Structural color textile fabric with excellent antibacterial performance and preparation method thereof
By using PDA@Ag@SiO2 microspheres to self-assemble on structural color textile fabrics to form an amorphous photonic crystal coating, the problem of insufficient fabric stability and antibacterial performance is solved, and high color fastness and antibacterial performance are achieved. It is suitable for For the development of green smart textile fabrics.
Patent Information
- Application Number
- CN202410958418.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-11
Smart Images

Figure CN118756491A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of functional fabrics, and particularly relates to a structural color textile fabric with excellent antibacterial performance and a preparation method thereof. Background Art
[0002] There are two main ways to color textile fabrics. The first is pigment coloring, which is to produce color by applying dyes or pigments to the fabrics; the second is structural coloring, which uses special ordered structures (such as photonic crystal structures) to produce visual effects through selective reflection phenomena such as scattering and diffraction of light.
[0003] Compared with traditional dyeing technology, structural color is an eco-friendly bionic coloring technology that saves energy and reduces emissions. It can replace traditional high-pollution dyeing methods. Although the current research on photonic crystal structural colors has achieved good coloring effects on fabrics, the stability of the obtained structural colors on fabrics is very poor. Under simple external forces such as immersion, bending, friction, and washing, the structural colors on the fabrics are prone to deformation, cracks, or even disappearance. Therefore, it is crucial to improve the stability of photonic crystal structural colors on fabrics.
[0004] Introducing polydopamine (PDA) into traditional structural color materials is an important way to solve the above problems. PDA has good biocompatibility, contains many phenolic hydroxyl groups and nitrogen-containing functional groups, and can adhere to the surface of almost all materials to form a uniform nanofilm. In addition, PDA, a black substance, can absorb background stray light, and its introduction can improve the color saturation of structural colors.
[0005] As we all know, silver nanoparticles (Ag NPs) are a good inorganic antibacterial agent with strong bactericidal activity against a variety of bacteria, and also have excellent properties in conductivity, antistatic, and UV resistance. The most prominent problem of Ag NPs in antibacterial finishing of fabrics is the lack of adhesion to the fibers, resulting in poor washing resistance of antibacterial fabrics. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a structural color textile fabric with excellent antibacterial properties and a preparation method thereof. The fabric has high color fastness and excellent antibacterial properties, providing a new idea for the development of green and new intelligent textile fabrics.
[0007] The invention provides a structural color textile fabric with excellent antibacterial performance, which is obtained by depositing PDA@Ag@SiO2 microspheres on the surface of the fabric modified by a silane coupling agent through self-assembly to form an amorphous photonic crystal coating.
[0008] Preferably, the PDA@Ag@SiO2 microspheres are obtained by introducing polydopamine on the outer layer of silica microspheres to obtain PDA@SiO2 microspheres; and then loading nanosilver on the surface of the microspheres by in-situ reduction.
[0009] Preferably, the fabric includes cotton fabric, cotton fiber or a blended fabric thereof.
[0010] The present invention also provides a method for preparing a structural color textile fabric with excellent antibacterial performance, comprising the following steps:
[0011] (1) preparing silica nanoparticle powder; adding tris(hydroxymethylaminomethane) Tris to water, dissolving it and adjusting the pH to 8-9; then adding dopamine hydrochloride and mixing well to obtain a mixed solution; adding silica nanoparticle powder to the mixed solution under nitrogen protection, stirring at room temperature, and after the reaction is completed, centrifuging, washing and drying to obtain PDA@SiO2 nanoparticle powder;
[0012] (2) adding ethanol to water, mixing evenly, adding silver nitrate and the PDA@SiO2 nanoparticle powder in step (1), and dispersing by ultrasonication at room temperature to obtain a PDA@Ag@SiO2 suspension solution for later use;
[0013] (3) The PDA@Ag@SiO2 suspension solution in step (2) is dropped onto the surface of the fabric modified with a silane coupling agent to form an amorphous photonic crystal coating, which is then dried to obtain a structural color textile fabric with excellent antibacterial properties.
[0014] Preferably, the preparation steps of the silica nanoparticle powder in step (1) are as follows: ethanol and ammonia water are added to water, mixed evenly and nitrogen is introduced, then heated in a water bath to 70-80° C., after standing, ethyl orthosilicate is added to react for 4-6 hours, and after the reaction is completed, centrifugation and washing are performed to obtain the silica nanoparticle powder.
