A preparation process of electromagnetic wire for wind power generation
The wire-encapsulated paint is prepared by the reaction of modified polyether ether ketone and modified nanoalumina, which solves the problems of insufficient mechanical strength, scratch resistance and thermal conductivity in wind power generation applications, and achieves the excellent electromagnetic wires for wind power generation Performance and self-healing capabilities.
Patent Information
- Application Number
- CN202411239924.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-05
AI Technical Summary
When faced with complex mechanical stress and physical factors, existing enameled wires are difficult to meet the requirements of high mechanical strength, scratch resistance and thermal conductivity, and their self-repairing performance is insufficient, which affects its reliability in wind power applications.
The wire-encapsulated paint is prepared by reaction of modified polyether ether ketone and modified nanoalumina. By wetting and drying on the bare copper wire core, an electromagnetic wire for wind power generation with excellent tensile properties, anti-aging properties and thermal conductivity are formed. . Specific steps include preparing modified nanoalumina and functionalized polysiloxane and combining with modified polyether ether ketone to form a wire-encapsulated paint that enhances the crosslinking effect.
The tensile performance, anti-aging performance, thermal conductivity and self-repair performance of electromagnetic wires for wind power generation are improved, ensuring their stability and reliability in complex environments.
Smart Images

Figure FDA0005079765910000021 
Figure FDA0005079765910000031 
Figure FDA0005079765910000032
Abstract
Description
Technical Field
[0001] The invention relates to the field of electromagnetic wires, in particular to a preparation process of an electromagnetic wire for wind power generation. Background Art
[0002] Enameled wire is made by coating metal wires such as copper, aluminum, and manganese-copper alloy with polymer insulating paint according to a specific production process. This specific insulating paint is called wire enameled paint. Enameled wire is mainly used as a winding coil. Its function is to realize the energy conversion between "electricity" and "magnetism" during the operation of components, so enameled wire is also called electromagnetic wire. The function of enameled wire insulating paint is to produce a good insulating layer between the wires in the winding to prevent the flow of current. Wire enameled paint belongs to electrical insulating paint. As an electrical insulating paint, in addition to having good dielectric and chemical properties, it must also have excellent tensile properties and thermal conductivity.
[0003] With the rapid development of industrial appliances, household appliances, telecommunications, electronic products, etc., the market demand for enameled wires has expanded dramatically in recent years. my country's enameled wires are in a state of rapid development, which has brought a wider application field and market for enameled wires, but at the same time, higher requirements are put forward for enameled wires. Not only are the paint films required to have excellent mechanical strength, scratch resistance, and good adhesion to the conductor, but they must also have good elasticity and flexibility so that they can withstand the various complex mechanical stresses and physical factors during the processing and operation of motors and electrical appliances. Therefore, the present invention prepares an electromagnetic wire for wind power generation with excellent tensile properties, anti-aging properties, thermal conductivity, and self-repairing properties. Summary of the invention
[0004] The purpose of the present invention is to provide a preparation process of electromagnetic wire for wind power generation to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] The invention discloses a preparation process of an electromagnetic wire for wind power generation. The electromagnetic wire for wind power generation is obtained by infiltrating a bare copper wire core into a wire coating obtained by reacting modified polyetheretherketone and modified nano-alumina and then drying the wire coating.
[0007] As an optimization, the modified polyetheretherketone is obtained by polymerizing 4,4'-difluorobenzophenone, bisphenol A and functionalized polysiloxane and reacting with pyridine-2-carboxaldehyde.
[0008] As an optimization, the functionalized polysiloxane is obtained by reacting 1,3,5,7-tetramethylcyclotetrasiloxane, 3-aminopropylmethyldimethoxysilane and 1,3-bis(hydroxypropyl)tetramethyldisiloxane.
[0009] As an optimization, the modified nano-alumina is obtained by reacting nano-alumina with 5,6-epoxyhexyltriethoxysilane and N-allyl hindered phenol in sequence.
[0010] As an optimization, the N-allyl hindered phenol is prepared by reacting 3,5-di-tert-butyl-4-hydroxybenzylamine and allyl chloride.
[0011] As an optimization, a preparation process of an electromagnetic wire for wind power generation includes the following preparation steps:
[0012] (1) 3,5-di-tert-butyl-4-hydroxybenzylamine, potassium carbonate, tetrabutylammonium iodide and acetonitrile are mixed in a mass ratio of 1:(1-2):(0.05-0.15):(18-20), stirred at 20-30° C. and 100-200 rpm for 20-30 min, allyl chloride in an amount of 0.9-1.1 times the molar amount of 3,5-di-tert-butyl-4-hydroxybenzylamine is added, stirring is continued for 11-13 h, saturated ammonium chloride solution in an amount of 18-20 times the mass of 3,5-di-tert-butyl-4-hydroxybenzylamine is added, stirring is continued for 4-6 min, extraction is performed with ethyl acetate, the organic phase is dried with anhydrous sodium sulfate for 40-60 min, and after reduced pressure distillation, chromatographic separation is performed with ethyl acetate and petroleum ether in a volume ratio of 1:5 to obtain N-allyl hindered phenol;
[0013] (2) 5,6-epoxyhexyltriethoxysilane and anhydrous ethanol are mixed at a mass ratio of 1:(39-41), the pH is adjusted to 3-4 with a 5-15% mass fraction citric acid aqueous solution, magnetic stirring is performed for 2-4 minutes, and the mixture is allowed to stand for 55-65 minutes to obtain a 5,6-epoxyhexyltriethoxysilane alcoholysis solution; nano-alumina and the 5,6-epoxyhexyltriethoxysilane alcoholysis solution are mixed at a mass ratio of 1:(18-22), ultrasonically dispersed for 9-11 minutes, stirred at 75-85°C and 250-350 r / min for 2-4 hours, and then filtered. Wash with anhydrous ethanol for 3 to 5 times, dry at 55 to 65° C. for 11 to 13 hours to obtain pre-modified nano-alumina; mix the pre-modified nano-alumina and acetonitrile at a mass ratio of 1:(30 to 40), add N-allyl hindered phenol, the ratio of the molar amount of nitrogen element in N-allyl hindered phenol to the molar amount of epoxy group in the pre-modified nano-alumina is 1:1, stir at 70 to 80° C. and 150 to 250 rpm for 10 to 12 hours, cool naturally to room temperature and then centrifuge, wash with anhydrous ethanol for 3 to 5 times, dry at 65 to 75° C. for 13 to 15 hours to obtain modified nano-alumina;
[0014] (3) 1,3,5,7-tetramethylcyclotetrasiloxane, 3-aminopropylmethyldimethoxysilane and tetramethylammonium hydroxide silicon alkoxide are mixed in a mass ratio of 1:(1.4-1.5):(0.011-0.013), nitrogen is passed through for 15-25 minutes, and the mixture is stirred at 80-85° C. and 100-200 rpm for 2-3 hours. 1,3-bis(hydroxypropyl)tetramethyldisiloxane (0.2-0.4 times the mass of 1,3,5,7-tetramethylcyclotetrasiloxane) is added, the mixture is heated to 95-105° C. and stirred for 7-9 hours, the mixture is heated to 130-140° C. at a rate of 10-20° C. / min and stirred for 40-50 minutes, and distilled at 0.1-0.3 MPa for 1-2 hours to obtain a functionalized polysiloxane.
