Flame-retardant PTT polyester fiber and production method thereof

By modifying phosphorus-containing flame retardants and cutinase pretreatment technology, combined with supercritical CO2 fluid treatment, the problem of insufficient flame retardant performance and heat resistance of existing flame-retardant PTT polyester fibers has been solved, and the flame retardancy of the fibers has been significantly improved. Performance and mechanical properties, suitable for textile and clothing fields.

CN118756368AInactive Publication Date: 2024-10-11YANCHENG LONGJIANG TEXTILE CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411002615.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing flame-retardant PTT polyester fiber has insufficient flame retardant performance and heat resistance. The main chain phosphorus flame retardant is easily thermally oxidized during use, causing the polyester macromolecular chain to break, increasing the possibility of melting droplets, and the char-forming effect is not good. good.

Method used

The modified phosphorus-containing flame retardant DDP is reacted with ethylene glycol to prepare a side-chain phosphorus flame retardant, and combined with cutinase pretreatment of PTT polyester and polyether ester masterbatch for screw extrusion spinning, and supercritical CO2 Fluid treatment improves the mechanical properties and flame retardancy of the fibers.

Benefits of technology

It improves the flame retardant and heat-resistant properties of the fiber, enhances the tensile strength and mechanical properties of the fiber, reduces process energy consumption, is environmentally friendly, and broadens the application market in the textile and clothing field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756368A_ABST
    Figure CN118756368A_ABST
Patent Text Reader

Abstract

The invention discloses a flame-retardant PTT polyester fiber and a production method thereof, and relates to the technical field of high polymer materials, and the flame-retardant PTT polyester fiber comprises the following raw materials in parts by weight: 80-95 parts of PTT polyester, 2.5-8 parts of a modified phosphorus-containing flame retardant, 4-10 parts of polyether ester master batch, 0.1-0.5 part of a stabilizer and 0.1-0.5 part of an antioxidant. According to the flame-retardant PTT polyester fiber and the production method thereof, PTT polyester is pretreated through cutinase, ester bonds on the PTT polyester fiber are hydrolyzed to generate hydrophilic groups, the hydrophilic modification effect is achieved on the basis that the advantage performance of the fiber is kept unchanged, the additional value of the fiber is increased, and the application market of the fiber in the textile and garment field is widened; meanwhile, as cutinase has specificity, high efficiency, mildness and biodegradability, the cutinase is environment-friendly, energy consumption in the technological process is reduced, and the cutinase is green, environment-friendly and pollution-free.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, in particular to a flame-retardant PTT polyester fiber and a production method thereof. Background Art

[0002] Polytrimethylene terephthalate (PTT), as a new polyester polymer material with excellent comprehensive properties, has been widely used in the fields of fibers, films, engineering plastics, etc. However, the use of PTT alone has problems such as poor flame retardancy, poor heat resistance, and low dimensional stability, which limits its application.

[0003] The Chinese patent with publication number CN104862813A discloses a flame retardant PTT polyester fiber and a preparation method thereof, wherein the components are as follows by mass percentage: PTT 80% to 95%, flame retardant monomer 2% to 8%, polyethylene glycol 2% to 6%, benzyl silicone 0.5% to 2%, potassium perfluorobutyl sulfonate 0.1% to 0.5%, stabilizer 0.1% to 0.5%, antioxidant 0.1% to 0.5%, lubricant 0.1% to 1%, the PTT is polytrimethylene terephthalate with an intrinsic viscosity of 0.7 to 0.9 dL / g prepared from terephthalic acid and 1,3-propylene glycol, and the flame retardant monomer is 2-hydroxyethyl (phenyl) phosphinic acid. The beneficial effect of the present invention is that the present invention has excellent flame retardant properties and heat resistance, its limiting oxygen index can reach more than 38%, and it is soft to the touch, strong in wearability, and suitable for the field of textile fibers. However, the above technical solution has the following shortcomings: 2-hydroxyethyl (phenyl) phosphinic acid is used as a flame retardant, which belongs to a phosphorus-based flame retardant with a main chain structure. This type of flame retardant is prone to thermal oxidation degradation of the phosphorus structure in the main chain during use, resulting in the breakage of the polyester macromolecular chain, thereby increasing the possibility of polyester producing droplets, resulting in poor charring effect, and the flame retardant performance needs to be improved; therefore, the present invention provides a flame-retardant PTT polyester fiber and a production method thereof to solve the above problems. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a flame-retardant PTT polyester fiber and a production method thereof, which solves the problems mentioned in the above background technology.

