Method for preparing calcium sulfate whiskers by recycling filtrate
By recycling the normal pressure salt solution method of filtrate, combined with spacer compensation inorganic crystallization agent and acid, the problems of high energy consumption and environmental pollution in the preparation of calcium sulfate whiskers are solved, and high-quality, low-cost calcium sulfate whiskers are achieved. production, promoting industrialization and environmental protection.
Patent Information
- Application Number
- CN202410893693.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-11
AI Technical Summary
When preparing calcium sulfate whiskers in the existing technology, the hydrothermal method consumes high energy and the organic modifier treatment is complicated. The normal pressure salt solution method leads to environmental pollution and increased production costs, and frequent reagent compensation increases the difficulty and cost of the operation.
The normal pressure salt solution method that recycles the filtrate is used. The filtrate obtained through the reaction of the initial normal pressure salt solution method is mixed with desulfurization gypsum, and the inorganic moderator and acid are compensated at intervals. The reaction conditions and pH value are controlled to conduct a second round of normal pressure salt solution. reaction, reducing direct emissions and raw material inputs.
It reduces production costs and avoids environmental pollution. The calcium sulfate whiskers are of high quality, with a length of up to 182 μm and an aspect ratio of 13.8. It reduces the amount of crystal modifier and sulfuric acid, optimizes the process steps, and is suitable for industrial production.
Smart Images

Figure CN118756342A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparing calcium sulfate whiskers, and in particular relates to a method for preparing calcium sulfate whiskers by recycling filtrate. Background Art
[0002] As human beings' requirements for the environment increase, the resource utilization of a large amount of desulfurized gypsum solid waste generated by flue gas desulfurization devices such as coal-fired power plants has attracted the attention of scientific researchers at all levels of industry, academia and research. Among them, converting desulfurized gypsum into high-quality calcium sulfate whiskers through different methods is an important research project. At present, the hydrothermal method is widely used in China to prepare calcium sulfate whiskers. The process has harsh reaction conditions, high energy consumption, and is difficult to mass produce.
[0003] Patent CN101311337B uses hydrochloric acid, nitric acid and the like to control the pH value of the reaction, and uses stearic acid, titanate, tetraethyl orthosilicate, polyvinyl alcohol or phosphate as a modifier to prepare calcium sulfate whiskers with a length of 15 to 240 μm, a diameter of 0.2 to 4 μm and a purity of 98% through hydrothermal crystallization. However, the traditional hydrothermal method for preparing calcium sulfate whiskers in large-scale industrialization consumes a lot of energy, and the many organic modifiers added must be treated as waste liquid, which greatly increases the complexity of the process flow.
[0004] Patent CN102352535B uses a dilute solution of inorganic acid (such as hydrochloric acid or nitric acid) to wash desulfurized gypsum, and after mixed dissolution, adds a crystal conversion agent (such as silane coupling agent KH570, KH560, magnesium salt, citric acid, stearic acid, glycerol, oleic acid, etc.) to separate the solid and liquid, and induces crystallization by cooling, and finally obtains calcium sulfate whiskers after washing and drying. The calcium sulfate whiskers prepared by this method have high purity, good whiteness, regular morphology, less agglomeration, good dispersibility, a primary yield of up to 60%, and a total yield of 95%. However, the process uses excessive inorganic acid for acid dissolution, which will bring about the problem of equipment corrosion, and it is necessary to neutralize or treat the waste acid.
[0005] Patent CN104499041A uses desulfurized gypsum as raw material, aluminum chloride, magnesium chloride, copper chloride, magnesium sulfate, aluminum sulfate (one or two) as crystal mediators to add or compensate, and prepares calcium sulfate whiskers through filtrate clarification, slurry preparation, reagent compensation, hydrothermal reaction, dehydration and drying steps. The diameter of the calcium sulfate whiskers prepared within a certain number of cycles is uniformly distributed, and the surface crystallization is good (diameter 2 to 5 μm, aspect ratio of about 80 to 160). However, in this patent, 20-40% of inorganic crystal mediators and 15-40% of sulfuric acid need to be compensated for each cycle, and the compensation amount is large. In addition, frequent reagent compensation will also increase the difficulty and cost of operation.