[0015] (4) 4,4'-difluorobenzophenone, bisphenol A, functionalized polysiloxane, anhydrous potassium carbonate and sulfolane were mixed in a molar ratio of 1:(0.5-0.7):(0.3-0.5):(1.1-1.2):(20-22), stirred at 115-125°C and 100-200 rpm for 1-3 h under a nitrogen environment, heated to 225-235°C and continued to stir for 4-5 h, added deionized water 20-30 times the mass of 4,4'-difluorobenzophenone, cooled to room temperature, filtered and crushed, and washed with methanol and deionized water respectively. The pre-modified polyetheretherketone is mixed with tetrahydrofuran in a mass ratio of 1:(18-20), pyridine-2-carboxaldehyde is added, and the ratio of the molar amount of the aldehyde group in the pyridine-2-carboxaldehyde to the molar amount of the amino group in the pre-modified polyetheretherketone is 1:1, and the mixture is stirred at 55-65°C and 200-300rpm for 2-4h in a nitrogen atmosphere, and filtered after naturally cooling to room temperature, washed with deionized water for 3-5 times, and dried at 55-65°C for 8-10h to obtain modified polyetheretherketone;
[0016] (5) Modified polyetheretherketone, modified nano-alumina, chloroplatinic acid and N,N-dimethylformamide are mixed in a mass ratio of 1:(0.1-0.2):(0.01-0.02):(2-3), and stirred at 30-40°C and 200-300 rpm for 25-35 min to obtain a wire coating; a bare copper wire core with a diameter of 1.4-1.6 mm is soaked in the wire coating and taken out, and then allowed to stand at 85-95°C for 30-40 min and then soaked again, and the process is repeated until the paint film thickness is 16-20 μm, and then dried at 115-125°C for 25-35 min, heated to 145-155°C for drying for 25-35 min, heated to 175-185°C for further drying for 25-35 min, allowed to stand at 215-225°C for 2-3 h, and naturally cooled to room temperature to obtain an electromagnetic wire for wind power generation.
[0017] As an optimization, the reaction equation of the N-allyl hindered phenol in step (1) is:
[0018]
[0019] As an optimization, the reaction equation for the modified nano-alumina in step (2) is:
[0020]
[0021] As an optimization, the reaction equation of the functionalized polysiloxane in step (3) is:
[0022]
[0023] As an optimization, the reaction equation of the modified polyetheretherketone in step (4) is:
[0024]
[0025] Where R is:
[0026]
[0027] As an optimization, when the electromagnetic wire for wind power generation is used, the electromagnetic wire for wind power generation can be wound around the iron core.
[0028] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0029] When preparing electromagnetic wire for wind power generation, the present invention comprises the following steps: reacting 3,5-di-tert-butyl-4-hydroxybenzylamine and allyl chloride to obtain N-allyl hindered phenol; reacting nano-alumina with 5,6-epoxyhexyltriethoxysilane and N-allyl hindered phenol in sequence to obtain modified nano-alumina; reacting 1,3,5,7-tetramethylcyclotetrasiloxane, 3-aminopropylmethyldimethoxysilane and 1,3-bis(hydroxypropyl)tetramethyldisiloxane to obtain functionalized polysiloxane; polymerizing 4,4'-difluorobenzophenone, bisphenol A and functionalized polysiloxane and reacting with pyridine-2-carboxaldehyde to obtain modified polyetheretherketone; and soaking a bare copper wire core in a wire coating varnish obtained by reacting the modified polyetheretherketone and the modified nano-alumina, followed by drying to prepare the electromagnetic wire for wind power generation.
[0030] Firstly, 3,5-di-tert-butyl-4-hydroxybenzylamine and allyl chloride are reacted to obtain N-allyl hindered phenol; then, nano-alumina is reacted with 5,6-epoxyhexyltriethoxysilane and N-allyl hindered phenol in sequence to obtain modified nano-alumina; 5,6-epoxyhexyltriethoxysilane is grafted on the nano-alumina to improve the dispersibility of the nano-alumina and enhance the thermal conductivity of the electromagnetic wire for wind power generation; N-allyl hindered phenol is grafted on by reacting the epoxy groups retained on the surface with secondary amines, and the hydrogen on the phenolic hydroxyl group combines with oxygen-containing free radicals to destroy the activity of the free radicals, terminate the chain reaction of thermal oxidative aging, and improve the anti-aging performance of the electromagnetic wire for wind power generation; at the same time, a double bond structure is introduced to react with the silicon-hydrogen bond on the main chain of polyetheretherketone to enhance the cross-linking effect and improve the tensile performance of the electromagnetic wire for wind power generation.
