Manufacturing process of anti-perspective regenerated semi-gloss fiber

By using the anti-see-through regenerated semi-optical fiber manufacturing process in textiles, the problem of insufficient shielding properties of light and thin textiles is solved, and fibers with excellent physical and chemical properties and high light-shielding effects are prepared, achieving both lightness and shielding properties, and simplifying the process. and improved production efficiency.

CN118756359AActive Publication Date: 2024-10-11浙江佳人新材料有限公司

Patent Information

Application Number
CN202410759870.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-11
Estimated Expiration
2044-06-13

AI Technical Summary

Technical Problem

Existing light and thin textiles have deficiencies in covering properties, especially products made of white fine fibers. It is difficult to balance lightness and covering properties, resulting in a contradiction between the aesthetics and functionality of clothing.

Method used

Using an anti-see-through regenerated semi-optical fiber manufacturing process, the regenerated semi-dull polyester chips are blended with matte masterbatch, and are prepared through melt extrusion, spinning, post-heating, cooling, pre-networking and drafting and shaping. Fibers with special-shaped cross-sections and excellent physical and chemical properties can achieve matting, anti-transparent, and shading effects.

Benefits of technology

This process successfully improves the shading and opacity of the fiber, while meeting the requirements of thinness and see-through. Compared with traditional methods, the process is simpler and the production efficiency is higher.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756359A_ABST
    Figure CN118756359A_ABST
Patent Text Reader

Abstract

The invention discloses a manufacturing process of anti-perspective regenerated semi-dull fibers, which comprises the following steps of: (a) crystallizing and drying regenerated semi-dull polyester chips, blending the regenerated semi-dull polyester chips with dull master batches through a double-component automatic batching machine, conveying the mixture into a screw extruder for melt extrusion, conveying the melt into a spinning box body, and spinning the melt into a spinning box body; after metering by a metering pump, pressing into a spinning assembly for spinning to form a primary tow; the spinning assembly comprises a spinneret plate, and the section of a discharging hole of the spinneret plate is a special-shaped section. And (b) carrying out post-heating, windless area cooling, circular blowing cooling and bundling oiling treatment on the nascent tows, and then carrying out pre-interlacing, drafting setting and winding to obtain the anti-perspective regenerated semi-gloss fiber with the special-shaped cross section. The preparation method can be used for preparing the fiber with delustering, anti-transparent and shading effects and excellent physical and chemical properties, and meanwhile, the high requirements on light and thin properties, perspectivity and shading properties of fabrics are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyester fibers, and more particularly to a manufacturing process of anti-see-through regenerated semi-optical fibers. Background Art

[0002] With the development of economy, the concepts of low carbon, environmental protection and sustainable development have gradually gained popularity. People have more demands on the functions and characteristics of textiles, and conventional products can no longer meet the needs of the market. Visual shielding is an important function of textiles, which not only affects the application of textiles in real life, but also determines the competitiveness of textiles in the market to a certain extent. In recent years, with the continuous pursuit of personalized textiles and the advantages of thin and light textiles in the market, especially summer clothing, thin and light and comfortable textiles are becoming more and more popular. However, thin and light textiles often have the problem of poor shielding, especially for white fabrics made of fine denier fibers, which makes the contradiction between the aesthetics, lightness and shielding of clothing. This puts forward higher demands on current thin and light textiles-both meeting the requirements of lightness and having good shielding. Therefore, the development of fine denier polyester fibers with anti-see-through and moisture absorption and perspiration functions has a good application prospect. Summary of the invention

[0003] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a manufacturing process for anti-see-through regenerated semi-optical fiber, which can prepare fibers with extinction, anti-see-through, shading effects and excellent physical and chemical properties, while meeting the high requirements for the lightness, see-through and shading properties of the fabric.

[0004] In order to achieve the above object, the present invention adopts the following technical solution:

[0005] A manufacturing process of an anti-see-through regenerated semi-optical fiber comprises the following steps:

[0006] (a) crystallizing and drying the regenerated semi-dull polyester chips, then blending them with the matte masterbatch through a two-component automatic batching machine, conveying the mixture to a screw extruder for melt extrusion, and then conveying the melt to a spinning manifold, and after being metered by a metering pump, pressing the melt into a spinning assembly for spinning to form a primary filament bundle; the spinning assembly includes a spinneret, and the cross-section of the discharge hole of the spinneret is a special-shaped cross-section;

[0007] (b) The spun filament bundle is subjected to post-heating, windless zone cooling, annular air cooling, and bundling oiling treatment, and then pre-networking, drawing and shaping, and winding to obtain a perspective-proof regenerated semi-optical fiber with a special-shaped cross-section.