[0006] Guan et al. (Chemical Engineering Journal 174 (2011) 296–303) explored the preparation of calcium sulfate whiskers by atmospheric pressure salt solution method and the circulation of its filtrate. After the filtrate was circulated seven times, desulfurized gypsum could still be converted into calcium sulfate whiskers. In a medium-scale experiment, the salt solution could still be used as a crystallization medium for desulfurized gypsum to prepare whiskers after eight cycles and the addition of 20-30% salt in subsequent operations. However, the morphology of the whiskers changed to a certain extent due to the change in the concentration of the circulating filtrate, and the mechanical strength was reduced.
[0007] It can be seen that the atmospheric pressure salt solution method has more advantages than the hydrothermal method and the atmospheric pressure acidification method, but the direct discharge of the high-concentration salt solution it uses will cause pollution to the environment. At the same time, the production cost is greatly increased, which is not conducive to the resource utilization of desulfurization gypsum solid waste.
[0008] In view of this, the present invention is proposed. Summary of the invention
[0009] The object of the present invention is to provide a method for preparing calcium sulfate whiskers by recycling filtrate to solve the above problems.
[0010] In order to achieve the above objectives, the present invention particularly adopts the following technical solutions:
[0011] The present invention provides a method for preparing calcium sulfate whiskers by recycling filtrate, wherein the filtrate obtained by preparing calcium sulfate whiskers by using desulfurized gypsum as raw material and adopting a normal pressure salt solution method is recycled to a reaction process of preparing calcium sulfate whiskers by using desulfurized gypsum as raw material and adopting a normal pressure salt solution method. Preferably, the number of recycling is less than or equal to 8 times, and the quality of calcium sulfate whiskers prepared by desulfurized gypsum is not significantly reduced.
[0012] The method specifically comprises the following steps:
[0013] S1: The product obtained by the initial normal pressure salt solution method reaction is filtered and dehydrated, and the filtrate and the filter cake are collected separately. After the filter cake is dried, calcium sulfate whiskers are obtained. The filtrate is collected separately and clarified, and then mixed with the desulfurized gypsum raw material of the second round of normal pressure salt solution method to obtain a slurry. It should be noted that in each cycle reaction, the added reaction raw materials include desulfurized gypsum; and the final slurry will be compensated with inorganic crystal mediators and acids according to the reaction settings;
[0014] Preferably, an inorganic crystal medium is added to the slurry obtained in S1 at intervals of 1-2 times, and a certain amount of acid is added for reagent compensation.
[0015] The clarification treatment time is not less than 12 hours, preferably 24-48 hours;
[0016] Preferably, the mass concentration of the desulfurized gypsum in the slurry is controlled to be 10%-15%;
[0017] S2: subjecting the slurry to a second round of normal pressure salt solution reaction; the conditions of the second round of normal pressure salt solution reaction are: temperature of 95-105°C; stirring rate of 400-500rpm; reaction time of 240-300min.
[0018] The inorganic crystal medium includes one or more of sodium chloride, magnesium chloride, calcium chloride, magnesium sulfate, and sodium sulfate; the mass of the inorganic crystal medium is 2-6% of the mass of the inorganic crystal medium used in the initial normal pressure salt solution method reaction;
[0019] Furthermore, the inorganic crystallizing agent is of the same type as that used in the initial normal pressure salt solution method reaction.
[0020] The acid includes one or more of acetic acid, oxalic acid, sulfuric acid and hydrochloric acid, and the volume of the acid is 2-6% of the volume of the acid used in the initial normal pressure salt solution method reaction.
[0021] S3: The reaction product of S2 is filtered and dehydrated, and the filtrate and the filter cake are collected separately. After the clarification, the filtrate continues to enter the next round of normal pressure salt solution method reaction for recycling. The filter cake is dried at 60-200° C. for 60-300 min to obtain calcium sulfate whiskers.
[0022] The preparation of the initial reaction solution of the initial normal pressure salt solution method reaction described in the present invention includes: mixing desulfurized gypsum, an inorganic crystal medium, an acid and water to obtain an initial reaction solution; wherein the mass proportion of the desulfurized gypsum in the initial reaction solution is 10%-15%, preferably 12%; the concentration of the inorganic crystal medium is 1-1.5 mol / L; the acid is used as a pH regulator, and its amount is sufficient to adjust the pH of the reaction solution to 2-3.