[0031] Secondly, 1,3,5,7-tetramethylcyclotetrasiloxane, 3-aminopropylmethyldimethoxysilane and 1,3-bis(hydroxypropyl)tetramethyldisiloxane are reacted to obtain functionalized polysiloxane; 4,4'-difluorobenzophenone, bisphenol A and functionalized polysiloxane are polymerized and then reacted with pyridine-2-carboxaldehyde to obtain modified polyetheretherketone; the bare copper wire core is infiltrated in a wire coating obtained by reacting modified polyetheretherketone and modified nano-alumina, and then dried to prepare electromagnetic wire for wind power generation; functionalized polysiloxane participates in the polymerization of the main chain of polyetheretherketone, and a flexible long silicon-oxygen chain with strong polarity and high bond energy is introduced into the main chain to enhance the thermal conductivity and tensile properties of the electromagnetic wire for wind power generation; at the same time, the amino group on the functionalized polysiloxane can react with the aldehyde group on pyridine-2-carboxaldehyde to form a stable five-membered ring structure that chelates metal ions, thereby enhancing the bonding effect with the copper wire and improving the self-healing performance of the electromagnetic wire for wind power generation. DETAILED DESCRIPTION
[0032] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0033] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the electromagnetic wire for wind power generation prepared in the following examples are as follows:
[0034] Tensile properties: The wire varnish obtained in each example and the comparative example were poured into a 5cm*1cm*18μm mold for curing, and stretched with an electronic wire drawing machine at a stretching speed of 10mm / min to measure the tensile breaking strength (Rm0).
[0035] Anti-aging performance: The wire varnish obtained in each embodiment and the comparative example were poured into a 5cm*1cm*18μm mold for curing, aged at 100°C for 5 days, taken out, naturally cooled to room temperature, stretched with an electronic wire drawing machine at a stretching speed of 10mm / min, and the tensile breaking strength (Rm1) was measured. Compared with the tensile performance results, the retention rate (Rm1 / Rm0*100%) was calculated.
[0036] Thermal conductivity: The wire varnish obtained in each embodiment and the comparative example were poured into a 5cm*1cm*18μm mold for curing, and the thermal conductivity was tested at 250°C in a nitrogen environment.
[0037] Self-repairing performance: The wire coating obtained in each embodiment and the comparative example were respectively applied and cured on two tinplates meeting the requirements of GB / T9271 to a thickness of 18 μm to obtain two samples in each group; one sample was taken from each group and heated at 50°C in a 0.26 g / L copper chloride solution and a 50 g / L sodium chloride solution at a temperature of 1 ml / 50 cm 2 ·h spray volume for 12h, and measure the initial defect area and make appearance rating according to GB / T6461; scratch the other piece with the same depth and size, let it stand at 25℃ for 24h, and then conduct the same copper-accelerated acetic acid salt spray test, measure the defect area after repair and make appearance rating, calculate whether it is degraded, and judge the self-repairing performance.
[0038] Embodiment 1:
[0039] A preparation process of an electromagnetic wire for wind power generation, the preparation process of the electromagnetic wire for wind power generation comprising the following preparation steps:
[0040] (1) 3,5-di-tert-butyl-4-hydroxybenzylamine, potassium carbonate, tetrabutylammonium iodide and acetonitrile were mixed in a mass ratio of 1:1:0.05:18, stirred at 20°C and 100 rpm for 30 minutes, allyl chloride was added in an amount of 0.9 times the molar amount of 3,5-di-tert-butyl-4-hydroxybenzylamine, and stirring was continued for 13 hours, saturated ammonium chloride solution was added in an amount of 18 times the mass of 3,5-di-tert-butyl-4-hydroxybenzylamine, and stirring was continued for 6 minutes, extracted with ethyl acetate, and the organic phase was dried over anhydrous sodium sulfate for 40 minutes, and after reduced pressure distillation, chromatographic separation was performed using ethyl acetate and petroleum ether in a volume ratio of 1:5 to obtain N-allyl hindered phenol;
[0041] (2) 5,6-epoxyhexyltriethoxysilane and anhydrous ethanol were mixed at a mass ratio of 1:39, the pH was adjusted to 4 with a 5% citric acid aqueous solution, magnetic stirring was performed for 2 minutes, and the mixture was allowed to stand for 55 minutes to obtain a 5,6-epoxyhexyltriethoxysilane alcoholysis solution; nano-alumina and the 5,6-epoxyhexyltriethoxysilane alcoholysis solution were mixed at a mass ratio of 1:18, ultrasonically dispersed for 9 minutes, stirred at 75°C and 250 r / min for 4 hours, and then filtered. Wash with anhydrous ethanol for 3 times, dry at 55°C for 13 hours to obtain pre-modified nano-alumina; mix the pre-modified nano-alumina and acetonitrile at a mass ratio of 1:30, add N-allyl hindered phenol, the ratio of the molar amount of nitrogen element in N-allyl hindered phenol to the molar amount of epoxy group in the pre-modified nano-alumina is 1:1, stir at 70°C and 150rpm for 12 hours, cool naturally to room temperature and then centrifuge, wash with anhydrous ethanol for 3 times, dry at 65°C for 15 hours to obtain modified nano-alumina;
[0042] (3) 1,3,5,7-tetramethylcyclotetrasiloxane, 3-aminopropylmethyldimethoxysilane and tetramethylammonium hydroxide silicon alkoxide were mixed in a mass ratio of 1:1.4:0.011, nitrogen was passed for 15 minutes, and the mixture was stirred at 80°C and 100 rpm for 3 hours. 1,3-bis(hydroxypropyl)tetramethyldisiloxane (0.2 times the mass of 1,3,5,7-tetramethylcyclotetrasiloxane) was added, the temperature was raised to 95°C and stirring was continued for 9 hours, the temperature was raised to 130°C at 10°C / min and stirring was continued for 50 minutes, and distilled at 0.1 MPa for 2 hours to obtain functionalized polysiloxane;