[0005] To achieve the above objectives, the present invention is implemented through the following technical scheme: a flame retardant PTT polyester fiber, comprising the following raw materials in parts by weight: 80 to 95 parts of PTT polyester, 2.5 to 8 parts of modified phosphorus-containing flame retardant, 4 to 10 parts of polyether ester masterbatch, 0.1 to 0.5 parts of stabilizer, and 0.1 to 0.5 parts of antioxidant.

[0006] Preferably, the stabilizer is one of trimethyl phosphate or triphenyl phosphate, and the antioxidant is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate].

[0007] Preferably, the specific preparation method of the modified phosphorus-containing flame retardant is: nitrogen is introduced into a four-necked flask, ethylene glycol and DDP are added, and the reaction is carried out under normal pressure; after the reaction is completed, the temperature is increased, and the residual ethylene glycol and water are distilled off under reduced pressure to obtain the modified phosphorus-containing flame retardant.

[0008] Preferably, the molar ratio of ethylene glycol to DDP is (2.3-2.5):1.

[0009] Preferably, the reaction temperature of the ethylene glycol and DDP is 160-180° C., and the reaction time is 6-6.5 h; after the reaction is completed, the temperature is raised to 190-200° C.

[0010] A method for producing a flame-retardant PTT polyester fiber comprises the following preparation steps:

[0011] Step 1: Place the pretreated PTT polyester in a drying oven at 110-120°C and dry for 24-28 hours;

[0012] Step 2: Place the polyetherester masterbatch in a drying oven at 90-100°C for 1.5-2.5 hours, then evacuate and heat to 105-108°C for 3.5-4 hours;

[0013] Step 3, slicing the dried PTT polyester and polyether ester masterbatch;

[0014] Step 4: Add the sliced ​​PTT polyester and polyether ester masterbatch, modified phosphorus-containing flame retardant, stabilizer and antioxidant into a screw extruder, melt and spin to obtain flame-retardant PTT polyester fiber.

[0015] Preferably, in step 4, the melt temperature of spinning is 245-255° C., the winding speed is 500-4000 m / min, the heat setting temperature is 80-150° C., and the drafting multiple is 2-5 times.

[0016] Preferably, in step 1, the pretreatment method of PTT polyester is:

[0017] S1. Add cutinase to the buffer and raise the temperature to 50-60°C;

[0018] S2, placing the PTT polyester in the mixed solution and immersing it for 22 to 24 hours;

[0019] S3, then washing with 1g / L Na2CO3 and deionized water in turn;

[0020] S4, dry at room temperature;

[0021] Wherein, in S1, the pH of the buffer solution is 8, and the buffer solution is a mixture of 0.05 mol / L Tris solution and 0.05 mol / L HCl solution.

[0022] Preferably, the method for producing the flame retardant PTT polyester fiber further comprises:

[0023] Ⅰ. Put the flame-retardant PTT polyester fiber prepared in step 4 into a high-pressure reactor and seal it;

[0024] Ⅱ. Pass CO2 to clean the high pressure axe 2 to 4 times;

[0025] III. Raise the temperature to a constant temperature for reaction, at which time the high pressure axe automatically increases the pressure;

[0026] IV. Then stir under constant temperature and pressure conditions, and finally convert the autoclave to normal pressure, and the treatment is completed.

[0027] Preferably, in III, the pressure is increased to 20-30 MPa and the constant temperature is 75-80°C. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The present invention provides a fiber cross-section SEM photograph of a flame-retardant PTT polyester fiber and a production method thereof.

[0029] Beneficial Effects

[0030] The present invention provides a flame retardant PTT polyester fiber and a production method thereof. Compared with the prior art, the present invention has the following beneficial effects:

[0031] (1) The flame-retardant PTT polyester fiber and its production method pre-treat PTT polyester with cutinase, so that the ester bonds on the PTT polyester fiber are hydrolyzed to generate hydrophilic groups, and the hydrophilic modification effect is achieved on the basis of maintaining the advantageous properties of the fiber itself, which is beneficial to improving the added value of the fiber and broadening its application market in the field of textiles and clothing; at the same time, because the cutinase itself is specific, efficient, mild and biodegradable, it is environmentally friendly, reduces the energy consumption of the process, and is green, environmentally friendly and pollution-free; at the same time, polyether ester itself is added to the polyester fiber as an elastomer, which can effectively improve the tensile strength of the fiber.

