, by grinding the material obtained by the first sintering and fully pressing it, a sintered raw material with high mechanical strength and good density is obtained. At the same time, compared with the first sintering, the solid phase reaction of the secondary sintering raw material is more sufficient. In the present invention, the grinding conditions preferably include: grinding in an agate mortar for 20 to 60 minutes. In the present invention, the screening conditions preferably include: using a standard sorting sieve with a particle size of 20 to 200 meshes to screen the ground powder and press the screened material. In the present invention, the pressing conditions preferably include: using a mold to press the material to make the raw material into a block. A hydraulic press can be used for initial compression molding, and then an isostatic press can be used for further compaction after sealing.
[0057] The present invention uses a melt method to grow the obtained calcined material into crystals to obtain a broadband near-infrared laser crystal. In the present invention, the melt method preferably includes: any one of a Czochralski method, a laser base heating method, a guided mold method, a kypermeation method and a heat exchange method.
[0058] The present invention also provides the application of the broadband near-infrared laser crystal described in the above technical solution in one or more of spectroscopy, communication sensing, medical treatment and military defense.
[0059] In order to further illustrate the present invention, the present invention is described in detail below in conjunction with embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0060] Example 1
[0061] According to the chemical formula of 0.5xYb2O3+yMgO+(3-y)CaCO3+0.5(2-x)Y2O3+3SiO2→Yb x Y 2- x Mg y Ca 3-y(SiO4)3+(3-y)CO2↑, where x=0.001, y=0.5, calculate the mass of the required raw materials Yb2O3 (purity of 99.999%) 0.0035g, MgO (purity of 99.999%) 0.3557g, CaCO3 (purity of 99.999%) 4.4170g, Y2O3 (purity of 99.999%) 3.9841g, SiO2 (purity of 99.999%) 3.1819g and weigh them accurately, then put the prepared raw materials into the mixer to mix them evenly. Press the mixed sample into blocks and place them in a crucible. Then place the sample in a muffle furnace and calcine it at a sintering temperature of 1250℃ and a time of 10 hours. After that, place the crucible containing the sintered material in a pulling furnace for crystal growth. The furnace is sealed, the temperature is raised to 50°C above the melting point, and then the temperature is slowly lowered to the crystallization point to allow crystal growth.
[0062] During the growth process, the pulling speed was 2 mm / h and the rotation speed was 10 rpm. After the melt growth process was completed, it was cooled to room temperature at an annealing rate of 15 °C / h. 0.001 Y 1.999 Mg 0.5 Ca 2.5 (SiO4)3 crystals are taken out.
[0063] The grown crystals were polished to optical grade and the absorption spectrum was tested using a UV-visible spectrophotometer. Figure 2 In the absorption spectrum shown, it can be observed that Yb 0.001 Y 1.999 Mg 0.5 Ca 2.5 Yb in (SiO4)3 crystal 3+ Ions from the ground state 2 F 7 / 2 to excited state 2 F 5 / 2 Typical absorption band of the transition. It can be seen that in the range of 850-1000nm, there is a wide absorption peak of 850-960nm and a sharp absorption peak with a central wavelength of about 976nm, which corresponds to the wavelength of commercial high-power LD. The large absorption FWHM and absorption cross section of the crystal mean that the crystal has a high efficiency in absorbing pump light and is suitable for InGaAs laser diode pumping.
[0064] Example 2
[0065] According to the chemical formula of 0.5xYb2O3+yMgO+(3-y)CaCO3+0.5(2-x)Y2O3+3SiO2→Yb x Y 2- x Mgy Ca 3-y (SiO4)3+(3-y)CO2↑, where x=0.05, y=1, calculate the masses of the required raw materials Yb2O3 (purity of 99.999%) 0.1751g, MgO (purity of 99.999%) 0.7162g, CaCO3 (purity of 99.999%) 3.5572g, Y2O3 (purity of 99.999%) 3.9124g, SiO2 (purity of 99.999%) 3.2032g and weigh them accurately, then put the prepared raw materials into the mixer to mix them evenly. Press the mixed sample into blocks and place them in a crucible. Then place the sample in a muffle furnace and calcine it at a sintering temperature of 1300℃ and a time of 12 hours. After that, place the crucible containing the sintered material in a pulling furnace for crystal growth. The furnace is sealed, the temperature is raised to 50°C above the melting point, and then the temperature is slowly lowered to the crystallization point to allow crystal growth.