[0008] Furthermore, the cross section of the discharge hole of the spinneret is W-shaped.

[0009] Furthermore, in step (a), the matte masterbatch is a polyester masterbatch with a titanium dioxide content of 2.5%, and the amount of the matte masterbatch added is 3-6% of the recycled semi-matt polyester chips.

[0010] Furthermore, in step (a), the crystallization temperature is 155-160° C., the drying temperature is 162-168° C., and the drying air pressure is 0.1-0.12 MPa.

[0011] Furthermore, in step (a), the diameter of the screw extruder is 65 mm, the aspect ratio is 25, the heating temperatures of zones 1 to 5 are 272-280°C for zone 1, 280-285°C for zone 2, 280-285°C for zone 3, 285-290°C for zone 4, and 285-290°C for zone 5, respectively; the extrusion pressure of the screw extruder is 10.5-11.5 MPa, and the pressure after filtration is 9-9.7 MPa.

[0012] Furthermore, in step (a), the pump supply of the metering pump is 20-22 g / min, and the spinning temperature is 290-295°C.

[0013] Furthermore, in step (b), the post-heating temperature is 302-308° C., the height of the windless zone is 46 mm, and the wind pressure of the annular air cooling is 37-42 Pa.

[0014] Furthermore, in step (b), the concentration ratio of the oil agent is 11%.

[0015] Furthermore, in step (b), the pre-network pressure is 0.06-0.08Mpa; the rotation speed of the first stretching roller during stretching and shaping is 2500-2700m / min, and the rotation speed of the second stretching roller is 2600-2800m / min; the winding speed during winding shaping is 2500-2750m / min, and the winding tension is 7-9cN.

[0016] The beneficial effects of the present invention are:

[0017] By mixing semi-matt polyester chips with matt masterbatch in proportion, fibers with special cross-sections are obtained through melt spinning and optimization and adjustment of spinning parameters. The fibers have matt, anti-transmission, light-shielding effects and excellent physical and chemical properties, while meeting consumers' requirements for lightness, transparency and light-shielding properties of fabrics. Compared with the existing production method of skin-core structure anti-transmission fibers, the process is simpler and the production efficiency is high. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a schematic cross-sectional view of a spinneret hole of a spinneret in this embodiment;

[0019] Figure 2 This is a schematic structural diagram of the initial state of the oiling device after improvement in Example 2;

[0020] Figure 3 This is a schematic diagram of the structure in which the sealing plate of the oiling device is deflected to one side after improvement of Example 2;.

[0021] Figure 4 This is a schematic structural diagram of the improved oiling device sealing plate deflected to the other side in Example 2;

[0022] Figure numerals: blade 1, oil tank 2, upper chamber 21, lower chamber 22, abutment block 23, oil roller 3, sealing plate 4, oil storage tank 5, limit block 51, cylinder 52, upper conduit 6, lower conduit 7, filter screen 71, sealing plug 8, inclined wall 81, vacuum cleaner 9. DETAILED DESCRIPTION

[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] The manufacturing process of the anti-see-through regenerated semi-optical fiber of the present invention comprises the following steps:

[0025] (a) The regenerated semi-dull polyester chips are crystallized and dried (the crystallization temperature is 155-160° C., the drying temperature is 162-168° C., and the drying air pressure is 0.1-0.12 MPa), and then the chips are blended with the matte masterbatch through a two-component automatic batching machine (the matte masterbatch is a polyester masterbatch with a titanium dioxide content of 2.5%, and the amount of the matte masterbatch added is 3-6% of the regenerated semi-dull polyester chips), and the mixture is transported to a screw extruder for melt extrusion (the diameter of the screw extruder is 65 mm, the aspect ratio is 25, The heating temperatures of zones one to five are 272-280°C for zone one, 280-285°C for zone two, 280-285°C for zone three, 285-290°C for zone four and 285-290°C for zone five, respectively; the extrusion pressure of the screw extruder is 10.5-11.5Mpa, and the pressure after filtration is 9-9.7Mpa). The melt is then transported to the spinning box, and after being metered by a metering pump, is pressed into the spinning assembly for spinning to form a primary filament bundle. The pump supply of the metering pump is 20-22g / min, and the spinning temperature is 290-295°C.