[0015] Preferably, the molar amount of tris(hydroxymethyl)aminomethane in step (1) is 10-15 mol% of the molar amount of water; the molar amount of dopamine hydrochloride is 1-10 mol% of the molar amount of water; and the mass of the silica nanoparticles is 3-10 wt% of the mass of water.
[0016] Preferably, in step (1), stirring is performed at room temperature for 6-12 hours.
[0017] Preferably, the mass of ethanol in step (2) is 50-55wt% of the mass of water; the mass of silver nitrate is 3-10wt% of the mass of the water / ethanol mixed solution; the mass of the nanoparticle PDA@SiO2 is 3-10wt% of the mass of the water / ethanol mixed solution.
[0018] Preferably, the ultrasonic dispersion time in step (2) is 10-30 min.
[0019] Preferably, the silane coupling agent in step (3) is γ-aminopropyltriethoxysilane, and the mass of the silane coupling agent is 3-10 wt % of the mass of water.
[0020] Preferably, the modification temperature of the fabric modified with the silane coupling agent in step (3) is 50-70° C., and the modification time is 6-12 h.
[0021] Preferably, the drying temperature in step (3) is 50-70°C.
[0022] The principle of the present invention is:
[0023] The present invention designs a structural color textile fabric with excellent antibacterial properties based on structural color textile fabrics: the first step is to prepare monodisperse nano silicon dioxide (SiO2) microspheres, and coat the microspheres with dopamine (PDA) to obtain PDA@SiO2 microspheres; the second step is to load nano silver (Ag) on the surface of PDA@SiO2 microspheres by in-situ reduction to obtain PDA@Ag@SiO2 microspheres; the third step is to self-assemble PDA@Ag@SiO2 microspheres onto the surface of cotton fabric modified with γ-aminopropyltriethoxysilane by drop coating to form an amorphous photonic crystal coating. Finally, a non-anisotropic structural color textile fabric with high color fastness and high level of antibacterial properties is obtained.
[0024] In the first step, silica SiO2 microspheres can be used to color the surface of cotton fabrics with structural colors. The special ordered structure (photonic crystal structure) formed by the self-assembly of silica produces structural colors through selective reflection phenomena such as light scattering and diffraction, thereby obtaining structural color textile fabrics. PDA is used to coat SiO2 microspheres to obtain PDA@SiO2 microspheres because the melanin substance polydopamine can absorb background stray light and provide strong adhesion, which can greatly improve the color saturation of structural color textile fabrics. In the second step, nanosilver is loaded on the surface of PDA@SiO2 microspheres by in-situ reduction. The polyhydroxyl groups of PDA itself have certain reducing properties, which can reduce Ag. + Reduction to Ag 0 , giving structural color textile fabrics good antibacterial properties. In the third step, γ-aminopropyltriethoxysilane is a silane coupling agent, which is used to modify cotton fabrics to obtain amino-activated cotton fabrics. Then, the PDA@Ag@SiO2 microspheres are self-assembled onto amino-activated cotton fabrics by drop coating to achieve multiple chemical bond connections, further improving the mechanical properties of the photonic crystal coating and the surface of the photonic crystal coating and cotton fabric.
[0025] Beneficial Effects
[0026] (1) The structural color textile fabric of the present invention has non-anisotropic structural color rendering, and the displayed structural color has low angle dependence. Compared with the general anisotropic photonic crystal structural color, this non-anisotropic structural color is more in line with the dyeing requirements of traditional textile fabrics.
[0027] (2) The structural color textile fabric of the present invention has strong antibacterial properties, and the coating is non-toxic to cells and is safe and harmless to the human body. After being immersed in water for 30 days, it still maintains a high degree of structural integrity and color display performance, while still maintaining excellent antibacterial properties. After 90 times of washing, 60 times of bending and 60 times of friction tests, it also maintains good structural color display and antibacterial properties, showing high color fastness and antibacterial properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The scanning electron microscope images of the PDA@SiO2 microspheres in Comparative Example 1 and the PDA@Ag@SiO2 microspheres in Example 1 are shown.
[0029] Figure 2 These are optical photographs of the PDA@SiO2 microspheres in Comparative Example 1 and the PDA@Ag@SiO2 microspheres in Example 1 self-assembled into ordered structures (photonic crystals) on modified cotton fabrics.
[0030] Figure 3 The reflection spectrum of the yellow film formed by PDA@Ag@SiO2 microspheres in Example 1 at different incident angles.
[0031] Figure 4 The structural color reflectance spectra of the modified structural color cotton fabric colored by PDA@Ag@SiO2 microsphere drop coating in Example 1 after 0, 30, 60 and 90 washes and the corresponding OD regeneration values of Staphylococcus aureus and Escherichia coli.