[0032] (2) The flame-retardant PTT polyester fiber and its production method are prepared by subjecting the prepared flame-retardant PTT polyester fiber to supercritical CO2 fluid treatment. Since the process has a strong penetration effect on non-polar or hydrophobic fibers, it has good diffusion properties in the fibers and can easily penetrate into the fibers to cause them to swell, affecting the interaction force between the fiber macromolecules, resulting in changes in the supramolecular structure such as fiber orientation and crystallinity, thereby improving the mechanical properties of the fibers.

[0033] (2) The flame-retardant PTT polyester fiber and its production method are characterized by adding DDP as a flame retardant, which is a side chain phosphorus flame retardant. The phosphorus element appears in the side group, and by modifying it, when the material is thermally decomposed, the breaking of the P-0 bond will not affect the structure of the main chain. On the contrary, the breaking of the side chain has a certain protective effect on the main chain structure, thereby improving the flame retardant properties of the polyester fiber. DETAILED DESCRIPTION

[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] In the present technical scheme, the preparation method of PTT polyester is as follows: a certain amount of reactants terephthalic acid, 1,3-propylene glycol, catalyst Ti(0Bu)4+Sb203, and antioxidant triphenylphosphine are added into a reactor, and then nitrogen is introduced for 30 minutes, the air in the reactor is discharged, the temperature is raised to 230°C for pre-condensation for 3 hours, and at the same time, the water and unreacted small molecule alcohols produced in the reaction system are pumped out with a water pump, and the temperature is continued to be raised to 255°C for condensation reaction for 3 hours to obtain PTT polyester.

[0036] Example 1

[0037] A method for producing a flame-retardant PTT polyester fiber comprises the following preparation steps:

[0038] Step 1, pre-treating the PTT polyester: adding cutinase to a mixture of a 0.05 mol / L Tris solution and a 0.05 mol / L HCI solution at pH 8, heating to 50° C., and then placing the PTT polyester in the mixed solution, immersing for 22 hours, washing once with 1 g / L Na2CO3, and then washing twice with deionized water, and drying at room temperature;

[0039] Step 2: Place 80 g of the pretreated PTT polyester in a drying oven at 110° C. and dry for 24 hours;

[0040] Step 3: Place 10 g of polyetherester masterbatch in a drying oven at 90°C for 1.5 h, then evacuate and heat to 105°C for 3.5 h;

[0041] Step 4: Slice the dried PTT polyester and polyether ester masterbatch;

[0042] Step 5: adding the sliced ​​PTT polyester and polyether ester masterbatch, 8 g of modified phosphorus-containing flame retardant, 0.5 g of trimethyl phosphate and 0.5 g of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] into a screw extruder, and melting and spinning to obtain flame-retardant PTT polyester fiber;

[0043] The specific preparation method of the modified phosphorus-containing flame retardant is as follows: nitrogen is introduced into a four-necked flask, and then ethylene glycol and DDP are added in a molar ratio of 2.3:1, and reacted at 160°C for 6 hours under normal pressure; after the reaction is completed, the temperature is raised to 190°C, and the residual ethylene glycol and water are distilled off under reduced pressure to obtain the modified phosphorus-containing flame retardant;

[0044] Step six, place the flame-retardant PTT polyester fiber prepared in step five into a high-pressure reactor and seal it, then pass CO2 to clean the high-pressure reactor twice, and then heat it to a constant temperature of 7°C for reaction. At this time, the high-pressure reactor is automatically pressurized to 20MPa, and then stirred under constant temperature and pressure conditions. Finally, the autoclave is converted to normal pressure and the treatment is completed.