[0026] The spinning assembly includes a spinneret, and the cross section of the discharge hole of the spinneret is a special-shaped cross section. The cross section of the discharge hole of the spinneret is preferably W-shaped, such as Figure 1 As shown, the cross section of the discharge hole of the spinneret includes four leaves (1) connected in a W shape, the angle between two connected leaves (1) is 60°, and the length l of each leaf (1) is 0.28 mm and the width m is 0.07 mm.

[0027] (b) The spun filament bundle is subjected to post-heating, windless zone cooling, annular air cooling, and bundling oiling treatment, and then pre-networking, drawing and shaping, and winding to obtain a perspective-proof regenerated semi-optical fiber with a special-shaped cross-section.

[0028] Among them, the post-heating temperature is 302-308℃, the height of the windless zone is 46mm, the wind pressure of the annular air cooling is 37-42Pa; the oil concentration ratio is 11%; the pre-network pressure is 0.06-0.08Mpa; the speed of the first drafting roller during stretching and shaping is 2500-2700m / min, and the speed of the second drafting roller is 2600-2800m / min; the winding speed during winding forming is 2500-2750m / min, and the winding tension is 7-9cN.

[0029] The method of the present invention obtains fibers with special cross-sections by mixing semi-dull polyester chips with matt masterbatch and melt spinning, so that the fibers have the effects of matt, anti-transmission and light-shielding and excellent physical and chemical properties; this method is different from the existing production method of anti-transmission fibers with skin-core structure and has a simpler process. Preferred specific embodiments are as follows:

[0030] Example 1

[0031] (a) The regenerated semi-dull polyester chips were crystallized and dried (crystallization temperature was 158°C, drying temperature was 165°C, and drying air pressure was 0.1 MPa), and then blended with the matte masterbatch through a two-component automatic batching machine (the matte masterbatch was a polyester masterbatch with a titanium dioxide content of 2.5%, and the amount of the matte masterbatch added was 3.8% of the regenerated semi-dull polyester chips), and the mixture was transported to a screw extruder for melt extrusion (the diameter of the screw extruder was 65 The melt is transported to the spinning box, measured by the metering pump, and pressed into the spinning assembly for spinning to form a primary filament bundle. The pump supply of the metering pump is 21.7 g / min, and the spinning temperature is 290°C.

[0032] The spinning assembly includes a spinneret, and the cross section of the discharge hole of the spinneret is a special-shaped cross section. The cross section of the discharge hole of the spinneret is preferably W-shaped, such as Figure 1 As shown, the cross section of the discharge hole of the spinneret includes four leaves (1) connected in a W shape, the angle between two connected leaves (1) is 60°, and the length l of each leaf (1) is 0.28 mm and the width m is 0.07 mm.

[0033] (b) The spun filament bundle is subjected to post-heating, windless zone cooling, annular air cooling, and bundling oiling treatment, and then pre-networking, drawing and shaping, and winding to obtain a perspective-proof regenerated semi-optical fiber with a special-shaped cross-section.

[0034] Among them, the post-heating temperature is 305°C, the height of the windless zone is 46mm, the wind pressure of the annular air cooling is 40Pa; the oil concentration ratio is 11%; the pre-network pressure is 0.07Mpa; the speed of the first stretching roller during stretching and shaping is 2690m / min, and the speed of the second stretching roller is 2700m / min; the winding speed during winding forming is 2674m / min, and the winding tension is 8cN.

[0035] The performance test results of the fiber prepared in Example 1 are shown in Table 1 (the anti-see-through effect was evaluated using a ColorFlex EZ colorimeter).

[0036] Table 1

[0037] project Measured value Line density 81.28dtex strength 2.21cN / dtex Elongation at break 129.7% Heat stress 48.59cN 60% elongation strength 79.8cN Strip uniformity cv 0.7% Oil content 0.5% Shading rate (white fabric) 92.71% Opacity (white fabric) 99.2%

[0038] Example 2

[0039] The anti-transmission regenerated semi-optical fiber is manufactured according to the method of Example 1, but the traditional oil roller oiling device used in Example 1 is replaced by an improved oiling device.