[0032] Figure 5 The structural color reflectance spectra of the modified structural color cotton fabric colored by PDA@Ag@SiO2 microsphere drop coating in Example 1 after being bent 0 times, 20 times, 40 times and 60 times, and the corresponding OD regeneration values of Staphylococcus aureus and Escherichia coli.
[0033] Figure 6 The structural color reflectance spectra of the modified structural color cotton fabric colored by PDA@Ag@SiO2 microsphere drop coating in Example 1 after 0, 20, 40 and 60 times of mechanical friction and the corresponding OD regeneration values of Staphylococcus aureus and Escherichia coli. DETAILED DESCRIPTION
[0034] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0035] Example 1
[0036] (1) Preparation of PDA@SiO2 microspheres: 50 g of ethanol and 5 g of ammonia water were added to 50 g of water, mixed evenly and introduced with nitrogen, then heated in a water bath to 70°C, allowed to stand for 30 min, and then 5 g of tetraethyl orthosilicate was added to start the reaction. After the reaction was completed, the silica nanoparticle powder was centrifuged and washed; 100 g of Tris was added to 1000 g of water, dissolved and the pH was adjusted to about 8.5; then 100 g of dopamine hydrochloride was added and mixed evenly to obtain a mixed solution; under nitrogen protection, the above 3 g of silica nanoparticle powder was added to 100 g of the mixed solution, mixed evenly, and then stirred at room temperature for 12 h. After the reaction was completed, the PDA@SiO2 nanoparticle powder was centrifuged, washed and dried to obtain the PDA@SiO2 nanoparticle powder;
[0037] (2) Preparation of PDA@Ag@SiO2 microspheres: Add 50 g of ethanol to 50 g of water, mix well, add 3 g of silver nitrate and 3 g of PDA@SiO2 nanoparticle powder in step (1), and disperse by ultrasonic at room temperature for 30 min to obtain a PDA@Ag@SiO2 suspension solution for use;
[0038] (3) Finishing into a structural color textile fabric with excellent antibacterial properties and good color fastness: adding 3g of γ-aminopropyltriethoxysilane to 100g of water, stirring evenly, immersing a 5cm x 5cm cotton fabric therein, heating to 70°C, stirring continuously for 12h, washing with water and then drying to obtain the modified amino-activated cotton fabric; applying 10g of the PDA@Ag@SiO2 suspension solution in step (2) to the modified amino-activated cotton fabric, and then drying at 70°C to obtain a structural color textile fabric with excellent antibacterial properties.
[0039] Example 2
[0040] (1) Preparation of PDA@SiO2 microspheres: 30 g of ethanol and 3 g of ammonia water were added to 70 g of water, mixed evenly and introduced with nitrogen, then heated in a water bath to 70°C, allowed to stand for 30 min, and then 5 g of tetraethyl orthosilicate was added to start the reaction. After the reaction was completed, the silica nanoparticle powder was centrifuged and washed; 100 g of Tris was added to 1000 g of water, dissolved and the pH was adjusted to about 8.5; then 100 g of dopamine hydrochloride was added and mixed evenly to obtain a mixed solution; under nitrogen protection, the above 7 g of silica nanoparticle powder was added to 100 g of the mixed solution, mixed evenly, and then stirred at room temperature for 12 h. After the reaction was completed, the powder was centrifuged, washed and dried to obtain PDA@SiO2 nanoparticle powder;
[0041] (2) Preparation of PDA@Ag@SiO2 microspheres: Add 50 g of ethanol to 50 g of water, mix well, add 7 g of silver nitrate and 7 g of PDA@SiO2 nanoparticle powder in step (1), and disperse by ultrasonic at room temperature for 30 min to obtain a PDA@Ag@SiO2 suspension solution for use;
[0042] (3) Finishing into a structural color textile fabric with excellent antibacterial properties and good color fastness: adding 7g of γ-aminopropyltriethoxysilane to 100g of water, stirring evenly, immersing a 5cm x 5cm cotton fabric therein, heating to 70°C, stirring continuously for 12h, washing with water and then drying to obtain the modified amino-activated cotton fabric; dripping 30g of the PDA@Ag@SiO2 suspension solution in step (2) onto the modified amino-activated cotton fabric, and then drying at 70°C to obtain a structural color textile fabric with excellent antibacterial properties.