[0043] (4) 4,4'-difluorobenzophenone, bisphenol A, functionalized polysiloxane, anhydrous potassium carbonate and sulfolane were mixed in a molar ratio of 1:0.5:0.3:1.1:20, stirred at 115°C and 100 rpm for 3 h under a nitrogen environment, heated to 225°C and stirred for 5 h, added with deionized water 20 times the mass of 4,4'-difluorobenzophenone, cooled to room temperature, filtered and crushed, washed with methanol and deionized water for 3 times, and then heated to 500 °C. 5°C for 12 hours to obtain pre-modified polyetheretherketone; pre-modified polyetheretherketone and tetrahydrofuran were mixed at a mass ratio of 1:18, pyridine-2-carboxaldehyde was added, the ratio of the molar amount of aldehyde groups in pyridine-2-carboxaldehyde to the molar amount of amino groups in pre-modified polyetheretherketone was 1:1, stirred at 55°C and 200rpm for 4 hours in a nitrogen atmosphere, naturally cooled to room temperature and then filtered, washed with deionized water for 3 times, and dried at 55°C for 10 hours to obtain modified polyetheretherketone;
[0044] (5) Modified polyetheretherketone, modified nano-alumina, chloroplatinic acid and N,N-dimethylformamide were mixed in a mass ratio of 1:0.1:0.01:2, and stirred at 30°C and 200 rpm for 35 minutes to obtain a wire coating; a bare copper wire core with a diameter of 1.4 mm was soaked in the wire coating and taken out, and then allowed to stand at 85°C for 40 minutes and then soaked again, and the process was repeated until the paint film thickness reached 16 μm, and then dried at 115°C for 35 minutes, heated to 145°C for drying for 35 minutes, heated to 175°C for further drying for 35 minutes, and allowed to stand at 215°C for 3 hours, and naturally cooled to room temperature to obtain electromagnetic wire for wind power generation.
[0045] Embodiment 2:
[0046] A preparation process of an electromagnetic wire for wind power generation, the preparation process of the electromagnetic wire for wind power generation comprising the following preparation steps:
[0047] (1) 3,5-di-tert-butyl-4-hydroxybenzylamine, potassium carbonate, tetrabutylammonium iodide and acetonitrile were mixed in a mass ratio of 1:1.5:0.1:19, stirred at 25°C and 150 rpm for 25 minutes, allyl chloride was added in an amount of 1 times the molar amount of 3,5-di-tert-butyl-4-hydroxybenzylamine, and stirring was continued for 12 hours, saturated ammonium chloride solution was added in an amount of 19 times the mass of 3,5-di-tert-butyl-4-hydroxybenzylamine, and stirring was continued for 5 minutes, extracted with ethyl acetate, and the organic phase was dried over anhydrous sodium sulfate for 50 minutes, and after reduced pressure distillation, chromatographic separation was performed using ethyl acetate and petroleum ether in a volume ratio of 1:5 to obtain N-allyl hindered phenol;
[0048] (2) 5,6-epoxyhexyltriethoxysilane and anhydrous ethanol were mixed at a mass ratio of 1:40, the pH was adjusted to 3.5 with a 10% citric acid aqueous solution, magnetic stirring was performed for 3 minutes, and the mixture was allowed to stand for 60 minutes to obtain a 5,6-epoxyhexyltriethoxysilane alcoholysis solution; nano-alumina and 5,6-epoxyhexyltriethoxysilane alcoholysis solution were mixed at a mass ratio of 1:20, ultrasonically dispersed for 10 minutes, stirred at 80°C and 300 r / min for 3 hours, and then passed through Filter, wash with anhydrous ethanol 4 times, dry at 60°C for 12h to obtain pre-modified nano-alumina; mix the pre-modified nano-alumina and acetonitrile at a mass ratio of 1:35, add N-allyl hindered phenol, the ratio of the molar amount of nitrogen element in N-allyl hindered phenol to the molar amount of epoxy group in the pre-modified nano-alumina is 1:1, stir at 75°C and 200rpm for 11h, cool naturally to room temperature and then centrifuge, wash with anhydrous ethanol 4 times, dry at 70°C for 14h to obtain modified nano-alumina;
[0049] (3) 1,3,5,7-tetramethylcyclotetrasiloxane, 3-aminopropylmethyldimethoxysilane and tetramethylammonium hydroxide silicon alkoxide were mixed in a mass ratio of 1:1.45:0.012, nitrogen was passed through for 20 minutes, and the mixture was stirred at 82.5°C and 150 rpm for 2.5 hours. 1,3-bis(hydroxypropyl)tetramethyldisiloxane (0.3 times the mass of 1,3,5,7-tetramethylcyclotetrasiloxane) was added, the mixture was heated to 100°C and stirred for 8 hours, the mixture was heated to 135°C at a rate of 15°C / min and stirred for 45 minutes, and the mixture was distilled at 0.2 MPa for 1.5 hours to obtain a functionalized polysiloxane.
[0050] (4) 4,4'-difluorobenzophenone, bisphenol A, functionalized polysiloxane, anhydrous potassium carbonate and sulfolane were mixed in a molar ratio of 1:0.6:0.4:1.15:21, stirred at 120°C and 150 rpm for 2 h under a nitrogen environment, heated to 230°C and stirred for 4.5 h, added with deionized water 25 times the mass of 4,4'-difluorobenzophenone, cooled to room temperature, filtered and crushed, washed with methanol and deionized water four times respectively, Dry at 60°C for 11 hours to obtain pre-modified polyetheretherketone; mix the pre-modified polyetheretherketone and tetrahydrofuran at a mass ratio of 1:19, add pyridine-2-carboxaldehyde, the ratio of the molar amount of aldehyde groups in pyridine-2-carboxaldehyde to the molar amount of amino groups in the pre-modified polyetheretherketone is 1:1, stir at 60°C and 250rpm for 3 hours in a nitrogen atmosphere, cool naturally to room temperature and then filter, wash with deionized water 4 times, and dry at 60°C for 9 hours to obtain modified polyetheretherketone;
[0051] (5) Modified polyetheretherketone, modified nano-alumina, chloroplatinic acid and N,N-dimethylformamide were mixed in a mass ratio of 1:0.15:0.015:2.5, and stirred at 35°C and 250 rpm for 30 min to obtain a wire coating; a bare copper wire core with a diameter of 1.5 mm was soaked in the wire coating and taken out, and then allowed to stand at 90°C for 35 min and then soaked again, and the process was repeated until the paint film thickness reached 18 μm, and then dried at 120°C for 30 min, heated to 150°C and dried for 30 min, heated to 180°C and continued to dry for 30 min, and allowed to stand at 220°C for 2.5 h, and naturally cooled to room temperature to obtain electromagnetic wire for wind power generation.