[0040] The traditional oil roller oiling device is to add oil into the oil tank and immerse the oil over the lower end of the oil roller, and the fiber is oiled from the lower end of the oil roller. However, during the fiber production process, the oil is stored statically in the oil tank, and the oil will precipitate or partially solidify. During the oiling process, the fiber will bring dust, lint and other impurities into the oil, resulting in impurities in the oil, which affects the oiling quality. Although the oil can be circulated to the filter for filtration, as the impurities adsorbed on the filter gradually increase, it will gradually have an adverse effect on the oiling quality, and the filter must be stopped after a period of production to clean the filter, which is not conducive to continuous production and ensuring production efficiency.

[0041] like Figure 2-Figure 4As shown, the oiling device used in the present embodiment comprises an oiling component and two groups of impurity removal components respectively distributed on both sides of the oiling component, the oiling component comprises an oil tank 2, an oil roller 3 rotatably mounted in the inner cavity of the oil tank 2 and a sealing plate 4 movably and sealably embedded in the inner cavity of the oil tank 2, the oil roller is located above the sealing plate 4, the sealing plate 4 is capable of being alternately deflected in a positive and negative direction on a vertical plane, and the sealing plate 4 always separates the inner cavity of the oil tank 2 into an upper chamber 21 and a lower chamber 22 (the sealing plate 4 is preferably made of a hard plate coated with a layer of sealing material (such as rubber), and the sealing plate 4 can always maintain a seal with the inner wall of the oil tank 2 during the deflection process), each group of the impurity removal components comprises an oil storage tank 5, a sealing plug 8 sealably embedded in the inner cavity of the oil storage tank 5 and capable of moving up and down, and a row of upper conduits 6 and a row of lower conduits 7 distributed up and down, each of the lower conduits 7 is installed with a filter screen 71, One end of the upper conduit 6 is communicated with the upper part of the oil storage tank 5, and the other end of the upper conduit 6 is communicated with the upper part of the oil tank 2. One end of the lower conduit 7 is communicated with the middle part of the oil storage tank 5, and the other end of the lower conduit 7 is communicated with the lower part of the oil tank 2. During the deflection of the sealing plate 4, the upper conduit 6 is always communicated with the upper chamber 21. When the sealing plate 4 is deflected, the end of the sealing plate 4 can repeatedly pass through the connection port between the lower conduit 7 and the oil tank 2 up and down, and the end of the sealing plate 4 can deflect downward to a position below the connection port between the lower conduit 7 and the oil tank 2. The sealing plug 8 moves up to the end of the sealing plug 8 close to the upper conduit 6 at the lower end of the connection port between the upper conduit 6 and the oil storage tank 5 (the sealing plug 8 is made of rubber material, the inner walls of the left and right sides of the oil tank 2 are arc-shaped, and the front and rear sides of the oil tank 2 are straight plates. The sealing plug 8 always maintains a seal with the inner walls of the four sides of the oil storage tank 5 when it moves up and down), and a vacuum cleaner 9 is connected to the bottom of the oil tank 2.

[0042] A row of upper conduits 6 is arranged at intervals along the length direction of the oil roller 3. One end of the upper conduit 6 connected to the oil storage tank 5 is higher than the other end of the upper conduit 6 connected to the oil tank 2. The sealing plug 8 includes an inclined wall 81 arranged downward and inclined toward the oil tank 2. When the sealing plug 8 moves to the highest point, the inclined wall 81 has the same inclination as the upper conduit 6 on the same side as the sealing plug 8 moved to the highest point. At the same time, the end of the inclined wall 81 close to the oil tank 2 is lower than the connecting port between the upper conduit 6 and the oil storage tank 5. A limit block 51 is provided in the upper part of the oil storage tank 5, and the sealing plug 8 moves up to abut the limit block 51.