[0045] Example 2

[0046] A method for producing a flame-retardant PTT polyester fiber comprises the following preparation steps:

[0047] Step 1, pre-treating the PTT polyester: adding cutinase to a mixture of a 0.05 mol / L Tris solution and a 0.05 mol / L HCI solution at a pH of 8, heating to 55° C., and then placing the PTT polyester in the mixed solution, immersing for 23 hours, washing once with 1 g / L Na2CO3, and then washing twice with deionized water, and drying at room temperature;

[0048] Step 2: Place 85 g of the pretreated PTT polyester in a drying oven at 115° C. and dry for 26 hours;

[0049] Step 3: Place 7 g of polyether ester masterbatch in a drying oven at 95°C for 2 hours, then evacuate the oven, and heat to 106°C for 4 hours;

[0050] Step 4: Slice the dried PTT polyester and polyether ester masterbatch;

[0051] Step 5: adding the sliced ​​PTT polyester and polyether ester masterbatch, 5 g of modified phosphorus-containing flame retardant, 0.3 g of triphenyl phosphate and 0.3 g of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] into a screw extruder, and melting and spinning to obtain flame-retardant PTT polyester fiber;

[0052] The specific preparation method of the modified phosphorus-containing flame retardant is as follows: nitrogen is introduced into a four-necked flask, and then ethylene glycol and DDP are added in a molar ratio of 2.4:1, and reacted at 170°C for 6.5 hours under normal pressure; after the reaction is completed, the temperature is raised to 195°C, and the residual ethylene glycol and water are distilled off under reduced pressure to obtain the modified phosphorus-containing flame retardant;

[0053] Step six, place the flame-retardant PTT polyester fiber prepared in step five into a high-pressure reactor and seal it, then pass CO2 to clean the high-pressure reactor three times, and then heat it to a constant temperature of 80°C for reaction. At this time, the high-pressure reactor is automatically pressurized to 25MPa, and then stirred under constant temperature and pressure conditions. Finally, the autoclave is converted to normal pressure and the treatment is completed.

[0054] Example 3

[0055] A method for producing a flame-retardant PTT polyester fiber comprises the following preparation steps:

[0056] Step 1, pre-treating the PTT polyester: adding cutinase to a mixture of a 0.05 mol / L Tris solution and a 0.05 mol / L HCI solution at a pH of 8, heating to 60° C., and then placing the PTT polyester in the mixed solution, immersing for 24 hours, first washing once with 1 g / L Na2CO3, then washing twice with deionized water, and drying at room temperature;

[0057] Step 2: Place 95 g of the pretreated PTT polyester in a drying oven at 120° C. and dry for 28 hours;

[0058] Step 3: Place 4 g of polyetherester masterbatch in a drying oven at 100°C for 2.5 hours, then evacuate and heat to 108°C for 4 hours;

[0059] Step 4: Slice the dried PTT polyester and polyether ester masterbatch;

[0060] Step 5: adding the sliced ​​PTT polyester and polyether ester masterbatch, 2.5 g of modified phosphorus-containing flame retardant, 0.1 g of trimethyl phosphate and 0.1 g of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] into a screw extruder, and melting and spinning to obtain flame-retardant PTT polyester fiber;

[0061] The specific preparation method of the modified phosphorus-containing flame retardant is as follows: nitrogen is introduced into a four-necked flask, and then ethylene glycol and DDP are added in a molar ratio of 2.5:1, and reacted at 180°C for 6.5 hours under normal pressure; after the reaction is completed, the temperature is raised to 200°C, and the residual ethylene glycol and water are distilled off under reduced pressure to obtain the modified phosphorus-containing flame retardant;

[0062] Step six, place the flame-retardant PTT polyester fiber prepared in step five into a high-pressure reactor and seal it, then pass CO2 to clean the high-pressure reactor 4 times, and then heat it to a constant temperature of 80°C for reaction. At this time, the high-pressure reactor is automatically pressurized to 30MPa, and then stirred under constant temperature and pressure conditions. Finally, the autoclave is converted to normal pressure and the treatment is completed.

[0063] Comparative Example 1

[0064] A method for producing a flame-retardant PTT polyester fiber comprises the following preparation steps:

[0065] Step 1, pre-treating the PTT polyester: adding cutinase to a mixture of a 0.05 mol / L Tris solution and a 0.05 mol / L HCI solution at pH 8, heating to 50° C., and then placing the PTT polyester in the mixed solution, immersing for 22 hours, washing once with 1 g / L Na2CO3, and then washing twice with deionized water, and drying at room temperature;

[0066] Step 2: Place 80 g of the pretreated PTT polyester in a drying oven at 110° C. and dry for 24 hours;

[0067] Step 3: Place 10 g of polyetherester masterbatch in a drying oven at 90°C for 1.5 h, then evacuate and heat to 105°C for 3.5 h;

[0068] Step 4: Slice the dried PTT polyester and polyether ester masterbatch;