[0023] When preparing calcium sulfate whiskers, the pH is in the range of 2-3. 2+ 、SO 4 2- The dissolved concentration is higher, and the higher the concentration, the more conducive it is to convert into CaSO 4 Whiskers. For inorganic crystal mediators, MgCl 2 For example, within the appropriate range of Mg 2+ Preferentially adsorbed on the side of the whisker, guiding the CaSO 4 The crystallization is preferentially ordered along the c-axis, promoting and forming calcium sulfate whiskers with a large aspect ratio, while the excess Mg 2+ It will inhibit CaSO 4 The crystal growth of the reaction solution is 2+The concentration and control within a certain range are very important for preparing calcium sulfate whiskers of the same quality. The method of compensating the reagent 1-2 times at intervals in the present invention not only optimizes the process production steps but also can adjust the pH and Mg of the circulating filtrate. 2+ The concentration is controlled within this range. The method for recycling the filtrate of calcium sulfate whiskers prepared from industrial desulfurized gypsum provided by the present invention reduces the environmental pollution caused by the direct discharge of the filtrate generated during the reaction by recycling the filtrate and using desulfurized gypsum as a raw material to continuously synthesize calcium sulfate whiskers by a normal pressure salt solution method, thereby achieving green production and reducing the input of raw materials through the recycling of materials, thereby significantly reducing production costs.
[0024] Beneficial effects of the present invention:
[0025] The method provided by the present invention not only reduces the production cost of preparing calcium sulfate whiskers from desulfurized gypsum, but also avoids the pollution to the environment caused by direct discharge of filtrate. The prepared calcium sulfate whiskers are of high quality. According to the test, the whisker length of the product can reach 182 μm, and the aspect ratio can reach 13.8. The present invention is conducive to promoting environmental protection and promoting the industrialization of calcium sulfate whisker production, bringing significant social and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0027] Figure 1 This is a schematic diagram of the continuous reaction of recycling the filtrate in Example 1;
[0028] Figure 2 This is a SEM image of the calcium sulfate whisker obtained in Example 1;
[0029] Figure 3 This is the SEM image of the calcium sulfate whisker prepared in Example 2. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0031] Example 1
[0032] This embodiment provides a method for preparing calcium sulfate whiskers by recycling filtrate, and the specific steps are:
[0033] The desulfurized gypsum raw material was ground, and the filtrate collected after the initial atmospheric pressure salt solution reaction was clarified for 24 hours to prepare a new reaction slurry and move it into the reaction device; three cycles were carried out with an initial dose of 3.3wt.% of magnesium chloride and 3.8% of the initial volume of oxalic acid at intervals of one cycle. The reaction conditions were: temperature of 105°C, stirring rate of 500rpm, reaction time of 240min, and after the reaction was completed, the filtrate was filtered and dehydrated, and dried at 60°C for 300min to obtain calcium sulfate whiskers. The schematic diagram of the continuous reaction is shown in the figure below. Figure 1 The SEM photo of the prepared calcium sulfate whisker at 500 magnification is shown in Figure 2 shown.
[0034] Through measurement and calculation, the whisker prepared in this embodiment has a length of 182 μm and an aspect ratio of about 13.8.
[0035] Example 2
[0036] This embodiment provides a method for preparing calcium sulfate whiskers by recycling filtrate, and the specific steps are:
[0037] The desulfurized gypsum raw material was ground, and the filtrate collected after the initial normal pressure salt solution reaction was clarified for 24 hours to prepare a new reaction slurry and transfer it into the reaction device; four cycles were carried out in a manner of compensating magnesium chloride with 3.3wt.% of the initial dose and compensating acetic acid with 2% of the initial volume dosage at each cycle interval. The specific reaction conditions were: temperature of 105°C, stirring rate of 500rpm, reaction time of 240min, and after the reaction was completed, the filter was filtered and dehydrated, and the filter cake was dried at 60°C for 300min to obtain calcium sulfate whiskers. The SEM photo of the obtained calcium sulfate whiskers magnified 500 is shown as follows: Figure 3 shown.
[0038] Through measurement and calculation, the whisker prepared in this embodiment has a length of 128 μm and an aspect ratio of about 12.0.
[0039] Depend on Figure 2 and Figure 3 It can be seen that within the number of filtrate cycles specified in the present invention, through reagent compensation, the quality of calcium sulfate whiskers prepared from desulfurized gypsum by a continuous atmospheric pressure salt solution method does not decrease significantly, but is maintained at a good level, with uniform diameter distribution and good surface crystallization.