[0043] A row of the down conduits 7 is arranged at intervals along the length direction of the oil roller 3. One end of the down conduit 7 connected to the oil storage tank 5 is lower than the other end of the down conduit 7 connected to the oil tank 2. When one end of the sealing plate 4 deviates to the lowest point, the sealing plate 4 has the same inclination as the down conduit 7 on the same side as the end of the sealing plate 4 deviated to the lowest point, and the end of the sealing plate 4 is lower than the communication port between the down conduit 7 and the oil tank 2. Abutment blocks 23 are provided on both sides of the lower part of the oil tank 2, and the sealing plate 4 deviates downward to abut against the abutment blocks 23.

[0044] Initially, the sealing plate 4 is in a horizontal state, the sealing plug 8 on one side is at the bottom of the oil storage tank 5, and the sealing plug 8 on the other side is upwardly abutted against the limit block 51; the upper chamber 21 is filled with oiling agent, the oiling agent partially immerses the oil roller 3 and the oiling agent liquid level is lower than the connection port between the upper conduit 6 and the oil tank 2, as shown in FIG. Figure 2 After a period of oiling, the oil contains certain impurities, and the motor 24 is started to drive the sealing plate 4 to deflect, so that one end of the sealing plate 4 abuts against the abutment block 23, and the upper chamber 21 is connected with the lower conduit 7 and the oil storage tank 5 located on the same side as the lower end of the sealing plate 4. Part of the oil enters the oil storage tank 5 after being filtered by the filter screen 71 in the lower conduit 7. At this time, the oil in the upper chamber 21 still controls a part of the oil roller 3 to be immersed, as shown in FIG. Figure 3 As shown; when the oil liquid level in the oil storage tank 5 is about 5 cm below the connection port between the lower guide tube 7 and the oil storage tank 5, the sealing plate 4 is reversed, so that one end of the sealing plate 4 is deflected upward, and the other end of the sealing plate 4 is deflected downward to abut against the abutment block 23. At the same time, the cylinder 52 on one side drives the sealing plug 8 to move up to the abutment limit block 51, and the other side ( Figure 4 The cylinder 52 on the right side drives the sealing plug 8 to move downward to abut the bottom of the oil storage tank 5, and the upper chamber 21 becomes connected with the oil storage tank 5 on the other side and is no longer connected with the oil storage tank 5 on the original side. Part of the oil is filtered by the filter screen 71 in the lower conduit 7 and enters the inner cavity of the oil storage tank 5 located above the sealing plug 8 on the other side, while the oil in the oil storage tank 5 on the original side moves upward under the push of the sealing plug 8 and flows back to the upper chamber 21 through the upper conduit 6. The space below the sealing plug 8 of the oil storage tank 5 on the original side is connected with the lower chamber 22. Figure 4 As shown, before the oil liquid level in the oil storage tank 5 on the other side reaches about 5 cm below the connection between the downpipe 7 and the oil storage tank 5, the vacuum cleaner 9 is started to remove impurities from the filter screen 71 in the downpipe 7 on one side. When the oil liquid level in the oil storage tank 5 on the other side reaches about 5 cm below the connection between the downpipe 7 and the oil storage tank 5, the sealing plate 4 is deflected according to the above method, the oil storage tank 5 on one side is used to filter the oil, and the oil storage tank on the other side is vacuum-cleaned. The alternating decontamination reflux of the oil and the alternating decontamination of the two groups of filter screens 71 are achieved by repeatedly and alternately deflecting the sealing plate 4, so that the oil can always be decontaminated during the continuous fiber production process, ensuring the oiling quality and production efficiency.

[0045] The light blocking rate of the white fabric of the fiber of Example 2 is 96.58% and the opacity is 99.9%. After mass production of the same fineness fiber according to the methods of Examples 1 and 2, it is found that under the same production volume, the hair breakage rate of the fiber of Example 1 is 0.97%, while the hair breakage rate of the fiber of Example 2 is 0.52% lower than that of Example 1; at the same time, 30 samples produced at the same time are taken for performance testing, and it is found that the average breaking strength of the fiber samples produced in Example 2 is 0.8 cN / dtex higher than that of Example 1, and the average breaking elongation is 7.03% higher than that of Example 1.

[0046] Comparative Example 1

[0047] Fibers were prepared as in Example 1 except that the spinneret holes had a circular cross section.

[0048] Comparative Example 2

[0049] Fibers were prepared as in Example 2 except that the spinneret holes had a circular cross section.

[0050] Comparative Example 3

[0051] Fibers were prepared as in Example 1 except that the cross-section of the spinneret holes was cross-shaped.