[0069] Step 5: adding the sliced ​​PTT polyester and polyether ester masterbatch, 8 g of modified phosphorus-containing flame retardant, 0.5 g of trimethyl phosphate and 0.5 g of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] into a screw extruder, and melting and spinning to obtain flame-retardant PTT polyester fiber;

[0070] Among them, the specific preparation method of the modified phosphorus-containing flame retardant is: nitrogen is introduced into a four-necked flask, and then ethylene glycol and DDP are added in a molar ratio of 2.3:1, and react at a temperature of 160°C for 6 hours under normal pressure conditions; after the reaction is completed, the temperature is raised to 190°C, and the residual ethylene glycol and water are distilled off under reduced pressure to obtain the modified phosphorus-containing flame retardant.

[0071] Comparative Example 2

[0072] A method for producing a flame-retardant PTT polyester fiber comprises the following preparation steps:

[0073] Step 1: Place 80 g of PTT polyester in a drying oven at 110° C. and dry for 24 hours;

[0074] Step 2: Place 10 g of polyetherester masterbatch in a drying oven at 90°C for 1.5 h, then evacuate and heat to 105°C for 3.5 h;

[0075] Step 3, slicing the dried PTT polyester and polyether ester masterbatch;

[0076] Step 4: Add the sliced ​​PTT polyester and polyether ester masterbatch, 8 g of 2-carboxyethyl-phenyl hypophosphorous acid, 0.5 g of trimethyl phosphate and 0.5 g of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] into a screw extruder and melt-spin to obtain flame-retardant PTT polyester fiber.

[0077] Tensile performance test: in accordance with GB / T3916-2013, the clamping distance is 250mm, the tensile speed is 250mm / min, the pre-tension is 0.05+0.01cN / dtex, the test temperature is 20°C, the humidity is 65%RH, the experiment is repeated 15 times and the average value is calculated; the sample size is 100mm×20mm; the results are shown in Table 1.

[0078] Contact angle measurement: The sample was equilibrated in a constant temperature and humidity chamber at 20°C and 65% relative humidity for 24 hours, and then the contact angle of the water droplet on the sample surface was measured using a drop shape analyzer; the results are shown in Table 1.

[0079] Air permeability test: The air permeability tester produced by Wenzhou Fangyuan Instrument Co., Ltd. was used for the test. First, the air pump and computer software were turned on. The test was carried out according to GB / T5453:1997. The sample pressure difference was set to 100Pa and the sample area was 20cm. 2 , and then lay the sample flat, the instrument automatically selects the appropriate orifice plate for testing, moves the sample position after the test is completed, repeats the test 10 times, and calculates the average value; the results are shown in Table 1.

[0080] Limiting oxygen index (LOI) test: According to GB / T2406.2-2009 Determination of combustion behavior of plastics by oxygen index method, the limiting oxygen index of the flame retardant polyester strips was tested. After the samples were vacuum dried at 120°C for 24 hours, they were tested using an intelligent oxygen index tester. The sample size was 100mm×10mm×4mm. The results are shown in Table 1.

[0081] Vertical combustion test: The test is carried out according to the standard UL-94. The test method is as follows: The test method is to fix the sample vertically on the sample clamp, the clamped part of the upper end of the sample is 6mm, the distance between the lower end of the sample and the horizontally laid 6mm thick absorbent cotton is 300mm, and a Bunsen burner with a flame height of 20mm and a blue flame is used to apply flame to the sample at a distance of 150mm from the bottom end of the sample for 10s and then remove the flame, record the flame burning time of the sample, after the flame burning of the sample is extinguished, apply flame again for 10s according to the above method, and record the flame burning and flameless burning time of the sample after removing the flame; the size of the sample is 125mm×13mm×3.2mm; the results are shown in Table 1.

[0082] Table 1

[0083]

[0084] As can be seen from Table 1, the mechanical properties, flame retardant properties and air permeability of samples 1-3 are significantly improved compared with those of comparative examples 1-2.

[0085] like Figure 1 As shown, in Comparative Example 2, the particles are unevenly distributed in the PTT, and there is no obvious stratification phenomenon in the cross section, and there are concave-convex changes, indicating that the fiber has undergone tough fracture; in Comparative Example 1, it can be seen that the particles are scattered and the cracks in the cross section become dense. The dense cracks can make the spline withstand higher energy impact. Therefore, compared with Comparative Example 2, the toughness of the sample in Comparative Example 1 is increased, and its impact resistance is improved; there are no obvious particles in the cross section of Example 1, and the surface is uneven with a more obvious yield phenomenon. Therefore, compared with Comparative Examples 1-2, the toughness of the sample in Example 1 is significantly improved.