[0066] During the growth process, the pulling speed was 1.5 mm / h and the rotation speed was 12 rpm. After the melt growth process was completed, it was cooled to room temperature at an annealing rate of 18 °C / h. 0.05 Y 1.995 Mg1Ca2(SiO4)3 crystals are taken out.
[0067] The grown crystals were polished to optical grade and the absorption spectrum was tested using a UV-visible spectrophotometer. Figure 3 In the absorption spectrum shown, it can be observed that Yb 0.05 Y 1.995 Yb in Mg1Ca2(SiO4)3 crystal 3+ Ions from the ground state 2 F 7 / 2 to excited state 2 F 5 / 2 The typical absorption band of the transition shows that in the range of 850-1000nm, there is a wide absorption peak of 850-960nm and a sharp absorption peak with a central wavelength of about 976nm, which corresponds to the wavelength of commercial high-power LD. The large absorption FWHM of the crystal means that the crystal has a high efficiency in absorbing pump light and is suitable for InGaAs laser diode pumping.
[0068] Example 3
[0069] According to the chemical formula of 0.5xYb2O3+yMgO+(3-y)CaCO3+0.5(2-x)Y2O3+3SiO2→Yb x Y 2- x Mg y Ca 3-y(SiO4)3+(3-y)CO2↑, where x=0.15, y=2, calculate the mass of the required raw materials Yb2O3 (purity of 99.999%) 0.5322g, MgO (purity of 99.999%) 1.4514g, CaCO3 (purity of 99.999%) 1.8022g, Y2O3 (purity of 99.999%) 3.7610g, SiO2 (purity of 99.999%) 3.2456g respectively and weigh them accurately, then put the prepared raw materials into the mixer to mix them evenly. Press the mixed sample into blocks and place them in a crucible. Then place the sample in a muffle furnace and calcine it at a sintering temperature of 1400℃ and a time of 15 hours. After that, place the crucible containing the sintered material in a pulling furnace for crystal growth. The furnace is sealed, the temperature is raised to 60°C above the melting point, and then the temperature is slowly lowered to the crystallization point to allow crystal growth.
[0070] During the growth process, the pulling speed was 2 mm / h and the rotation speed was 8 rpm. After the melt growth process was completed, it was cooled to room temperature at an annealing rate of 20 °C / h. 0.15 Y 1.85 Mg2Ca1(SiO4)3 crystals are taken out.
[0071] The grown crystals were polished to optical grade and the absorption spectrum was tested using a UV-visible spectrophotometer. Figure 4 In the absorption spectrum shown, it can be observed that Yb 0.15 Y 1.85 In Mg2Ca1(SiO4)3 crystal, Yb 3+ Ions from the ground state 2 F 7 / 2 to excited state 2 F 5 / 2 Typical absorption band of the transition. It can be seen that in the range of 850-1000nm, there is a wide absorption peak of 850-960nm and a sharp absorption peak with a central wavelength of about 976nm, which corresponds to the wavelength of commercial high-power LD. The large absorption FWHM of the crystal means that the crystal has a high efficiency in absorbing pump light and is suitable for InGaAs laser diode pumping.