[0052] Comparative Example 4

[0053] Fibers were prepared according to the method of Example 2 except that the cross-section of the spinneret hole was cross-shaped.

[0054] The results show that the shading rates of the fiber white fabrics of Comparative Examples 1-4 are 80.41, 80.37, 87.02, and 88.11%, respectively, and the opacities are 85.6, 85.63, 90.5, and 90.64%, respectively.

[0055] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.

Claims

1. A manufacturing process for anti-see-through regenerated semi-optical fiber, It is characterized in that The following steps are involved: (a) crystallizing and drying the regenerated semi-dull polyester chips, then blending them with the matte masterbatch through a two-component automatic batching machine, conveying the mixture to a screw extruder for melt extrusion, and then conveying the melt to a spinning manifold, and after being metered by a metering pump, pressing the melt into a spinning assembly for spinning to form a primary filament bundle; the spinning assembly includes a spinneret, and the cross-section of the discharge hole of the spinneret is a special-shaped cross-section; (b) The spun filament bundle is subjected to post-heating, windless zone cooling, annular air cooling, and bundling oiling treatment, and then pre-networking, drawing and shaping, and winding to obtain a perspective-proof regenerated semi-optical fiber with a special-shaped cross-section.

2. A process for manufacturing an anti-see-through regenerated semi-optical fiber according to claim 1, It is characterized in that The discharge hole of the spinneret has a W-shaped cross section.

3. The manufacturing process of the anti-see-through regenerated semi-optical fiber according to claim 1, It is characterized in that In step (a), the matt masterbatch is a polyester masterbatch with a titanium dioxide content of 2.5%, and the amount of the matt masterbatch added is 3-6% of the recycled semi-matt polyester chips.

4. The manufacturing process of the anti-see-through regenerated semi-optical fiber according to claim 1, It is characterized in that In step (a), the crystallization temperature is 155-160° C., the drying temperature is 162-168° C., and the drying air pressure is 0.1-0.12 MPa.

5. The manufacturing process of the anti-see-through regenerated semi-optical fiber according to claim 1, It is characterized in that In step (a), the diameter of the screw extruder is 65 mm, the aspect ratio is 25, the heating temperatures of zones 1 to 5 are 272-280° C. for zone 1, 280-285° C. for zone 2, 280-285° C. for zone 3, 285-290° C. for zone 4, and 285-290° C. for zone 5, respectively; the extrusion pressure of the screw extruder is 10.5-11.5 MPa, and the pressure after filtration is 9-9.7 MPa.

6. A process for manufacturing an anti-see-through regenerated semi-optical fiber according to claim 1, It is characterized in that In step (a), the pump supply of the metering pump is 20-22 g / min, and the spinning temperature is 290-295°C.

7. A process for manufacturing an anti-see-through regenerated semi-optical fiber according to claim 1, It is characterized in that In step (b), the post-heating temperature is 302-308° C., the height of the windless zone is 46 mm, and the wind pressure of the annular air cooling is 37-42 Pa.

8. The manufacturing process of the anti-see-through regenerated semi-optical fiber according to claim 1, It is characterized in that In step (b), the concentration ratio of the oil agent is 11%.

9. A process for manufacturing an anti-see-through regenerated semi-optical fiber according to claim 1, It is characterized in that In step (b), the pre-network pressure is 0.06-0.08Mpa; during stretching and shaping, the rotation speed of the first stretching roller is 2500-2700m / min, and the rotation speed of the second stretching roller is 2600-2800m / min; during winding and shaping, the winding speed is 2500-2750m / min, and the winding tension is 7-9cN.

Citation Information

Patent Citations

  • Spinning method of regenerated polyester full-dull FDY filaments

    CN111005076A

  • Full-dull lightweight moisture-absorption quick-drying polyester fiber and preparation method thereof

    CN111254504A

  • Production method of moisture-absorbing, sweat-releasing, ice-cold and anti-ultraviolet DTY (Draw Textured Yarn)

    CN113106565A

  • Polyester complete extinction superfine denier POY fiber and production method thereof

    CN113737292A

  • Preparation method of coarse-denier non-crimp dumbbell-shaped full-dull polyester staple fiber

    CN115976667A

Cited By

  • Preparation method and application of water traceless fiber

    CN119685964A