[0052] Embodiment 3:
[0053] A preparation process of an electromagnetic wire for wind power generation, the preparation process of the electromagnetic wire for wind power generation comprising the following preparation steps:
[0054] (1) 3,5-di-tert-butyl-4-hydroxybenzylamine, potassium carbonate, tetrabutylammonium iodide and acetonitrile were mixed in a mass ratio of 1:2:0.15:20, stirred at 30° C. and 200 rpm for 20 min, allyl chloride in an amount of 1.1 times the molar amount of 3,5-di-tert-butyl-4-hydroxybenzylamine was added, stirring was continued for 11 h, saturated ammonium chloride solution in an amount of 20 times the mass of 3,5-di-tert-butyl-4-hydroxybenzylamine was added, stirring was continued for 4 min, extracted with ethyl acetate, and the organic phase was dried over anhydrous sodium sulfate for 60 min, and after reduced pressure distillation, chromatographic separation was performed using ethyl acetate and petroleum ether in a volume ratio of 1:5 to obtain N-allyl hindered phenol;
[0055] (2) 5,6-epoxyhexyltriethoxysilane and anhydrous ethanol were mixed at a mass ratio of 1:41, the pH was adjusted to 4 with a 15% mass fraction citric acid aqueous solution, magnetic stirring was performed for 4 minutes, and the mixture was allowed to stand for 65 minutes to obtain a 5,6-epoxyhexyltriethoxysilane alcoholysis solution; nano-alumina and 5,6-epoxyhexyltriethoxysilane alcoholysis solution were mixed at a mass ratio of 1:22, ultrasonically dispersed for 11 minutes, stirred at 85°C and 350 r / min for 2 hours, and then filtered , washing with anhydrous ethanol for 5 times, drying at 65°C for 11h to obtain pre-modified nano-alumina; mixing the pre-modified nano-alumina and acetonitrile at a mass ratio of 1:40, adding N-allyl hindered phenol, the ratio of the molar amount of nitrogen element in N-allyl hindered phenol to the molar amount of epoxy group in the pre-modified nano-alumina is 1:1, stirring at 80°C and 250rpm for 10h, cooling naturally to room temperature and centrifuging, washing with anhydrous ethanol for 5 times, drying at 75°C for 13h to obtain modified nano-alumina;
[0056] (3) 1,3,5,7-tetramethylcyclotetrasiloxane, 3-aminopropylmethyldimethoxysilane and tetramethylammonium hydroxide silicon alkoxide were mixed in a mass ratio of 1:1.5:0.013, nitrogen was passed for 25 minutes, and the mixture was stirred at 85°C and 200 rpm for 2 hours. 1,3-bis(hydroxypropyl)tetramethyldisiloxane (0.4 times the mass of 1,3,5,7-tetramethylcyclotetrasiloxane) was added, the temperature was raised to 105°C and stirring was continued for 7 hours, the temperature was raised to 140°C at 20°C / min and stirring was continued for 40 minutes, and distilled at 0.3 MPa for 1 hour to obtain functionalized polysiloxane;
[0057] (4) 4,4'-difluorobenzophenone, bisphenol A, functionalized polysiloxane, anhydrous potassium carbonate and sulfolane were mixed in a molar ratio of 1:0.7:0.5:1.2:22, stirred at 125°C and 200 rpm for 1 h under a nitrogen environment, heated to 235°C and stirred for 4 h, added with deionized water 30 times the mass of 4,4'-difluorobenzophenone, cooled to room temperature, filtered and crushed, washed with methanol and deionized water for 5 times, and then heated to 6 5°C for 10 hours to obtain pre-modified polyetheretherketone; the pre-modified polyetheretherketone and tetrahydrofuran were mixed at a mass ratio of 1:20, pyridine-2-carboxaldehyde was added, the ratio of the molar amount of aldehyde groups in pyridine-2-carboxaldehyde to the molar amount of amino groups in the pre-modified polyetheretherketone was 1:1, and the mixture was stirred at 65°C and 300rpm for 2 hours in a nitrogen atmosphere, and filtered after naturally cooling to room temperature, washed with deionized water for 5 times, and dried at 65°C for 8 hours to obtain modified polyetheretherketone;
[0058] (5) Modified polyetheretherketone, modified nano-alumina, chloroplatinic acid and N,N-dimethylformamide were mixed in a mass ratio of 1:0.2:0.02:3, and stirred at 40°C and 300 rpm for 25 minutes to obtain a wire coating; a bare copper wire core with a diameter of 1.6 mm was soaked in the wire coating and taken out, and then allowed to stand at 95°C for 30 minutes and then soaked again, and the process was repeated until the paint film thickness reached 20 μm, and then dried at 125°C for 25 minutes, heated to 155°C and dried for 25 minutes, heated to 185°C and continued to dry for 25 minutes, and allowed to stand at 225°C for 2 hours, and naturally cooled to room temperature to obtain electromagnetic wire for wind power generation.