[0086] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art.

[0087] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0088] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A flame retardant PTT polyester fiber, It is characterized in that The invention comprises the following raw materials in parts by weight: 80-95 parts of PTT polyester, 2.5-8 parts of modified phosphorus-containing flame retardant, 4-10 parts of polyether ester masterbatch, 0.1-0.5 parts of stabilizer and 0.1-0.5 parts of antioxidant.

2. The flame retardant PTT polyester fiber according to claim 1, Features: The stabilizer is one of trimethyl phosphate and triphenyl phosphate, and the antioxidant is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate.

3. The flame retardant PTT polyester fiber according to claim 1, Features: The specific preparation method of the modified phosphorus-containing flame retardant is as follows: nitrogen is introduced into a four-necked flask, ethylene glycol and DDP are added, and the reaction is carried out under normal pressure; after the reaction is completed, the temperature is increased, and the residual ethylene glycol and water are distilled off under reduced pressure to obtain the modified phosphorus-containing flame retardant.

4. The flame retardant PTT polyester fiber according to claim 3, Features: The molar ratio of ethylene glycol to DDP is (2.3-2.5):

1.

5. The flame retardant PTT polyester fiber according to claim 3, Features: The reaction temperature of ethylene glycol and DDP is 160-180° C., and the reaction time is 6-6.5 hours. After the reaction is completed, the temperature is raised to 190-200° C.

6. A method for producing the flame-retardant PTT polyester fiber according to claim 1, It is characterized in that The method comprises the following preparation steps: Step 1: Place the pretreated PTT polyester in a drying oven at 110-120°C and dry for 24-28 hours; Step 2: Place the polyetherester masterbatch in a drying oven at 90-100°C for 1.5-2.5 hours, then evacuate and heat to 105-108°C for 3.5-4 hours; Step 3, slicing the dried PTT polyester and polyether ester masterbatch; Step 4: Add the sliced ​​PTT polyester and polyether ester masterbatch, modified phosphorus-containing flame retardant, stabilizer and antioxidant into a screw extruder, melt and spin to obtain flame-retardant PTT polyester fiber.

7. The method for producing a flame-retardant PTT polyester fiber according to claim 6, Features: In the step 4, the melt temperature of spinning is 245-255° C., the winding speed is 500-4000 m / min, the heat setting temperature is 80-150° C., and the drafting multiple is 2-5 times.

8. The method for producing a flame-retardant PTT polyester fiber according to claim 6, Features: In the step 1, the pretreatment method of PTT polyester is: S1. Add cutinase to the buffer and raise the temperature to 50-60°C; S2, placing the PTT polyester in the mixed solution and immersing it for 22 to 24 hours; S3, then use 1g / L Na 2 CO 3 and washing with deionized water; S4, dry at room temperature; Wherein, in S1, the pH of the buffer solution is 8, and the buffer solution is a mixture of 0.05 mol / L Tris solution and 0.05 mol / L HCl solution.

9. The method for producing a flame-retardant PTT polyester fiber according to claim 6, Features: The production method of the flame-retardant PTT polyester fiber also includes: Ⅰ. Put the flame-retardant PTT polyester fiber prepared in step 4 into a high-pressure reactor and seal it; II. Introduction of CO 2 Clean the high pressure axe 2 to 4 times; III. Raise the temperature to a constant temperature for reaction, at which time the high pressure axe automatically increases the pressure; IV. Then stir under constant temperature and pressure conditions, and finally convert the autoclave to normal pressure, and the treatment is completed.

10. The method for producing a flame-retardant PTT polyester fiber according to claim 9, Features: In the above III, the pressure is increased to 20-30 MPa and the constant temperature is 75-80°C.

Citation Information

Patent Citations

  • Method for improving mechanical properties of aramid fiber in supercritical fluid through stretching orientation

    CN103469602A

  • Antistatic PTT / TPEE composite fiber and preparation method thereof

    CN104846481A

  • Flame-retardant polyolefin compound and preparation method thereof

    CN107304268A

  • Flame-retardant polyester roller shutter fabric and preparation method thereof

    CN112281277A

  • High-elasticity wear-resistant knitted jean fabric and preparation method thereof

    CN112458758A