[0043] Similar to Example 1, the structural color textile fabric has a strong bactericidal property against Escherichia coli and Staphylococcus aureus (its OD value is significantly different from that of the blank control, and the antibacterial rate is above 95%). After 30 days of immersion in water, 90 washes, 60 bends and 60 friction tests, the fabric still maintains a high level of antibacterial performance and structural color display.
[0044] Example 3
[0045] (1) Preparation of PDA@SiO2 microspheres: 40 g of ethanol and 4 g of ammonia water were added to 60 g of water, mixed evenly and introduced with nitrogen, then heated in a water bath to 70°C, allowed to stand for 30 min, and then 5 g of tetraethyl orthosilicate was added to start the reaction. After the reaction was completed, the silica nanoparticle powder was centrifuged and washed; 100 g of Tris was added to 1000 g of water, dissolved and the pH was adjusted to about 8.5; then 100 g of dopamine hydrochloride was added and mixed evenly to obtain a mixed solution; under nitrogen protection, the above 10 g of silica nanoparticle powder was added to 100 g of the mixed solution, mixed evenly, and then stirred at room temperature for 12 h. After the reaction was completed, the PDA@SiO2 nanoparticle powder was centrifuged, washed and dried to obtain the PDA@SiO2 nanoparticle powder;
[0046] (2) Preparation of PDA@Ag@SiO2 microspheres: Add 50 g of ethanol to 50 g of water, mix well, add 10 g of silver nitrate and 10 g of PDA@SiO2 nanoparticle powder in step (1), and disperse by ultrasonic at room temperature for 30 min to obtain a PDA@Ag@SiO2 suspension solution for use;
[0047] (3) Finishing into a structural color textile fabric with excellent antibacterial properties and good color fastness: adding 10 g of γ-aminopropyltriethoxysilane to 100 g of water, stirring evenly, immersing a 5 cm by 5 cm cotton fabric therein, heating to 70°C, stirring continuously for 12 h, washing with water and then drying to obtain the modified amino-activated cotton fabric; dripping 50 g of the PDA@Ag@SiO2 suspension solution in step (2) onto the modified amino-activated cotton fabric, and then drying at 70°C to obtain a structural color textile fabric with excellent antibacterial properties.
[0048] Similar to Example 1, the structural color textile fabric has a strong bactericidal property against Escherichia coli and Staphylococcus aureus (its OD value is significantly different from that of the blank control, and the antibacterial rate is above 95%). After 30 days of immersion in water, 90 washes, 60 bends and 60 friction tests, the fabric still maintains a high level of antibacterial performance and structural color display.
[0049] Comparative Example 1
[0050] (1) Preparation of PDA@SiO2 microspheres: 50 g of ethanol and 5 g of ammonia water were added to 50 g of water, mixed evenly and introduced with nitrogen, then heated in a water bath to 70°C, allowed to stand for 30 min, and then 5 g of tetraethyl orthosilicate was added to start the reaction. After the reaction was completed, the silica nanoparticle powder was centrifuged and washed; 100 g of Tris was added to 1000 g of water, dissolved and the pH was adjusted to about 8.5; then 100 g of dopamine hydrochloride was added and mixed evenly to obtain a mixed solution; under nitrogen protection, the above 3 g of silica nanoparticle powder was added to 100 g of the mixed solution, mixed evenly, and then stirred at room temperature for 12 h. After the reaction was completed, the PDA@SiO2 nanoparticle powder was centrifuged, washed and dried to obtain the PDA@SiO2 nanoparticle powder;
[0051] (2) Finishing into structural color textile fabrics: adding 3 g of γ-aminopropyltriethoxysilane to 100 g of water, stirring evenly, immersing a 5 cm x 5 cm cotton fabric therein, heating to 70°C, stirring continuously for 12 h, washing with water and then drying to obtain the modified amino-activated cotton fabric; applying 10 g of the PDA@SiO2 suspension solution in step (1) to the modified amino-activated cotton fabric, and then drying at 70°C to obtain the structural color textile fabric.
[0052] from Figure 1 It can be seen that the microstructures of the PDA@SiO2 microspheres in Comparative Example 1 and the PDA@Ag@SiO2 microspheres in Example 1 were observed by scanning electron microscopy (SEM), and Ag was successfully loaded on Example 1.
[0053] Figure 2 The optical photographs of the PDA@SiO2 microspheres in Comparative Example 1 and the PDA@Ag@SiO2 microspheres in Example 1 self-assembled into ordered structures (photonic crystals) on modified cotton fabrics. Based on the coordination between PDA and Ag ions in Example 1, the structural colors on the textiles are endowed with good large-area crack-free properties, giving them high color saturation. The amorphous photonic crystals assembled by silver ions and PDA@SiO2 microspheres interact with light scattering to produce non-iridescent structural colors with high color saturation.