[0040] Example 3
[0041] The difference from Example 2 is that, after the four cycles of reaction adopted in Example 2, water is added to the obtained slurry to reach the initial reaction volume, and then the fifth cycle is carried out at 105°C and a stirring rate of 500 rpm. After reacting for 240 minutes, the slurry is filtered and dehydrated, and dried at 60°C for 300 minutes to obtain calcium sulfate whiskers.
[0042] Through measurement and calculation, the whisker prepared in this embodiment has a length of 122 μm and an aspect ratio of about 11.8.
[0043] Example 4
[0044] The difference from Example 2 is that the filtrate is circulated 8 times.
[0045] Through measurement and calculation, the whisker prepared in this embodiment has a length of 155 μm and an aspect ratio of about 12.5.
[0046] The method for continuously preparing calcium sulfate whiskers provided by the present invention has uniform diameter distribution of the prepared calcium sulfate whiskers, good surface crystallization, and improved desulfurized gypsum conversion rate; the recycling of the filtrate not only avoids the pollution of the environment caused by its discharge, but also reduces the amount of crystal mediator and sulfuric acid, which is of great significance to environmental protection and the reduction of the production cost of preparing calcium sulfate whiskers from desulfurized gypsum.
[0047] Please note that the technical features of the above embodiments can be combined arbitrarily. In order to make the description concise, all possible combinations of the technical features in the above embodiments are not described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. The above embodiments only express several implementation methods of the present application, and their descriptions are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several variations and improvements can be made, which all belong to the scope of protection of the present application. Therefore, the scope of protection of the patent in this application shall be based on the attached claims.
Claims
1. A method for preparing calcium sulfate whiskers by recycling filtrate, It is characterized in that The method uses the filtrate obtained by using desulfurized gypsum as raw material and adopting the normal pressure salt solution method to prepare calcium sulfate whiskers, and recycles it in the reaction process of also using the desulfurized gypsum as raw material and adopting the normal pressure salt solution method to prepare calcium sulfate whiskers.
2. The method according to claim 1, It is characterized in that The steps include: S1: The product obtained by the initial normal pressure salt solution method reaction is filtered and dehydrated, and the filtrate and the filter cake are collected separately. After the filter cake is dried, calcium sulfate whiskers are obtained. The filtrate is collected separately and clarified, and then mixed with the desulfurized gypsum raw material of the second round of normal pressure salt solution method to obtain a slurry; S2: subjecting the slurry to a second round of normal pressure salt solution reaction; S3: The reaction product of S2 is filtered and dehydrated, and the filtrate and the filter cake are collected separately. After the clarification, the filtrate continues to enter the next round of normal pressure salt solution method reaction for recycling. The filter cake is dried at 60-200° C. for 60-300 min to obtain calcium sulfate whiskers.
3. The method according to claim 2, It is characterized in that The mass concentration of the desulfurized gypsum in the slurry in S1 is controlled to be 10%-15%.
4. The method according to claim 2, It is characterized in that The method further comprises: before the step S3, adding an inorganic crystal medium to the slurry obtained in S1 at intervals of 1-2 times, and adding a certain amount of acid for reagent compensation, and then carrying out the reaction of S3.
5. The method according to claim 4, It is characterized in that The inorganic crystal medium includes one or more of sodium chloride, magnesium chloride, calcium chloride, magnesium sulfate, and sodium sulfate; The acid includes one or more of acetic acid, oxalic acid, sulfuric acid and hydrochloric acid.
6. The method according to claim 4 or 5, It is characterized in that The mass of the inorganic crystal medium is 2-6% of the mass of the inorganic crystal medium used in the initial normal pressure salt solution method reaction.
7. The method according to claim 4 or 5, It is characterized in that The volume of the acid is 2-6% of the volume of the acid used in the initial atmospheric pressure salt solution process reaction.
8. The method according to claim 4, It is characterized in that The inorganic crystal mediator is of the same type as that used in the initial normal pressure salt solution method reaction.
9. The method according to claim 2, It is characterized in that The conditions for the secondary normal pressure salt solution reaction in S2 are: temperature of 95-105° C.; stirring rate of 400-500 rpm; reaction time of 240-300 min.
10. The method according to claim 1, It is characterized in that The number of recycling times is less than or equal to 8 times.