[0059] Comparative Example 1:
[0060] A preparation process of an electromagnetic wire for wind power generation, the preparation process of the electromagnetic wire for wind power generation comprising the following preparation steps:
[0061] (1) 1,3,5,7-tetramethylcyclotetrasiloxane, 3-aminopropylmethyldimethoxysilane and tetramethylammonium hydroxide silicon alkoxide were mixed in a mass ratio of 1:1.45:0.012, nitrogen was passed through for 20 minutes, and the mixture was stirred at 82.5°C and 150 rpm for 2.5 hours. 1,3-bis(hydroxypropyl)tetramethyldisiloxane (0.3 times the mass of 1,3,5,7-tetramethylcyclotetrasiloxane) was added, the mixture was heated to 100°C and stirred for 8 hours, the mixture was heated to 135°C at a rate of 15°C / min and stirred for 45 minutes, and the mixture was distilled at 0.2 MPa for 1.5 hours to obtain a functionalized polysiloxane.
[0062] (2) 4,4'-difluorobenzophenone, bisphenol A, functionalized polysiloxane, anhydrous potassium carbonate and sulfolane were mixed in a molar ratio of 1:0.6:0.4:1.15:21, stirred at 120°C and 150 rpm for 2 h under a nitrogen environment, heated to 230°C and stirred for 4.5 h, added with deionized water 25 times the mass of 4,4'-difluorobenzophenone, cooled to room temperature, filtered and crushed, washed with methanol and deionized water four times respectively, Dry at 60°C for 11 hours to obtain pre-modified polyetheretherketone; mix the pre-modified polyetheretherketone and tetrahydrofuran at a mass ratio of 1:19, add pyridine-2-carboxaldehyde, the ratio of the molar amount of aldehyde groups in pyridine-2-carboxaldehyde to the molar amount of amino groups in the pre-modified polyetheretherketone is 1:1, stir at 60°C and 250rpm for 3 hours in a nitrogen atmosphere, cool naturally to room temperature and then filter, wash with deionized water 4 times, and dry at 60°C for 9 hours to obtain modified polyetheretherketone;
[0063] (3) Modified polyetheretherketone, nano-alumina, chloroplatinic acid and N,N-dimethylformamide were mixed in a mass ratio of 1:0.15:0.015:2.5, and stirred at 35°C and 250 rpm for 30 min to obtain wire coating; a bare copper wire core with a diameter of 1.5 mm was soaked in the wire coating and taken out, and then allowed to stand at 90°C for 35 min and then soaked again, and the process was repeated until the paint film thickness reached 18 μm, and then dried at 120°C for 30 min, heated to 150°C and dried for 30 min, heated to 180°C and continued to dry for 30 min, and allowed to stand at 220°C for 2.5 h, and naturally cooled to room temperature to obtain electromagnetic wire for wind power generation.
[0064] Comparative Example 2:
[0065] A preparation process of an electromagnetic wire for wind power generation, the preparation process of the electromagnetic wire for wind power generation comprising the following preparation steps:
[0066] (1) 3,5-di-tert-butyl-4-hydroxybenzylamine, potassium carbonate, tetrabutylammonium iodide and acetonitrile were mixed in a mass ratio of 1:1.5:0.1:19, stirred at 25°C and 150 rpm for 25 minutes, allyl chloride was added in an amount of 1 times the molar amount of 3,5-di-tert-butyl-4-hydroxybenzylamine, and stirring was continued for 12 hours, saturated ammonium chloride solution was added in an amount of 19 times the mass of 3,5-di-tert-butyl-4-hydroxybenzylamine, and stirring was continued for 5 minutes, extracted with ethyl acetate, and the organic phase was dried over anhydrous sodium sulfate for 50 minutes, and after reduced pressure distillation, chromatographic separation was performed using ethyl acetate and petroleum ether in a volume ratio of 1:5 to obtain N-allyl hindered phenol;
[0067] (2) 5,6-epoxyhexyltriethoxysilane and anhydrous ethanol were mixed at a mass ratio of 1:40, the pH was adjusted to 3.5 with a 10% citric acid aqueous solution, magnetic stirring was performed for 3 minutes, and the mixture was allowed to stand for 60 minutes to obtain a 5,6-epoxyhexyltriethoxysilane alcoholysis solution; nano-alumina and 5,6-epoxyhexyltriethoxysilane alcoholysis solution were mixed at a mass ratio of 1:20, ultrasonically dispersed for 10 minutes, stirred at 80°C and 300 r / min for 3 hours, and then passed through Filter, wash with anhydrous ethanol 4 times, dry at 60°C for 12h to obtain pre-modified nano-alumina; mix the pre-modified nano-alumina and acetonitrile at a mass ratio of 1:35, add N-allyl hindered phenol, the ratio of the molar amount of nitrogen element in N-allyl hindered phenol to the molar amount of epoxy group in the pre-modified nano-alumina is 1:1, stir at 75°C and 200rpm for 11h, cool naturally to room temperature and then centrifuge, wash with anhydrous ethanol 4 times, dry at 70°C for 14h to obtain modified nano-alumina;
[0068] (3) 4,4'-difluorobenzophenone, bisphenol A, functionalized polysiloxane, anhydrous potassium carbonate and sulfolane were mixed in a molar ratio of 1:0.6:0.4:1.15:21, stirred at 120°C and 150 rpm for 2 h under a nitrogen environment, heated to 230°C and continued to stir for 4.5 h, added with deionized water 25 times the mass of 4,4'-difluorobenzophenone, cooled to room temperature, filtered and crushed, washed with methanol and deionized water 4 times respectively, and dried at 60°C for 11 h to obtain modified polyetheretherketone;
[0069] (4) Modified polyetheretherketone, modified nano-alumina, chloroplatinic acid and N,N-dimethylformamide were mixed in a mass ratio of 1:0.15:0.015:2.5, and stirred at 35°C and 250 rpm for 30 minutes to obtain a wire coating; a bare copper wire core with a diameter of 1.5 mm was soaked in the wire coating and taken out, and then allowed to stand at 90°C for 35 minutes and then soaked again, and the process was repeated until the paint film thickness reached 18 μm, and then dried at 120°C for 30 minutes, heated to 150°C and dried for 30 minutes, heated to 180°C and continued to dry for 30 minutes, and allowed to stand at 220°C for 2.5 hours, and naturally cooled to room temperature to obtain electromagnetic wire for wind power generation.