[0054] Figure 3 The reflectance spectra of the yellow film formed by the PDA@Ag@SiO2 microspheres in Example 1 at different incident angles. The peak position does not change significantly from the detection angle of 0° to 90°. These results show that the structural color textiles based on short-range ordered amorphous photonic crystals have low angle dependence due to isotropy. Non-iridescent structural colors have the characteristics of wide viewing angle and can be perceived by the naked eye.
[0055] from Figure 4-Figure 6It can be seen that the structural color textile fabric in Example 1 has a strong bactericidal property against Escherichia coli and Staphylococcus aureus. After 30 days of immersion in water, 90 washes, 60 bends and 60 friction tests, the fabric still maintains a high level of antibacterial performance and structural color display.
[0056] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the scope of protection of the present invention.
Claims
1. A structural color textile fabric with excellent antibacterial properties, characterized in that: PDA@Ag@SiO2 microspheres are self-assembled and deposited on the surface of the fabric modified with silane coupling agent to form an amorphous photonic crystal coating.
2. The structural color textile fabric according to claim 1, characterized in that: The PDA@Ag@SiO2 microspheres are obtained by introducing polydopamine on the outer layer of the silica microspheres, and then loading nanosilver on the surface of the microspheres by in-situ reduction.
3. The structural color textile fabric according to claim 1, characterized in that: The fabric includes cotton fabric, cotton fiber or a blended fabric thereof.
4. A method for preparing a structural color textile fabric with excellent antibacterial properties, comprising the following steps: (1) preparing silica nanoparticle powder; adding tris(hydroxymethyl)aminomethane to water, dissolving it and adjusting the pH to 8-9; then adding dopamine hydrochloride and mixing well to obtain a mixed solution; adding silica nanoparticle powder to the mixed solution under nitrogen protection, and then stirring at room temperature. After the reaction is completed, centrifugation, washing and drying are performed to obtain PDA@SiO2 nanoparticle powder; (2) adding ethanol to water, mixing evenly, adding silver nitrate and the PDA@SiO2 nanoparticle powder in step (1), and dispersing by ultrasonication at room temperature to obtain a PDA@Ag@SiO2 suspension solution for use; (3) The PDA@Ag@SiO2 suspension solution in step (2) is dropped onto the surface of the fabric modified with a silane coupling agent to form an amorphous photonic crystal coating, which is then dried to obtain a structural color textile fabric with excellent antibacterial properties.
5. The preparation method according to claim 4, characterized in that: The preparation steps of the silica nanoparticle powder in step (1) are as follows: ethanol and ammonia water are added into water, mixed evenly and nitrogen is introduced, then heated in a water bath to 70-80° C., after standing, ethyl orthosilicate is added to react for 4-6 hours, and after the reaction is completed, centrifugation and washing are performed to obtain the silica nanoparticle powder.
6. The preparation method according to claim 4, characterized in that: The molar amount of tris(hydroxymethyl)aminomethane in step (1) is 10-15 mol% of the molar amount of water; the molar amount of dopamine hydrochloride is 1-10 mol% of the molar amount of water; and the mass of the silicon dioxide nanoparticles is 3-10 wt% of the mass of water.
7. The preparation method according to claim 4, characterized in that: The mass of ethanol in step (2) is 50-55wt% of the mass of water; the mass of silver nitrate is 3-10wt% of the mass of the water / ethanol mixed solution; the mass of the nanoparticle PDA@SiO2 is 3-10wt% of the mass of the water / ethanol mixed solution.
8. The preparation method according to claim 4, characterized in that: The silane coupling agent in step (3) is γ-aminopropyltriethoxysilane, and the mass of the silane coupling agent is 3-10wt% of the mass of water.
9. The preparation method according to claim 4, characterized in that: The modification temperature of the fabric modified with the silane coupling agent in step (3) is 50-70° C., and the modification time is 6-12 hours.
10. The preparation method according to claim 4, characterized in that: The drying temperature in step (3) is 50-70°C.
Citation Information
Patent Citations
Preparation method of polydopamine / nanosilver antibacterial textile
CN110578253A
Composite antibacterial finished non-woven fabric and preparation method thereof
CN113215820A
Photonic crystal self-assembly fabric and preparation method thereof
CN114369946A
Preparation method of structural color coating as well as product and application thereof
CN114836080A
Metastable-state amorphous photonic crystal pigment and preparation method thereof
CN116082860A