[0072] Example 4
[0073] The raw materials Yb2O3 (purity of 99.999%) 0.0357g, MgO (purity of 99.999%) 1.0963g, CaCO3 (purity of 99.999%) 2.7223g, Y2O3 (purity of 99.999%) 4.0742g, SiO2 (purity of 99.999%) 3.2655g are mixed according to the chemical formula 0.5xYb2O3+yMgO+(3-y)CaCO3+0.5(2-x)Y2O3+3SiO2→Yb x Y 2-x Mg y Ca 3-y (SiO4)3+(3-y)CO2↑, where x=0.01, y=1.5, calculate the required mass respectively and weigh accurately. Then put the raw materials into centrifuge tubes respectively and place them in a sealed box. Fix the sealed box on the mixer and mix for 20 hours to ensure uniform mixing. Use a press with an acrylic mold to press the mixed sample into a cake shape, then put it into a muffle furnace and sinter it in an air atmosphere. The sintering temperature is 1350℃ and the sintering time is 20 hours to obtain the first sintered polycrystalline material. Then put it into an agate mortar, grind it thoroughly, and use a standard sorting sieve to screen the ground powder (use a standard sorting sieve with a particle size of 200 mesh to screen the ground powder. The powder that does not pass the screening will be returned to the agate mortar for further grinding and then screened). Then use a glass rod and a funnel to load the screened powder into a balloon with a diameter of 5mm. During the loading process, use a glass rod to make it initially compacted and evenly compacted, and finally seal the balloon. The balloon is then pressed under high pressure using a press and sintered again at 1350°C for 20 hours to obtain the material rod required for laser-heated susceptor growth.
[0074] Grind the obtained material rod until the diameter is 1.8mm. Then fix the seed crystal to the seed crystal lifting rod in the laser heating pedestal furnace, and fix the material to the rod feeding rod. Keep the seed crystal and the material rod in the same vertical line and in the center of the laser beam circle. Close the furnace, turn on the water cooler and CO2 laser. Adjust the power to raise the temperature above the melting point, wait for the material rod to melt into a hemispherical shape, seed the crystal, set the appropriate pulling speed and material rod feeding speed to grow the crystal. When the growth process is completed, cool it to room temperature at a 0.1W / h annealing rate, and then take out the crystal Yb 0.01 Y 1.99 Mg 1.5 Ca 1.5 (SiO4)3.
[0075] The grown crystals were polished to optical grade and the absorption spectrum was tested using a UV-visible spectrophotometer. Figure 5 In the absorption spectrum shown, it can be observed that Yb 0.01 Y 1.99Mg 1.5 Ca 1.5 In (SiO4)3 crystal, Yb 3+ Ions from the ground state 2 F 7 / 2 to excited state 2 F 5 / 2 Typical absorption band of the transition. It can be seen that in the range of 850-1000nm, there is a wide absorption peak of 850-960nm and a sharp absorption peak with a central wavelength of about 976nm, which corresponds to the wavelength of commercial high-power LD. The large absorption FWHM of the crystal means that the crystal has a high efficiency in absorbing pump light and is suitable for InGaAs laser diode pumping.
[0076] Example 5
[0077] The raw materials Yb2O3 (purity of 99.999%) 0.7143g, MgO (purity of 99.999%) 1.8264g, CaCO3 (purity of 99.999%) 0.9071g, Y2O3 (purity of 99.999%) 3.6838g, SiO2 (purity of 99.999%) 3.2673g are mixed according to the chemical formula 0.5xYb2O3+yMgO+(3-y)CaCO3+0.5(2-x)Y2O3+3SiO2→Yb x Y 2-x Mg y Ca 3-y (SiO4)3+(3-y)CO2↑, where x=0.2, y=2.5, calculate the required mass respectively and weigh accurately. Then put the raw materials into centrifuge tubes respectively and place them in a sealed box. Fix the sealed box on the mixer and mix for 28 hours to ensure uniform mixing. Use a press with an acrylic mold to press the mixed sample into a cake shape, then put it into a muffle furnace and sinter it in an air atmosphere. The sintering temperature is 1280℃ and the sintering time is 9 hours to obtain the first sintered polycrystalline material. Then put it into an agate mortar, grind it thoroughly, and use a standard sorting sieve to screen the ground powder (use a standard sorting sieve with a particle size of 200 mesh to screen the ground powder. The powder that does not pass the screening will be returned to the agate mortar for further grinding and then screened). Then use a glass rod and a funnel to load the screened powder into a balloon with a diameter of 8mm. During the loading process, use a glass rod to make it initially compacted and evenly compacted, and finally seal the balloon. The balloon is then pressed under high pressure using a press and sintered again at 1280°C for 13 hours to obtain the material rod required for laser-heated susceptor growth.