[0070] Comparative Example 3:
[0071] A preparation process of an electromagnetic wire for wind power generation, the preparation process of the electromagnetic wire for wind power generation comprising the following preparation steps:
[0072] (1) 3,5-di-tert-butyl-4-hydroxybenzylamine, potassium carbonate, tetrabutylammonium iodide and acetonitrile were mixed in a mass ratio of 1:1.5:0.1:19, stirred at 25°C and 150 rpm for 25 minutes, allyl chloride was added in an amount of 1 times the molar amount of 3,5-di-tert-butyl-4-hydroxybenzylamine, and stirring was continued for 12 hours, saturated ammonium chloride solution was added in an amount of 19 times the mass of 3,5-di-tert-butyl-4-hydroxybenzylamine, and stirring was continued for 5 minutes, extracted with ethyl acetate, and the organic phase was dried over anhydrous sodium sulfate for 50 minutes, and after reduced pressure distillation, chromatographic separation was performed using ethyl acetate and petroleum ether in a volume ratio of 1:5 to obtain N-allyl hindered phenol;
[0073] (2) 5,6-epoxyhexyltriethoxysilane and anhydrous ethanol were mixed at a mass ratio of 1:40, the pH was adjusted to 3.5 with a 10% citric acid aqueous solution, magnetic stirring was performed for 3 minutes, and the mixture was allowed to stand for 60 minutes to obtain a 5,6-epoxyhexyltriethoxysilane alcoholysis solution; nano-alumina and 5,6-epoxyhexyltriethoxysilane alcoholysis solution were mixed at a mass ratio of 1:20, ultrasonically dispersed for 10 minutes, stirred at 80°C and 300 r / min for 3 hours, and then passed through Filter, wash with anhydrous ethanol 4 times, dry at 60°C for 12h to obtain pre-modified nano-alumina; mix the pre-modified nano-alumina and acetonitrile at a mass ratio of 1:35, add N-allyl hindered phenol, the ratio of the molar amount of nitrogen element in N-allyl hindered phenol to the molar amount of epoxy group in the pre-modified nano-alumina is 1:1, stir at 75°C and 200rpm for 11h, cool naturally to room temperature and then centrifuge, wash with anhydrous ethanol 4 times, dry at 70°C for 14h to obtain modified nano-alumina;
[0074] (3) 4,4'-difluorobenzophenone, bisphenol A, anhydrous potassium carbonate and sulfolane were mixed in a molar ratio of 1:0.6:0.4:1.15:21, stirred at 120°C and 150 rpm for 2 h under a nitrogen environment, heated to 230°C and stirred for 4.5 h, added with deionized water 25 times the mass of 4,4'-difluorobenzophenone, cooled to room temperature, filtered and crushed, washed with methanol and deionized water 4 times respectively, and dried at 60°C for 11 h to obtain polyetheretherketone;
[0075] (4) Polyetheretherketone, modified nano-alumina, chloroplatinic acid and N,N-dimethylformamide were mixed in a mass ratio of 1:0.15:0.015:2.5, and stirred at 35°C and 250 rpm for 30 minutes to obtain a wire coating; a bare copper wire core with a diameter of 1.5 mm was soaked in the wire coating and taken out, and then allowed to stand at 90°C for 35 minutes and then soaked again, and the process was repeated until the paint film thickness reached 18 μm, and then dried at 120°C for 30 minutes, heated to 150°C and dried for 30 minutes, heated to 180°C and continued to dry for 30 minutes, and allowed to stand at 220°C for 2.5 hours, and naturally cooled to room temperature to obtain electromagnetic wire for wind power generation.
[0076] Effect example
[0077] Table 1 below shows the analysis results of the tensile properties, anti-aging properties, thermal conductivity and self-repairing properties of electromagnetic wires for wind power generation using Examples 1 to 3 of the present invention and Comparative Examples 1 to 3.
[0078] Table 1
[0079]
[0080]
[0081] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 3 in Table 1, it can be found that the electromagnetic wire for wind power generation prepared by the present invention has good tensile properties, anti-aging properties, thermal conductivity and self-repairing properties.
[0082] By comparison, the tensile breaking strength, retention rate and thermal conductivity of Examples 1, 2 and 3 are higher than those of Comparative Example 1, which shows that the grafting of 5,6-epoxyhexyltriethoxysilane on the nano-alumina improves the dispersibility of the nano-alumina and enhances the thermal conductivity of the electromagnetic wire for wind power generation; the N-allyl hindered phenol is grafted by reacting the epoxy groups retained on the surface with the secondary amines, and the hydrogen on the phenolic hydroxyl group combines with the oxygen-containing free radicals to destroy the activity of the free radicals, terminate the chain reaction of thermal oxidative aging, and improve the anti-aging performance of the electromagnetic wire for wind power generation; at the same time, the double bond structure is introduced to react with the silicon-hydrogen bonds on the main chain of the polyetheretherketone to enhance the cross-linking effect and improve the tensile properties of the electromagnetic wire for wind power generation.
[0083] By comparison, the appearance rating of Examples 1, 2, and 3 compared with Comparative Example 2 has not been downgraded, indicating that the functionalized polysiloxane participates in the copolymerization of the polyetheretherketone main chain, and the introduced amino group can react with the aldehyde group on pyridine-2-carboxaldehyde to form a stable five-membered ring structure that chelates metal ions, thereby enhancing the bonding effect with the copper wire and improving the self-healing performance of the electromagnetic wire for wind power generation.
[0084] By comparison, Examples 1, 2, and 3 have higher tensile strength at break and thermal conductivity than Comparative Example 3, and their appearance rating is not downgraded, indicating that by participating in the polymerization of the polyetheretherketone main chain with functionalized polysiloxane, a flexible long silicon-oxygen chain with strong polarity and high bond energy is introduced into the main chain, thereby enhancing the thermal conductivity and tensile properties of the electromagnetic wire for wind power generation. At the same time, the silicon-hydrogen bonds can undergo addition reactions with the carbon-carbon double bonds on the modified nano-alumina, thereby enhancing the chemical cross-linking effect and further improving the tensile properties of the electromagnetic wire for wind power generation.