[0078] Grind the obtained material rod until the diameter is 1.55mm. Then fix the seed crystal to the seed crystal lifting rod in the laser heating pedestal furnace, and fix the material to the rod feeding rod. Keep the seed crystal and the material rod in the same vertical line and in the center of the laser beam circle. Close the furnace, turn on the water cooler and CO2 laser. Adjust the power to raise the temperature above the melting point, wait for the material rod to melt into a hemispherical shape, seed the crystal, set the appropriate pulling speed and material rod feeding speed to grow the crystal. When the growth process is completed, cool it to room temperature at a 0.1W / h annealing rate, and then take out the crystal Yb 0.2 Y 1.8 Mg 2.5 Ca 0.5 (SiO4)3.
[0079] The grown crystals were polished to optical grade and the absorption spectrum was tested using a UV-visible spectrophotometer. Figure 6 In the absorption spectrum shown, it can be observed that Yb 0.2 Y 1.8 Mg 2.5 Ca 0.5 Yb in (SiO4)3 crystal 3+ Ions from the ground state 2 F 7 / 2 to excited state 2 F 5 / 2 Typical absorption band of the transition. It can be seen that in the range of 850-1000nm, there is a wide absorption peak of 850-960nm and a sharp absorption peak with a central wavelength of about 976nm, which corresponds to the wavelength of commercial high-power LD. The large absorption FWHM of the crystal means that the crystal has a high efficiency in absorbing pump light and is suitable for InGaAs laser diode pumping.
[0080] Example 6
[0081] The raw materials Yb2O3 (purity of 99.999%) 0.2954g, MgO (purity of 99.999%) 2.2655g, CaCO3 (purity of 99.999%) 0g, Y2O3 (purity of 99.999%) 4.0617g, SiO2 (purity of 99.999%) 3.3774g are prepared according to the chemical formula 0.5xYb2O3+yMgO+(3-y)CaCO3+0.5(2-x)Y2O3+3SiO2→Yb x Y 2-x Mg y Ca 3-y(SiO4)3+(3-y)CO2↑, where x=0.08, y=3, calculate the required mass respectively, and weigh accurately. Then put the raw materials into centrifuge tubes respectively and place them in a sealed box. Fix the sealed box on the mixer and mix for 30 hours to ensure uniform mixing. Use a press with an acrylic mold to press the mixed sample into a cake shape, then put it into a muffle furnace and sinter it in an air atmosphere. The sintering temperature is 1380℃ and the sintering time is 14 hours to obtain the first sintered polycrystalline material. Then put it into an agate mortar, grind it thoroughly, and use a standard sorting sieve to screen the ground powder (use a standard sorting sieve with a particle size of 200 mesh to screen the ground powder. The powder that does not pass the screening will be returned to the agate mortar for further grinding and then screened). Then use a glass rod and a funnel to load the screened powder into a balloon with a diameter of 7.5mm. During the loading process, use a glass rod to make it initially compacted and evenly compacted, and finally seal the balloon. The balloon is then pressed under high pressure using a press and sintered again at 1380°C for 14 hours to obtain the material rod required for laser-heated susceptor growth.
[0082] Grind the obtained material rod until the diameter is 1.85mm. Then fix the seed crystal to the seed crystal lifting rod in the laser heating pedestal furnace, and fix the material to the rod feeding rod. Keep the seed crystal and the material rod in the same vertical line and in the center of the laser beam circle. Close the furnace, turn on the water cooler and CO2 laser. Adjust the power to raise the temperature above the melting point, wait for the material rod to melt into a hemispherical shape, seed the crystal, set the appropriate pulling speed and material rod feeding speed to grow the crystal. When the growth process is completed, cool it to room temperature at a 0.15W / h annealing rate, and then take out the crystal Yb 0.08 Y 0.92 Mg3Ca0(SiO4)3.
[0083] The grown crystals were polished to optical grade and the absorption spectrum was tested using a UV-visible spectrophotometer. Figure 7 In the absorption spectrum shown, it can be observed that Yb 0.08 Y 0.92 Yb in Mg3Ca0(SiO4)3 crystal 3+ Ions from the ground state 2 F 7 / 2 to excited state 2 F 5 / 2 Typical absorption band of the transition. It can be seen that in the range of 850-1000nm, there is a wide absorption peak of 850-960nm and a sharp absorption peak with a central wavelength of about 976nm, which corresponds to the wavelength of commercial high-power LD. The large absorption FWHM of the crystal means that the crystal has a high efficiency in absorbing pump light and is suitable for InGaAs laser diode pumping.
[0084] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A broadband near-infrared laser crystal of ytterbium-doped silicate mixed crystal, characterized in that: The chemical formula of the broadband near-infrared laser crystal is Yb x Y 2-x Mg y Ca 3-y (SiO4)3, wherein x=0.001~0.20, y=0~3.
2. A method for preparing the broadband near-infrared laser crystal according to claim 1, characterized in that: The following steps are involved: 1) Yb2O3, Y2O3, MgO, CaCO3 and SiO2 are used as raw materials, and the ingredients are prepared and mixed according to the following chemical formula to obtain a mixed material; 0.5xYb2O3 + yMgO + (3 - y)CaCO3 + 0.5(2 - x)Y2O3 + 3SiO2 → Yb x Y 2-x Mg y Ca 3-y (SiO4)3 + (3 - y)CO2↑, where x = 0.001 - 0.20, y = 0 - 3; 2) pressing and calcining the mixed material obtained in step 1) to obtain a calcined material; 3) The calcined material obtained in step 2) is subjected to crystal growth by a melt method to obtain a broadband near-infrared laser crystal.
3. The preparation method according to claim 2, characterized in that: The calcination conditions in step 2) include: a temperature of 1250 to 1400° C. and a time of 10 to 15 hours.
4. The preparation method according to claim 2 or 3, characterized in that: The calcination conditions include: temperature of 1300° C. and time of 12 h.
5. The preparation method according to claim 2, characterized in that: The step 3) melt method comprises: heating to 50-60°C above the melting point, the pulling speed during crystal growth is 1.5-2mm / h, and the rotation speed is 8-12rpm; After the crystal growth is completed, cool at 15-20℃ / h.
6. A method for preparing the broadband near-infrared laser crystal according to claim 1, characterized in that: The following steps are involved: A. Yb2O3, Y2O3, MgO, CaCO3 and SiO2 are used as raw materials, and the ingredients are prepared and mixed according to the following chemical formula to obtain a mixed material; 0.5xYb2O3 + yMgO + (3 - y)CaCO3 + 0.5(2 - x)Y2O3 + 3SiO2 → Yb x Y 2-x Mg y Ca 3-y (SiO4)3 + (3 - y)CO2↑, where x = 0.001 - 0.20, y = 0 - 3; B. Pressing and calcining the mixed material obtained in step A to obtain a calcined material; C. The calcined material obtained in step B is subjected to crystal growth by a melt method to obtain a broadband near-infrared laser crystal.
7. The preparation method according to claim 6, characterized in that: The calcination conditions in step B include: a temperature of 1280 to 1380° C. and a time of 9 to 20 hours.
8. The preparation method according to claim 6, characterized in that: After the calcination, the step B further comprises: grinding, screening and pressing the calcined material, and then calcining to obtain a calcined material; The grinding conditions include: grinding in an agate mortar for 20 to 60 minutes; The screening conditions include: using a standard sorting sieve with a particle size of 20 to 200 meshes to screen the ground powder, and pressing the sieve-down material.
9. The preparation method according to claim 6, characterized in that: The melt method in step C includes any one of a Czochralski method, a laser base heating method, a guided mold method, a pyrolysis method and a heat exchange method.