[0085] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A process for preparing electromagnetic wire for wind power generation, It is characterized in that The method comprises the following preparation steps: (1) 3,5-di-tert-butyl-4-hydroxybenzylamine, potassium carbonate, tetrabutylammonium iodide and acetonitrile are mixed in a mass ratio of 1:(1-2):(0.05-0.15):(18-20), stirred at 20-30° C. and 100-200 rpm for 20-30 min, allyl chloride in an amount of 0.9-1.1 times the molar amount of 3,5-di-tert-butyl-4-hydroxybenzylamine is added, stirring is continued for 11-13 h, saturated ammonium chloride solution in an amount of 18-20 times the mass of 3,5-di-tert-butyl-4-hydroxybenzylamine is added, stirring is continued for 4-6 min, extraction is performed with ethyl acetate, the organic phase is dried with anhydrous sodium sulfate for 40-60 min, and after reduced pressure distillation, chromatographic separation is performed with ethyl acetate and petroleum ether in a volume ratio of 1:5 to obtain N-allyl hindered phenol; (2) 5,6-epoxyhexyltriethoxysilane and anhydrous ethanol are mixed at a mass ratio of 1:(39-41), the pH is adjusted to 3-4 with a 5-15% mass fraction citric acid aqueous solution, magnetic stirring is performed for 2-4 minutes, and the mixture is allowed to stand for 55-65 minutes to obtain a 5,6-epoxyhexyltriethoxysilane alcoholysis solution; nano-alumina and the 5,6-epoxyhexyltriethoxysilane alcoholysis solution are mixed at a mass ratio of 1:(18-22), ultrasonically dispersed for 9-11 minutes, stirred at 75-85°C and 250-350 r / min for 2-4 hours, and then filtered. Wash with anhydrous ethanol for 3 to 5 times, dry at 55 to 65° C. for 11 to 13 hours to obtain pre-modified nano-alumina; mix the pre-modified nano-alumina and acetonitrile at a mass ratio of 1:(30 to 40), add N-allyl hindered phenol, the ratio of the molar amount of nitrogen element in N-allyl hindered phenol to the molar amount of epoxy group in the pre-modified nano-alumina is 1:1, stir at 70 to 80° C. and 150 to 250 rpm for 10 to 12 hours, cool naturally to room temperature and then centrifuge, wash with anhydrous ethanol for 3 to 5 times, dry at 65 to 75° C. for 13 to 15 hours to obtain modified nano-alumina; (3) 1,3,5,7-tetramethylcyclotetrasiloxane, 3-aminopropylmethyldimethoxysilane and tetramethylammonium hydroxide silicon alkoxide are mixed in a mass ratio of 1:(1.4-1.5):(0.011-0.013), nitrogen is passed through for 15-25 minutes, and the mixture is stirred at 80-85° C. and 100-200 rpm for 2-3 hours. 1,3-bis(hydroxypropyl)tetramethyldisiloxane (0.2-0.4 times the mass of 1,3,5,7-tetramethylcyclotetrasiloxane) is added, the mixture is heated to 95-105° C. and stirred for 7-9 hours, the mixture is heated to 130-140° C. at a rate of 10-20° C. / min and stirred for 40-50 minutes, and distilled at 0.1-0.3 MPa for 1-2 hours to obtain a functionalized polysiloxane. (4) 4,4'-difluorobenzophenone, bisphenol A, functionalized polysiloxane, anhydrous potassium carbonate and sulfolane were mixed in a molar ratio of 1:(0.5-0.7):(0.3-0.5):(1.1-1.2):(20-22), stirred at 115-125°C and 100-200 rpm for 1-3 h under a nitrogen environment, heated to 225-235°C and continued to stir for 4-5 h, added deionized water 20-30 times the mass of 4,4'-difluorobenzophenone, cooled to room temperature, filtered and crushed, and washed with methanol and deionized water respectively. The pre-modified polyetheretherketone is mixed with tetrahydrofuran in a mass ratio of 1:(18-20), pyridine-2-carboxaldehyde is added, and the ratio of the molar amount of the aldehyde group in the pyridine-2-carboxaldehyde to the molar amount of the amino group in the pre-modified polyetheretherketone is 1:1, and the mixture is stirred at 55-65°C and 200-300rpm for 2-4h in a nitrogen atmosphere, and filtered after naturally cooling to room temperature, washed with deionized water for 3-5 times, and dried at 55-65°C for 8-10h to obtain modified polyetheretherketone; (5) Modified polyetheretherketone, modified nano-alumina, chloroplatinic acid and N,N-dimethylformamide are mixed in a mass ratio of 1:(0.1-0.2):(0.01-0.02):(2-3), and stirred at 30-40°C and 200-300 rpm for 25-35 min to obtain a wire coating; a bare copper wire core with a diameter of 1.4-1.6 mm is soaked in the wire coating and taken out, and then allowed to stand at 85-95°C for 30-40 min and then soaked again, and the process is repeated until the paint film thickness is 16-20 μm, and then dried at 115-125°C for 25-35 min, heated to 145-155°C for drying for 25-35 min, heated to 175-185°C for further drying for 25-35 min, allowed to stand at 215-225°C for 2-3 h, and naturally cooled to room temperature to obtain an electromagnetic wire for wind power generation.
2. A process for preparing a magnet wire for wind power generation according to claim 1, It is characterized in that The reaction equation of the N-allyl hindered phenol in step (1) is:
3. A process for preparing a magnet wire for wind power generation according to claim 1, It is characterized in that The reaction equation of the functionalized polysiloxane in step (3) is:
4. A process for preparing a magnet wire for wind power generation according to claim 1, It is characterized in that The reaction equation of the modified polyetheretherketone in step (4) is: Where R is: