Substrate processing method and substrate processing apparatus

Through a three-step etching process, including the first etching, pattern shape processing and the second etching process, using a phosphoric acid treatment solution with a high silicon concentration, the problem of poor pattern shape of the silicon oxide film on the high-rise laminated substrate is solved, and the silicon oxide film is realized good shape retention.

CN118762990APending Publication Date: 2024-10-11TOKYO ELECTRON LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410684647.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2019-02-05
Filing Date
2020-02-04
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

In the prior art, in a substrate with a silicon nitride film and a silicon oxide film laminated in a high layer, the pattern shape of the silicon oxide film after etching treatment is not good, and the pattern shape may be undesirable due to the deposition of silicon oxide on the surface of the silicon oxide film.

Method used

A three-step etching treatment method is adopted: the first etching step is to form a silicon nitride film and a silicon oxide film by etching with an etching liquid, the second is to process the silicon oxide film with a pattern-shaping processing liquid, and the third is to further process the substrate in the second etching step, using Phosphoric acid treatment solutions with high silicon concentrations control silicon oxide deposition.

Benefits of technology

Even for highly stacked substrates, a good pattern shape of the silicon oxide film can be obtained, avoiding the deposition of silicon oxide on the surface of the silicon oxide film, ensuring the clarity and shape of the pattern.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118762990A_ABST
    Figure CN118762990A_ABST
Patent Text Reader

Abstract

The invention provides a substrate processing method and a substrate processing apparatus. The substrate processing method includes: a first etching step of etching a portion of a silicon nitride film in a substrate on which a silicon oxide film and the silicon nitride film are highly laminated by an etching solution; a processing step in which, after the first etching step, a pattern formed from the silicon oxide film on the substrate is processed with a pattern shape processing liquid to etch the tip of the silicon oxide film or the silicon oxide formed on the silicon oxide film in the first etching step; and a second etching step in which, after the processing step, a portion of the silicon nitride film on the substrate that is not etched in the first etching step is etched with an etching liquid, the pattern-shape processing liquid does not have or has low etching ability with respect to the silicon nitride film, and the pattern-shape processing liquid is a phosphoric acid-treated liquid having a high phosphoric acid concentration. The first etching step is performed until a tip portion of the pattern formed of the silicon oxide film is exposed, and the processing step processes the exposed tip portion.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of an application with a filing date of February 4, 2020, application number 202010079765.4, and invention name “Substrate processing method and substrate processing device”. Technical Field

[0002] Embodiments of the present disclosure relate to a substrate processing method and a substrate processing apparatus. Background Art

[0003] Conventionally, there is known a technique for etching a substrate by immersing the substrate in a phosphoric acid treatment solution containing silicon in a substrate treatment apparatus (see Patent Document 1).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2016-143684 Summary of the invention

[0007] Problem that the invention aims to solve

[0008] The present disclosure provides a technology capable of obtaining a good pattern shape of a silicon oxide film even on a substrate having a silicon nitride film and a silicon oxide film stacked at a high level.

[0009] Solutions for solving problems

[0010] A substrate processing method according to one embodiment of the present disclosure includes a first etching step, a processing step, and a second etching step. The first etching step etches a substrate having a silicon oxide film and a silicon nitride film formed thereon by an etching liquid. The processing step processes a pattern formed by the silicon oxide film in the substrate by a pattern shape processing liquid after the first etching step. The second etching step etches the substrate by an etching liquid after the processing step.

[0011] Effects of the Invention

[0012] According to the present disclosure, even in a substrate having a silicon nitride film and a silicon oxide film stacked on top of each other, a good pattern shape of the silicon oxide film can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 It is a schematic plan view of a substrate processing apparatus according to an embodiment.

[0014] Figure 2 It is a schematic block diagram showing the structure of a processing tank for etching according to an embodiment.

[0015] Figure 3A FIG. 1 is a schematic diagram showing a cross section of a wafer before etching.

[0016] Figure 3B It is a schematic diagram showing the state of the wafer as the etching process progresses.

[0017] Figure 3C This is a schematic diagram showing the state of the wafer as the etching process further progresses.

[0018] Figure 3D It is a schematic diagram showing the state of the wafer after the etching process is completed.

[0019] Figure 4A It is an enlarged cross-sectional view of the vicinity of a groove of a wafer before etching according to the embodiment.

[0020] Figure 4B It is an enlarged cross-sectional view of the vicinity of the groove of the wafer after the first etching process according to the embodiment.

[0021] Figure 4C This is an enlarged cross-sectional view of the vicinity of a groove of a wafer after processing according to the embodiment.

[0022] Figure 4D It is an enlarged cross-sectional view of the vicinity of the groove of the wafer after the second etching process according to the embodiment.

[0023] Figure 5 This is a diagram showing an example of the transition of the film thickness of the silicon oxide film when etching is performed using a phosphoric acid treatment solution having a relatively high silicon concentration.

[0024] Fig. 6A This is an enlarged cross-sectional view of the vicinity of a groove of a wafer before etching according to Modification 1 of the embodiment.

[0025] Figure 6B This is an enlarged cross-sectional view of the vicinity of the groove of the wafer after the first etching process according to Modification 1 of the embodiment.

[0026] Figure 6C This is an enlarged cross-sectional view of the vicinity of a groove of a processed wafer according to Modification 1 of the embodiment.

[0027] Fig.6D This is an enlarged cross-sectional view of the vicinity of the groove of the wafer after the second etching process according to Modification 1 of the embodiment.

[0028] Fig. 6E This is an enlarged cross-sectional view of the vicinity of a groove of a wafer after additional processing according to Modification 1 of the embodiment.

[0029] Fig. 7A This is an enlarged cross-sectional view of the vicinity of a groove of a wafer before etching according to Modification 2 of the embodiment.

[0030] Figure 7B This is an enlarged cross-sectional view of the vicinity of the groove of the wafer after the first etching process according to Modification 2 of the embodiment.

[0031] Figure 7C This is an enlarged cross-sectional view of the vicinity of a groove of a wafer after processing according to Modification 2 of the embodiment.

[0032] Fig.7D This is an enlarged cross-sectional view of the vicinity of the groove of the wafer after the second etching process according to Modification 2 of the embodiment.

[0033] Figure 8 It is a graph showing the film thickness of the silicon oxide film after etching in Modification 1 of the embodiment and the reference example.

[0034] Fig. 9 It is a diagram for explaining an etching process in the substrate processing apparatus according to the embodiment.

[0035] Fig.10 It is a diagram for explaining an etching process in the substrate processing apparatus according to Modification 1 of the embodiment.

[0036] Fig.11 It is a diagram for explaining an etching process in a substrate processing apparatus according to Modification 2 of the embodiment.

[0037] Fig.12 It is a diagram for explaining an etching process in a substrate processing apparatus according to Modification 3 of the embodiment.

[0038] Fig.13 This is a schematic block diagram showing a configuration of a substrate processing apparatus according to Modification 4 of the embodiment.

[0039] Fig.14 Detailed description of the invention is provided herein.

[0040] Fig.15 This is a flowchart showing a processing procedure of an etching process according to Modification 1 of the embodiment. DETAILED DESCRIPTION

[0041] Below, the embodiments of the substrate processing method and substrate processing device disclosed in the present application are described in detail with reference to the accompanying drawings. In addition, the present disclosure is not limited by the embodiments shown below. In addition, it should be noted that the accompanying drawings are schematic, and the relationship between the dimensions of each element, the ratio of each element, etc. are sometimes different from the actual ones. In addition, sometimes the drawings also include parts with different dimensional relationships and ratios.

[0042] Conventionally, there is known a technique for performing an etching process on a substrate by immersing the substrate in a phosphoric acid treatment solution containing silicon in a substrate treatment apparatus.

[0043] For example, by immersing the substrate in the phosphoric acid treatment solution, the silicon nitride film among the silicon nitride film (SiN) and the silicon oxide film (SiO 2 ) stacked on the substrate can be selectively etched.

[0044] However, when a silicon nitride film is selectively etched in a substrate in which a silicon nitride film and a silicon oxide film are stacked in multiple layers (hereinafter also referred to as a "high stack"), a path for discharging components of the etched silicon nitride film to the outside of the substrate becomes long.

[0045] Therefore, the silicon concentration in the phosphoric acid treatment solution entering the gaps between the silicon oxide films may increase, and silicon oxide may be deposited on the silicon oxide films. As a result, the pattern formed by the multi-layer silicon oxide films may not have a desired shape due to the deposited silicon oxide.

[0046] Therefore, it is expected that a good pattern shape of the silicon oxide film can be obtained even in a substrate having a high number of stacked silicon nitride films and silicon oxide films.

[0047] <Structure of substrate processing apparatus>

[0048] First, refer to Figure 1 The structure of the substrate processing apparatus 1 according to the embodiment will be described. Figure 1 1 is a schematic plan view of the substrate processing apparatus 1. In the following, in order to clarify the positional relationship, the X-axis, Y-axis, and Z-axis are defined to be orthogonal to each other, and the positive direction of the Z-axis is defined as the vertical upward direction.

[0049] like Figure 1 As shown, a substrate processing apparatus 1 according to the embodiment includes a carrier loading and unloading unit 2 , a substrate group forming unit 3 , a substrate group placing unit 4 , a substrate group conveying unit 5 , a substrate group processing unit 6 , and a control unit 7 .

[0050] The carrier loading / unloading unit 2 loads and unloads a carrier 9 that stores a plurality of (eg, 25) wafers W arranged vertically in a horizontal posture. The wafer W is an example of a substrate.

[0051] The carrier loading and unloading unit 2 includes a carrier stage 10, a carrier conveying mechanism 11, carrier stock 12, 13, and a carrier placement stage 14. The carrier stage 10 places a plurality of carriers 9 conveyed from the outside.

[0052] The carrier transport mechanism 11 transports the carrier 9 between the carrier stage 10, the carrier storage units 12 and 13, and the carrier placement stage 14. The carrier storage units 12 and 13 temporarily store the carrier 9.

[0053] The substrate group forming unit 3 includes a substrate transfer mechanism 15, and forms a substrate group in the substrate group forming unit 3. The substrate group is composed of a plurality of (eg, 50) wafers W that are simultaneously processed by combining wafers W accommodated in one or more carriers 9.

[0054] The substrate transport mechanism 15 transports a plurality of wafers W. The substrate transport mechanism 15 can change the posture of the wafer W from a horizontal posture to a vertical posture and from a vertical posture to a horizontal posture during the transport of the wafer W.

[0055] The substrate transfer mechanism 15 transfers the wafer W from the carrier 9 mounted on the carrier mounting table 14 to the substrate group mounting portion 4 . Also, the substrate transfer mechanism 15 transfers the wafer W from the substrate group mounting portion 4 to the carrier 9 mounted on the carrier mounting table 14 .

[0056] The substrate group placement section 4 has a substrate group transfer table 16 for temporarily placing (standing by) a substrate group transferred between the substrate group forming section 3 and the substrate group processing section 6 by the substrate group transfer section 5. The substrate group transfer table 16 has an inlet-side substrate group placement table 16a and an outlet-side substrate group placement table 16b.

[0057] The substrate group before being processed formed by the substrate group forming unit 3 is placed on the loading-side substrate group placement table 16a. The substrate group processed by the substrate group processing unit 6 is placed on the unloading-side substrate group placement table 16b. A plurality of wafers W corresponding to one substrate group are placed on the loading-side substrate group placement table 16a and the unloading-side substrate group placement table 16b in a front-to-back arrangement in a vertical posture.

[0058] The substrate group transporting unit 5 includes a substrate group transporting mechanism 17, which transports the substrate group between the substrate group placing unit 4 and the substrate group processing unit 6 and inside the substrate group processing unit 6. The substrate group transporting unit 5 is an example of a transporting unit. The substrate group transporting mechanism 17 includes a guide rail 17a, a moving body 17b, and a substrate holding body 17c.

[0059] The guide rail 17a is arranged along the X-axis direction across the substrate group placement unit 4 and the substrate group processing unit 6. The movable body 17b is configured to be movable along the guide rail 17a while holding a plurality of wafers W. The substrate holding body 17c is provided on the movable body 17b and holds a plurality of wafers W arranged in a vertical orientation.

[0060] The substrate group conveying unit 5 conveys the substrate group placed on the carrying-in side substrate group placing table 16a to the substrate group processing unit 6. The substrate group conveying unit 5 conveys the substrate group processed by the substrate group processing unit 6 to the carrying-out side substrate group placing table 16b. The substrate group conveying unit 5 conveys the substrate group inside the substrate group processing unit 6.

[0061] The substrate group processing unit 6 treats a plurality of wafers W arranged in a vertical orientation as one substrate group and performs etching, cleaning, drying, etc. In the substrate group processing unit 6, for example, two processing tanks 18 and one processing tank each 19 to 24 are arranged along the guide rail 17a.

[0062] The processing tank 18 is an example of the first processing tank and the third processing tank, and is used for etching the substrate group. A phosphoric acid treatment solution for etching (hereinafter also referred to as "etching solution") is stored in the processing tank 18. The processing tank 18 will be described in detail later.

[0063] The processing tanks 19 and 22 perform a rinsing treatment on the substrate group. The processing tanks 19 and 22 store a rinsing treatment liquid (e.g., pure water, etc.). The processing tank 20 is an example of a second processing tank, and is used to perform a processing treatment on the substrate group. The processing tank 20 stores a processing liquid for processing (hereinafter also referred to as a "pattern shape processing liquid").

[0064] The processing tank 21 performs a cleaning process on the substrate group. In the processing tank 21, a processing liquid for cleaning (for example, SC-1 (a mixed liquid of ammonia, hydrogen peroxide, and water) or the like) is stored.

[0065] The processing tank 23 performs drying processing of the substrate group. A drying processing gas (such as IPA (isopropyl alcohol)) is supplied to the processing tank 23. The processing tank 24 performs cleaning processing of the substrate holder 17c. A processing liquid and a drying gas for cleaning the substrate holder 17c are supplied to the processing tank 24.

[0066] Substrate lifting mechanisms 18a to 22a are provided in the processing tanks 18 to 22, respectively. The substrate lifting mechanisms 18a to 22a are configured to be movable upward and downward, and hold a plurality of wafers W forming a substrate group in a vertical orientation arranged front to back.

[0067] The substrate lifting mechanisms 18a to 22a are used to immerse the plurality of wafers W held in the processing liquid in the processing tanks 18 to 22. The substrate lifting mechanism 23a is used to expose the plurality of wafers W held in the processing tank 23 to the processing gas for drying. The substrate holder 17c is exposed to the processing liquid and the drying gas for cleaning in the processing tank 24.

[0068] Details of the processing of the wafer W using the processing tanks 18 to 23 will be described later. Figure 1 Example.

[0069] The control unit 7 controls the operation of each unit (the carrier loading and unloading unit 2, the substrate group forming unit 3, the substrate group placing unit 4, the substrate group conveying unit 5, the substrate group processing unit 6, etc.) of the substrate processing apparatus 1. The control unit 7 controls the operation of each unit of the substrate processing apparatus 1 based on signals from switches, various sensors, etc.

[0070] The control unit 7 is, for example, a computer, and includes a computer-readable storage medium 8. The storage medium 8 stores a program for controlling various processes executed in the substrate processing apparatus 1.

[0071] The control unit 7 controls the operation of the substrate processing apparatus 1 by reading and executing a program stored in the storage medium 8. The program may be stored in a computer-readable storage medium 8 or installed in the storage medium 8 of the control unit 7 from another storage medium.

[0072] Examples of the computer-readable storage medium 8 include a hard disk (HD), a floppy disk (FD), a compact disk (CD), a magneto-optical disk (MO), and a memory card.

[0073] <Structure of the etching treatment tank>

[0074] Next, refer to Figure 2 The etching treatment tank 18 will be described. Figure 2 It is a schematic block diagram showing the structure of the etching processing tank 18 according to the embodiment.

[0075] In the processing tank 18 , the silicon nitride film (SiN) and the silicon oxide film (SiO 2 ) formed on the wafer W are selectively etched using a predetermined etching solution.

[0076] In the etching process of the silicon nitride film, a phosphoric acid treatment solution obtained by adding a silicon (Si)-containing compound to a phosphoric acid (H 3 PO 4 ) aqueous solution to adjust the silicon concentration is used as an etching solution.

[0077] The etching solution may further contain silicon oxide R (see Figure 4B )'s redeposition additive.

[0078] As a method for adjusting the silicon concentration of the etching solution, a method of dissolving silicon by immersing a dummy wafer in a phosphoric acid aqueous solution (aging treatment) or a method of dissolving a silicon-containing compound such as colloidal silica in a phosphoric acid aqueous solution can be used. Alternatively, a silicon-containing compound aqueous solution can be added to the phosphoric acid aqueous solution to adjust the silicon concentration.

[0079] The etching treatment tank 18 includes a phosphoric acid aqueous solution supply unit 30 , a silicon supply unit 31 , a DIW supply unit 32 , an inner tank 34 , an outer tank 35 , a temperature adjustment tank 36 , and an etching liquid discharge unit 37 .

[0080] The phosphoric acid aqueous solution supply unit 30 includes a phosphoric acid aqueous solution supply source 30 a , a phosphoric acid aqueous solution supply line 30 b , and a flow rate regulator 30 c .

[0081] The phosphoric acid aqueous solution supply source 30a supplies phosphoric acid aqueous solution concentrated to a desired concentration. The phosphoric acid aqueous solution supply line 30b connects the phosphoric acid aqueous solution supply source 30a and the temperature adjustment tank 36 to supply the phosphoric acid aqueous solution from the phosphoric acid aqueous solution supply source 30a to the temperature adjustment tank 36.

[0082] The flow regulator 30c is provided in the phosphoric acid aqueous solution supply line 30b, and regulates the supply amount of the phosphoric acid aqueous solution to the temperature adjustment tank 36. The flow regulator 30c is composed of an on-off valve, a flow control valve, a flow meter, and the like.

[0083] The silicon supply unit 31 includes a silicon supply source 31 a , a silicon supply line 31 b , and a flow rate regulator 31 c .

[0084] The silicon supply source 31 a is a tank storing an aqueous solution of a silicon-containing compound. The silicon supply line 31 b connects the silicon supply source 31 a and the temperature adjustment tank 36 to supply the aqueous solution of a silicon-containing compound from the silicon supply source 31 a to the temperature adjustment tank 36 .

[0085] The flow regulator 31c is provided in the silicon supply line 31b, and is used to adjust the supply amount of the silicon-containing compound aqueous solution supplied to the temperature regulating tank 36. The flow regulator 31c is composed of an on-off valve or a flow control valve, a flow meter, etc. The supply amount of the silicon-containing compound aqueous solution is adjusted by the flow regulator 31c, thereby adjusting the silicon concentration of the etching solution.

[0086] Furthermore, the silicon supply unit 31 may be configured to supply the silicon-containing compound aqueous solution to the outer tank 35. Thus, when the silicon concentration of the etching solution decreases during the etching process, the silicon supply unit 31 can directly adjust the silicon concentration of the etching solution.

[0087] The DIW supply unit 32 includes a DIW supply source 32a, a DIW supply line 32b, and a flow rate regulator 32c. The DIW supply unit 32 supplies DIW (Deionized Water) to the outer tank 35 to replenish water evaporated by heating the etching liquid.

[0088] The DIW supply line 32 b connects the DIW supply source 32 a and the outer tank 35 , and supplies DIW at a predetermined temperature from the DIW supply source 32 a to the outer tank 35 .

[0089] The flow regulator 32c is provided in the DIW supply line 32b, and is used to adjust the supply amount of DIW supplied to the outer tank 35. The flow regulator 32c is composed of an on-off valve or a flow control valve, a flow meter, etc. The supply amount of DIW is adjusted by the flow regulator 32c, thereby adjusting the temperature, phosphoric acid concentration, and silicon concentration of the etching solution.

[0090] The upper portion of the inner tank 34 is open, and the etching liquid is supplied to the vicinity of the upper portion of the inner tank 34. In the inner tank 34, a plurality of wafers W are immersed in the etching liquid by the substrate lifting mechanism 18a, and the wafers W are etched.

[0091] The outer tank 35 is provided around the upper part of the inner tank 34, and the upper part of the outer tank 35 is open. The etching liquid overflowing from the inner tank 34 flows into the outer tank 35. In addition, the preliminary liquid is supplied from the temperature adjustment tank 36 to the outer tank 35, and the DIW is supplied from the DIW supply unit 32 to the outer tank 35.

[0092] A temperature sensor 35a and a phosphoric acid concentration sensor 35b are provided in the outer tank 35. The temperature sensor 35a detects the temperature of the etching solution, and the phosphoric acid concentration sensor 35b detects the phosphoric acid concentration of the etching solution. The signals generated by the temperature sensor 35a and the phosphoric acid concentration sensor 35b are sent to the control unit 7 (refer to Figure 1 ).

[0093] The outer tank 35 and the inner tank 34 are connected via a circulation line 40. One end of the circulation line 40 is connected to the outer tank 35, and the other end of the circulation line 40 is connected to a processing liquid supply nozzle 39 provided in the inner tank 34.

[0094] A pump 41 , a heater 42 , a filter 43 , and a silicon concentration sensor 44 are provided in the circulation line 40 in this order from the outer tank 35 side.

[0095] The pump 41 is used to form a circulation flow of the etching liquid sent from the outer tank 35 to the inner tank 34 via the circulation line 40. In addition, the etching liquid overflows from the inner tank 34 and flows out again to the outer tank 35. In this way, the circulation path 45 of the etching liquid is formed. That is, the circulation path 45 is formed by the outer tank 35, the circulation line 40 and the inner tank 34.

[0096] The heater 42 adjusts the temperature of the etching solution circulating in the circulation line 40. In the circulation path 45, the outer tank 35 is provided on the upstream side of the heater 42 with respect to the inner tank 34.

[0097] The filter 43 is used to filter the etching liquid circulating in the circulation line 40. The silicon concentration sensor 44 detects the silicon concentration of the etching liquid circulating in the circulation line 40. The signal generated by the silicon concentration sensor 44 is sent to the control unit 7.

[0098] For example, when all etching solutions in the inner tank 34 and the outer tank 35 are replaced, a preliminary solution in which a phosphoric acid aqueous solution and a silicon-containing compound aqueous solution are mixed is generated and stored in the temperature control tank 36. In addition, when a part of the etching solution is replaced during etching, for example, a phosphoric acid aqueous solution is stored in the temperature control tank 36 as a preliminary solution.

[0099] The temperature regulating tank 36 is connected to a circulation line 50 that circulates the preliminary liquid in the temperature regulating tank 36. A pump 51 and a heater 52 are provided in the circulation line 50. The pump 51 is used to form a circulation flow of the preliminary liquid that returns from the temperature regulating tank 36 to the temperature regulating tank 36 via the circulation line 50. The heater 52 adjusts the temperature of the preliminary liquid circulating in the circulation line 50.

[0100] In addition, the temperature adjustment tank 36 is connected to one end of the supply line 53. The other end of the supply line 53 is connected to the outer tank 35. The supply line 53 is provided with a pump 54 and a flow rate regulator 55.

[0101] The pump 54 causes the preliminary liquid to flow from the temperature regulating tank 36 to the outer tank 35. The flow regulator 55 regulates the amount of the preliminary liquid supplied to the outer tank 35. The flow regulator 55 is composed of an on-off valve or a flow control valve, a flow meter, etc. The amount of the preliminary liquid supplied is regulated by the flow regulator 55, thereby regulating the temperature, phosphoric acid concentration, and silicon concentration of the etching solution.

[0102] The etching liquid discharge unit 37 discharges the etching liquid when replacing all or part of the etching liquid used in the etching process. The etching liquid discharge unit 37 includes a discharge line 37a, a flow rate regulator 37b, and a cooling tank 37c.

[0103] The discharge line 37a is connected to the circulation line 40. The flow regulator 37b is provided on the discharge line 37a to adjust the discharge amount of the discharged etching liquid. The flow regulator 37b is composed of an on-off valve, a flow control valve, a flow meter, and the like.

[0104] The cooling tank 37c temporarily stores and cools the etching liquid flowing through the discharge line 37a. In the cooling tank 37c, the discharge amount of the etching liquid is adjusted by the flow regulator 37b.

[0105] <Overview of Etching Process>

[0106] Next, refer to Figure 3A to Figure 3D The etching process according to the embodiment will be described. Figure 3A FIG. 1 is a schematic diagram showing a cross section of a wafer W before an etching process is performed. Figure 3B FIG. 2 is a schematic diagram showing the state of the wafer W as the etching process progresses. Figure 3C FIG. 2 is a schematic diagram showing the state of the wafer W as the etching process further progresses. Figure 3DFIG. 2 is a schematic diagram showing the state of the wafer W after the etching process is completed.

[0107] like Figure 3A As shown, a plurality of silicon nitride films SiN and silicon oxide films SiO2 are alternately stacked on a wafer W before etching. In addition, a plurality of grooves Wa are formed on the wafer W for etching the stacked silicon nitride films SiN by inserting an etching solution.

[0108] When the wafer W is immersed in the inner tank 34 (see Figure 2 ) to start etching, such as Figure 3B As shown, first, the silicon nitride film SiN near the groove Wa is etched. That is, in the etching process, the silicon nitride film SiN is etched sequentially from the area near the groove Wa.

[0109] The components of the silicon nitride film SiN dissolved into the etching solution by etching are discharged from the gap Wb formed by etching the silicon nitride film SiN into the groove Wa, and are discharged from the groove Wa to the outside of the wafer W. Then, by replacing the etching solution in the groove Wa and the gap Wb with new etching solution, the etching of the silicon nitride film SiN progresses.

[0110] Therefore, as the etching process progresses, Figure 3C As shown in FIG. 1 , the distance from the etched portion to the groove Wa becomes longer. That is, the distance over which the components of the silicon nitride film SiN dissolved into the etching solution are discharged to the outside of the wafer W becomes longer.

[0111] Therefore, when the etching rate of the silicon nitride film SiN is high, the silicon concentration contained in the etching solution in the groove Wa and the gap Wb becomes high. In particular, the silicon concentration of the etching solution becomes high in the gap Wb at the bottom of the groove Wa formed at the inner side of the groove Wa, that is, at a position far from the surface of the wafer W.

[0112] Therefore, during the period when the etching solution containing the component of the silicon nitride film SiN dissolved by etching is discharged to the outside of the wafer W, the silicon oxide R (see Figure 4B ) is deposited on the surface of the silicon oxide film SiO2. In addition, when the etching process is further advanced, as Figure 3D As shown, the gaps Wb on both sides are connected.

[0113] <Details of etching process>

[0114] Next, refer to Figure 4A to Figure 13 The details of the etching process according to the embodiment will be described. Figure 4A 1 is an enlarged cross-sectional view of the vicinity of the groove Wa of the wafer W before etching according to the embodiment.

[0115] like Figure 4AAs shown in FIG. 1 , a wafer W before etching is alternately stacked with a plurality of silicon nitride films SiN and silicon oxide films SiO 2 .

[0116] Then, a memory hole M is formed at a predetermined position of the silicon oxide film SiO2, and the memory hole M is filled with a bulk oxide film. The memory hole M is a hole provided for three-dimensionally arranging a plurality of memory cells.

[0117] In the etching process of the embodiment, first, the first etching process using the above-mentioned phosphoric acid treatment solution is performed. Figure 4B FIG. 2 is an enlarged cross-sectional view of the vicinity of the groove Wa of the wafer W after the first etching process according to the embodiment. Figure 4B As shown, in the first etching process, the silicon nitride film SiN near the groove Wa is etched, and a gap Wb is formed near the groove Wa.

[0118] In the first etching process, the silicon oxide R is deposited on the front end E of the silicon oxide film SiO2 exposed from the groove Wa and the gap Wb. The silicon oxide R may prevent the pattern formed by the multilayer silicon oxide film SiO2 from having a desired shape.

[0119] For example, since the silicon oxide R blocks the entrance of the gap Wb, the etching liquid cannot be supplied to the inner side of the gap Wb, so that the etching of the silicon nitride film SiN located in the inner side of the gap Wb may not proceed.

[0120] Therefore, in the embodiment, the wafer W is processed using the pattern processing liquid after the first etching process. Figure 4C FIG. 2 is an enlarged cross-sectional view of the vicinity of the groove Wa of the wafer W after processing according to the embodiment. Figure 4C As shown, in the processing, the silicon oxide R deposited on the front end E of the silicon oxide film SiO2 is etched using the pattern processing liquid.

[0121] The pattern processing liquid of the embodiment is a processing liquid that can etch silicon oxide R and silicon oxide film SiO2 and has no etching ability or low etching ability for silicon nitride film SiN. Figure 4C As shown, the shape of the silicon nitride film SiN can be maintained during the processing.

[0122] The patterning liquid is, for example, DHF (Diluted HydroFluoric acid), SC1 (a mixed liquid of ammonia, hydrogen peroxide, and water), etc. The patterning liquid is not limited to DHF and SC1.

[0123] For example, in a phosphoric acid treatment liquid having a high phosphoric acid concentration, the etching selectivity ratio between the silicon nitride film SiN and the silicon oxide film SiO 2 is reversed, and thus the phosphoric acid treatment liquid having a high phosphoric acid concentration can be used as a pattern processing liquid.

[0124] Furthermore, in the embodiment, a second etching treatment is performed using a phosphoric acid treatment solution after the processing treatment. Figure 4D FIG. 2 is an enlarged cross-sectional view of the vicinity of the groove Wa of the wafer W after the second etching process according to the embodiment. Figure 4D As shown, in the second etching process, the entire silicon nitride film SiN is etched.

[0125] Furthermore, in the second etching process of the embodiment, unlike the first etching process described above, Figure 4D As shown in FIG. 1 , silicon oxide R is hardly deposited on the surface of the silicon oxide film SiO 2 . The reason for this is described below.

[0126] Figure 5 This is a diagram showing an example of the change in the film thickness of the silicon oxide film SiO2 when etching is performed with a phosphoric acid treatment solution with a relatively high silicon concentration. Based on this result, the following phenomenon is found: when etching is performed with an etching solution with a relatively high silicon concentration, silicon oxide R is indeed deposited on the surface of the silicon oxide film SiO2 in the initial stage, and the film thickness of the silicon oxide film SiO2 increases.

[0127] On the other hand, it is clear that when the initial stage of the etching process is passed, even if the silicon concentration is a relatively high concentration, the increase in the film thickness of the silicon oxide film SiO2 will converge. In other words, it is clear that when the initial stage of the etching process is passed (i.e., the implementation stage of the first etching process), the phenomenon of silicon oxide R deposited on the surface of the silicon oxide film SiO2 will converge.

[0128] This result is considered to be due to the following phenomenon occurring in the wafer W. In the initial stage of the etching process, since the etching amount of the silicon nitride film SiN is large relative to the volume of the groove Wa, the silicon concentration inside the groove Wa (especially the lower side of the groove Wa) tends to become high. Therefore, in the initial stage of the etching process, the phenomenon of silicon oxide R being deposited on the surface of the silicon oxide film SiO2 occurs.

[0129] On the other hand, when the initial stage of the etching process is passed, the volume of the groove Wa increases due to the formation of the gap Wb, and on the other hand, the etching amount of the silicon nitride film SiN does not change much compared to the initial stage, so the silicon concentration inside the groove Wa is relatively reduced. Therefore, it is considered that: when the initial stage of the etching process is passed, the phenomenon of silicon oxide R being deposited on the surface of the silicon oxide film SiO2 converges.

[0130] Through the etching process described above, in the embodiment, even in the case of a wafer W in which the silicon nitride film SiN and the silicon oxide film SiO 2 are stacked at a high level, a good pattern shape of the silicon oxide film SiO 2 can be obtained.

[0131] like Figure 4B As shown, the first etching process of the embodiment can be performed in such a way that the storage hole M formed in the silicon oxide film SiO2 is not exposed from the gap Wb. For example, in the embodiment, the first etching process can be performed until the front end E of the silicon oxide film SiO2 is exposed, and the exposed front end E is processed by processing.

[0132] This can prevent the bulk oxide film filling the memory hole M from being erroneously etched in the processing after the first etching processing.

[0133] Next, various modified examples of the etching process according to the embodiment will be described. Fig. 6A FIG. 2 is an enlarged cross-sectional view of the vicinity of the groove Wa of the wafer W before etching according to the first modification of the embodiment. Fig. 6A As shown, the wafer W before the etching process has a plurality of layers of silicon nitride films SiN and silicon oxide films SiO2 alternately stacked.

[0134] Then, in Modification 1, similarly to the above-described embodiment, first, a first etching process is performed using a phosphoric acid treatment solution. Figure 6B FIG. 2 is an enlarged cross-sectional view of the vicinity of the groove Wa of the wafer W after the first etching process according to the modification example 1 of the embodiment. Figure 6B As shown, in the first etching process, a gap Wb is formed near the groove Wa, and silicon oxide R is deposited at the front end portion E of the silicon oxide film SiO2.

[0135] Next, in Modification 1, processing is performed using a pattern processing liquid. Figure 6C It is an enlarged cross-sectional view of the vicinity of the groove Wa of the wafer W after the processing according to the first modification of the embodiment.

[0136] Here, in the processing of Modification Example 1, Figure 6C As shown, in addition to the silicon oxide R deposited on the front end E of the silicon oxide film SiO2, the front end E of the silicon oxide film SiO2 itself is also etched. As a result, the entrance of the gap Wb is expanded, so that the entrance of the gap Wb can be effectively prevented from being blocked by the silicon oxide R during the subsequent second etching process.

[0137] For example, in Modification 1, the processing time of the patterning liquid may be longer than that of the above-mentioned embodiment. In Modification 1, etching may be performed using a patterning liquid having an etching rate higher than that of the embodiment.

[0138] Next, in Modification 1, a second etching process is performed using a phosphoric acid treatment solution. Fig.6D FIG. 2 is an enlarged cross-sectional view of the vicinity of the groove Wa of the wafer W after the second etching process according to the modification example 1 of the embodiment. Fig.6D As shown, in the second etching process of Modification 1, the entire silicon nitride film SiN is etched.

[0139] exist Fig.6D 2 also shows a state where silicon oxide R is deposited again on the surface of the front end E of the silicon oxide film SiO2. For example, when a phosphoric acid treatment solution with a high silicon concentration is used as an etching solution, silicon oxide R is sometimes deposited on the silicon oxide film SiO2 even in the second etching process after the initial stage of etching.

[0140] Therefore, in Modification 1, after the second etching process, an additional processing step is performed using a patterning liquid. Fig. 6E It is an enlarged cross-sectional view of the vicinity of the groove Wa of the wafer W after the additional processing according to the first modification of the embodiment.

[0141] like Fig. 6E As shown, at least a portion of the silicon oxide R deposited on the surface of the front end E of the silicon oxide film SiO2 is removed by this additional processing. Through the etching process described so far, in Modification Example 1, even for a wafer W with a high layer of silicon nitride film SiN and silicon oxide film SiO2 stacked on top, a good pattern shape of the silicon oxide film SiO2 can be obtained.

[0142] In the additional processing of Modification 1, a patterning liquid having an etching rate lower than that of the patterning liquid in the processing can be used. This can prevent the bulk oxide film of the storage hole M exposed from the gap Wb from being erroneously etched during the additional processing.

[0143] In the additional processing of Modification 1, only the silicon oxide R deposited on the surface of the front end portion E of the silicon oxide film SiO 2 may be removed, and the silicon oxide film SiO 2 itself may not be etched.

[0144] For example, the time for the additional processing is set to be the same as or shorter than the time required to remove the silicon oxide R. This can prevent the pattern shape of the silicon oxide film SiO 2 from being excessively etched.

[0145] In the additional processing of Modification 1, the same type of patterning liquid as that of the processing may be used, or a different type of patterning liquid may be used.

[0146] Fig. 7AFIG. 2 is an enlarged cross-sectional view of the vicinity of the groove Wa of the wafer W before etching according to the second modification of the embodiment. Fig. 7A As shown, a plurality of silicon nitride films SiN and silicon oxide films SiO2 are alternately stacked in the wafer W before the etching process.

[0147] Then, in Modification 2, first, a first etching process is performed using a phosphoric acid treatment solution. Figure 7B It is an enlarged cross-sectional view of the vicinity of the groove Wa of the wafer W after the first etching process according to the second modification of the embodiment.

[0148] Here, if Figure 7B As shown, the first etching process of Modification 2 is performed by adjusting the components of the etching solution and the like so that silicon oxide R is not deposited on the front end E of the silicon oxide film SiO2.

[0149] For example, by using a phosphoric acid treatment solution having a low silicon concentration as an etching solution, the first etching treatment can be performed so that silicon oxide R is not deposited on the front end portion E.

[0150] Next, in Modification 2, processing is performed using a pattern processing liquid. Figure 7C FIG. 2 is an enlarged cross-sectional view of the vicinity of the groove Wa of the wafer W after processing according to the second modification of the embodiment. Figure 7C As shown, in the processing of Modification 2, the front end E of the silicon oxide film SiO2 is etched.

[0151] As a result, the entrance of the gap Wb is expanded, and thus it is possible to effectively prevent the entrance of the gap Wb from being clogged by the silicon oxide R during the subsequent second etching process.

[0152] Next, in Modification 2, a second etching process is performed using a phosphoric acid treatment solution. Fig.7D FIG. 2 is an enlarged cross-sectional view of the vicinity of the groove Wa of the wafer W after the second etching process according to the modification example 2 of the embodiment. Fig.7D As shown, in the second etching process of Modification 2, the entire silicon nitride film SiN is etched.

[0153] Through the etching process described above, in Modification 2, even in the case of the wafer W having a high stack of silicon nitride film SiN and silicon oxide film SiO 2 , a good pattern shape of the silicon oxide film SiO 2 can be obtained.

[0154] Figure 8 The graph shows the film thickness of silicon oxide film SiO2 after etching in Modification 1 of the embodiment and Reference Example. Here, the Reference Example is the film thickness of silicon oxide film SiO2 after etching with the same etching solution (temperature 120°C, silicon concentration 0.1%).

[0155] In Modification 1, the first etching process and the second etching process were performed using the same etching solution as in the reference example (processing time of the first etching process:processing time of the second etching process=5:95).

[0156] In addition, processing was performed between the first etching process and the second etching process, and additional processing was performed after the second etching process. In addition, processing was performed in a manner that silicon oxide R was etched by 5 nm using DHF 0.2%, and additional processing was performed for 600 seconds using SC1 (ammonia: hydrogen peroxide: water = 1:2:50) at a temperature of 65°C.

[0157] like Figure 8 As shown in the figure, in the reference example, the film thickness of the silicon oxide film SiO2 increases compared to the reference value (initial value of the film thickness of the silicon oxide film SiO2). It can be seen that the film thickness of the silicon oxide film SiO2 increases significantly in the center (Middle) and the front end (Edge) of the bottom (Bottom) of the groove Wa, and a good pattern shape of the silicon oxide film SiO2 is not obtained in the reference example.

[0158] On the other hand, in Modification 1, the film thickness of the silicon oxide film SiO2 is close to or lower than the reference value in all regions. Therefore, it can be seen that in Modification 1, a good pattern shape of the silicon oxide film SiO2 is obtained.

[0159] In addition, although there is no Figure 8 As shown in the figure, it can be seen that in the embodiment and the second modification, a good pattern shape of the silicon oxide film SiO2 can be obtained in the same manner as in the first modification.

[0160] Fig. 9 1 is a diagram for explaining etching processing in the substrate processing apparatus 1 according to the embodiment. Fig. 9 As shown in (a) of FIG. 1 , in the embodiment, one processing tank 18 and one processing tank 20 are prepared in the substrate processing apparatus 1 .

[0161] The processing tank 18 stores a phosphoric acid processing solution having silicon concentration and phosphoric acid concentration adjusted to predetermined concentrations as an etching solution, and the processing tank 20 stores DHF having a predetermined concentration as a patterning liquid.

[0162] Then, the control unit 7 Fig. 9 As shown in (a) of FIG. 1 , the substrate group conveying section 5 (see Figure 1 ) The wafer W is transported to the processing tank 18, and a first etching process is performed on the wafer W in the processing tank 18. Fig. 9Although not shown in the figure, the control unit 7 transfers the wafer W after the first etching process to the processing tank 19 via the substrate group transfer unit 5 , and performs a rinsing process on the wafer W in the processing tank 19 .

[0163] Next, the control unit 7 Fig. 9 As shown in (b) of FIG. 1 , the wafer W after the first etching process and the rinsing process is transported to the processing tank 20 by the substrate group transport unit 5, and the wafer W is processed in the processing tank 20. Then, the control unit 7 performs the following steps: Fig. 9 As shown in (c), the wafer W after the processing is transferred to the processing tank 18 by the substrate group transfer unit 5, and the wafer W is subjected to the second etching process in the processing tank 18.

[0164] Although the subsequent processing is omitted in the figure, the control unit 7 transfers the wafer W after the second etching process to the processing tank 19 through the substrate group transfer unit 5, and performs a rinsing process on the wafer W in the processing tank 19. Then, the control unit 7 transfers the wafer W after the rinsing process to the processing tank 21 using the substrate group transfer unit 5, and performs a cleaning process on the wafer W in the processing tank 21.

[0165] Finally, the control unit 7 transports the wafer W after the cleaning process to the processing tank 22 through the substrate group transport unit 5, and performs a rinsing process on the wafer W in the processing tank 22, and the etching process involved in the embodiment is completed. In addition, the wafer W after the etching process is transported to the processing tank 23 for drying, and then the wafer W is transported to the substrate group loading unit 4.

[0166] Fig.10 1 is a diagram for explaining etching processing in the substrate processing apparatus 1 according to the first modification of the embodiment. Fig.10 As shown in (a) of FIG. 1 , in Modification 1, one processing tank 18 and one processing tank 20 are prepared in the substrate processing apparatus 1 in the same manner as in the embodiment.

[0167] Then, a phosphoric acid treatment solution whose silicon concentration and phosphoric acid concentration are adjusted to predetermined concentrations is stored in the treatment tank 18 as an etching solution, and DHF whose concentration is adjusted to predetermined concentration is stored in the treatment tank 20 as a patterning liquid.

[0168] Then, the control unit 7 Fig.10 As shown in (a), the substrate group conveying unit 5 (refer to Figure 1 ) The wafer W is transported to the processing tank 18, and a first etching process is performed on the wafer W in the processing tank 18. Fig.10 Although not shown in the figure, the control unit 7 transfers the wafer W after the first etching process to the processing tank 19 via the substrate group transfer unit 5 , and performs a rinsing process on the wafer W in the processing tank 19 .

[0169] Next, the control unit 7 Fig.10 As shown in (b) of FIG. 1 , the wafer W after the first etching process and the rinsing process is transported to the processing tank 20 by the substrate group transport unit 5, and the wafer W is processed in the processing tank 20. Then, the control unit 7 performs the following steps: Fig.10 As shown in (c), the processed wafer W is transferred to the processing tank 18 by the substrate group transfer unit 5, and the wafer W is subjected to the second etching process in the processing tank 18.

[0170] Then, although in Fig.10 Although not shown in the figure, the control unit 7 transports the wafer W after the second etching process to the processing tank 19 through the substrate group transport unit 5, and performs a rinsing process on the wafer W in the processing tank 19. Then, the control unit 7 Fig.10 As shown in (d), the wafer W subjected to the second etching process and the rinsing process is transported to the processing tank 20 by the substrate group transport unit 5, and the wafer W is subjected to an additional processing in the processing tank 20.

[0171] Although the subsequent processing is omitted in the figure, the control unit 7 transfers the wafer W after the additional processing to the processing tank 21 through the substrate group transfer unit 5, and performs a cleaning process on the wafer W in the processing tank 21. Finally, the control unit 7 transfers the wafer W after the cleaning process to the processing tank 22 through the substrate group transfer unit 5, and performs a rinsing process on the wafer W in the processing tank 22, and the etching process involved in the modification example 1 is completed.

[0172] Fig.11 2 is a diagram for explaining etching processing in the substrate processing apparatus 1 according to the second modification of the embodiment. Fig.11 As shown in (a) of FIG. 1 , in the second modification, two processing tanks 18 (hereinafter referred to as processing tanks 18A and 18B) and one processing tank 20 are prepared in the substrate processing apparatus 1 .

[0173] Then, a phosphoric acid treatment liquid with a low silicon concentration is stored in the treatment tank 18A as an etching liquid, and a phosphoric acid treatment liquid with a silicon concentration higher than that of the phosphoric acid treatment liquid in the treatment tank 18A is stored in the treatment tank 18B as an etching liquid. The treatment tank 18A is an example of a first treatment tank, and the treatment tank 18B is an example of a third treatment tank. In addition, DHF adjusted to a predetermined concentration is stored in the treatment tank 20 as a pattern shape processing liquid.

[0174] Then, the control unit 7 Fig.11 As shown in (a) of FIG. 1 , the substrate group conveying section 5 (see Figure 1 ) The wafer W is transported to the processing tank 18A, and the first etching process is performed on the wafer W in the processing tank 18A. Fig.11Although not shown in the figure, the control unit 7 transfers the wafer W after the first etching process to the processing tank 19 via the substrate group transfer unit 5 , and performs a rinsing process on the wafer W in the processing tank 19 .

[0175] Next, the control unit 7 Fig.11 As shown in (b) of FIG. 1 , the wafer W after the first etching process and the rinsing process is transported to the processing tank 20 by the substrate group transport unit 5, and the wafer W is processed in the processing tank 20. Then, the control unit 7 performs the following steps: Fig.11 As shown in (c), the wafer W after the processing is transferred to the processing tank 18B by the substrate group transfer unit 5, and the wafer W is subjected to the second etching process in the processing tank 18B.

[0176] Although the subsequent processing is omitted in the figure, the control unit 7 transfers the wafer W after the second etching process to the processing tank 19 through the substrate group transfer unit 5, and performs a rinsing process on the wafer W in the processing tank 19. Then, the control unit 7 transfers the wafer W after the rinsing process to the processing tank 21 through the substrate group transfer unit 5, and performs a cleaning process on the wafer W in the processing tank 21.

[0177] Finally, the control unit 7 transfers the wafer W after the cleaning process to the processing tank 22 through the substrate group transfer unit 5, and performs a rinsing process on the wafer W in the processing tank 22, thereby completing the etching process according to the second modification.

[0178] exist Fig.11 In the example, as described above, the silicon concentration of the etching solution used in the first etching process can be set lower than the silicon concentration of the etching solution used in the second etching process.

[0179] Thus, it is possible to suppress the deposition of silicon oxide R on the surface of the silicon oxide film SiO 2 during the first etching process.

[0180] In addition, Fig.11 In the example of FIG. 1 , the temperature of the etching solution used in the first etching process can be set lower than the temperature of the etching solution used in the second etching process. In this way, the etching rate of SiN can be reduced to suppress the increase in local silicon concentration and suppress the deposition of silicon oxide R that is likely to occur in the early stage of the first etching process.

[0181] That is, the temperature of the etching solution used in the second etching process can be set higher than the temperature of the etching solution used in the first etching process. As a result, the saturation concentration of silicon relative to the etching solution can be increased. Therefore, the silicon concentration of the etching solution in the second etching process can be made higher than the silicon concentration of the etching solution in the first etching process.

[0182] Furthermore, when the second etching process is performed, the etching rate of the silicon nitride film SiN can be increased, so that the processing time of the second etching process can be shortened.

[0183] In addition, Fig.11 The example shows the case where two processing tanks 18 are used in the etching process of Modification Example 2, but the etching process of Modification Example 2 may also be performed using one processing tank 18 as in the embodiment and Modification Example 1.

[0184] In this case, the silicon concentration of the etching solution stored in one treatment tank 18 can be increased during the second etching process compared to the silicon concentration during the first etching process. In addition, the temperature of the etching solution stored in one treatment tank 18 can be increased during the second etching process compared to the temperature during the first etching process.

[0185] In addition, not limited to the case of Modification 2, in the embodiment and Modification 1, the silicon concentration of the etching solution stored in one treatment tank 18 may be increased during the second etching process compared to the silicon concentration during the first etching process. In addition, the temperature of the etching solution stored in one treatment tank 18 may be increased during the second etching process compared to the temperature during the first etching process.

[0186] And, in Fig.11 The example shown in FIG. 1 shows a case where two processing tanks 18 are used for etching processing, but three or more processing tanks 18 may be used for etching processing. Fig.12 It is a diagram for explaining an etching process in the substrate processing apparatus 1 according to Modification 3 of the embodiment.

[0187] like Fig.12 As shown in (a) of FIG. 1 , in the modification 3, one processing bath 18A, three processing baths 18B ( 18B1 to 18B3 ), and one processing bath 20 are prepared in the substrate processing apparatus 1 .

[0188] A phosphoric acid treatment liquid with a low silicon concentration is stored in treatment tank 18A as an etching liquid, and a phosphoric acid treatment liquid with a higher silicon concentration than that in treatment tank 18A is stored in treatment tanks 18B1 to 18B3 as an etching liquid. In addition, DHF adjusted to a predetermined concentration is stored in treatment tank 20 as a patterning liquid.

[0189] Then, the control unit 7 Fig.12 As shown in (a) of FIG. 1 , the substrate group conveying section 5 (see Figure 1 ) The wafer W1 is transferred to the processing tank 18A, and a first etching process is performed on the wafer W1 in the processing tank 18A.

[0190] Next, the control unit 7 transfers the wafer W1 from the processing tank 18A to the processing tank 19 (not shown) and performs a rinsing process on the wafer W1. Fig.12 As shown in (b) of FIG. 8 , the wafer W1 is transferred to the processing tank 20 by the substrate group transfer unit 5 , and the wafer W1 is processed in the processing tank 20 .

[0191] At this time, the control unit 7 causes the substrate group transport unit 5 to transport the wafer W2 of another substrate group to the empty processing tank 18A, and performs the first etching process on the wafer W2 in the processing tank 18A.

[0192] Then, if Fig.12 As shown in (c), the control unit 7 transfers the wafer W1 to the processing tank 18B1 via the substrate group transfer unit 5, and performs the second etching process on the wafer W1 in the processing tank 18B1.

[0193] At this time, after the control unit 7 transfers the wafer W2 from the processing tank 18A to the processing tank 19 (not shown) through the substrate group conveying unit 5 and performs a rinsing process on the wafer W2, the control unit 7 transfers the wafer W2 to the processing tank 20 through the substrate group conveying unit 5 and performs a processing process on the wafer W2 in the processing tank 20.

[0194] Furthermore, at this time, the control unit 7 causes the substrate group transport unit 5 to transport the wafer W3 of another substrate group to the empty processing tank 18A, and performs the first etching process on the wafer W3 in the processing tank 18A.

[0195] Here, the second etching process takes longer time than the first etching process and subsequent processing (for example, several to dozens of times longer than the first etching process). Therefore, when the first etching process and processing of the wafer W2 are completed, the second etching process of the wafer W1 is not completed.

[0196] Therefore, in Variation 3, Fig.12 As shown in (d), the wafer W2 after the first etching and processing is transported to another processing tank 18B2 by the substrate group transport unit 5, and the second etching is performed. Thus, the second etching can be performed on the wafer W2 that is put in later without waiting until the second etching of the wafer W1 that was put in earlier is finished.

[0197] In addition, at this time, after the control unit 7 transfers the wafer W3 from the processing tank 18A to the processing tank 19 (not shown) through the substrate group conveying unit 5 and performs a rinsing treatment on the wafer W3, the control unit 7 transfers the wafer W3 to the processing tank 20 through the substrate group conveying unit 5 and performs a processing treatment on the wafer W3 in the processing tank 20.

[0198] Then, if Fig.12As shown in (e), the control unit 7 further transfers the wafer W3 from the processing tank 20 to another processing tank 18B3 via the substrate group transfer unit 5, and performs the second etching process on the wafer W3 in the processing tank 18B3.

[0199] Thus, the second etching process can be performed on the wafer W3 that is subsequently introduced without waiting until the second etching process of the previously introduced wafers W1 and W2 is completed. Figures 9 to 11 The examples are the same as those in FIG. 1 , so the description is omitted.

[0200] As described so far, in Modification 3, more processing tanks 18 (processing tanks 18B1 to 18B3 ) for performing the second etching process are provided than the processing tank 18 (processing tank 18A) for performing the first etching process.

[0201] Thus, the second etching process can be performed on the wafer W that is subsequently loaded without waiting until the second etching process on the previously loaded wafer W is completed. Therefore, according to Modification 3, the throughput of the etching process can be improved.

[0202] In addition, Fig.12 In the example shown in FIG. 1 , three processing tanks 18B for performing the second etching process are provided. However, the number of processing tanks 18B for performing the second etching process is not limited to three.

[0203] In the embodiment and various modifications described above, the case where the etching process on the wafers W is performed by batch processing has been described. However, the etching process of the embodiment and various modifications may be performed by single processing.

[0204] Fig.13 1A is a schematic block diagram showing a structure of a substrate processing apparatus 1A according to a fourth modification of the embodiment. Fig.13 In, with Figure 2 The same parts in the illustrated embodiments are denoted by the same reference numerals, and detailed descriptions thereof are omitted.

[0205] exist Fig.13 In the substrate processing apparatus 1A shown, the outer tank 35 is connected to the phosphoric acid aqueous solution supply unit 30, the silicon supply unit 31, and the DIW supply unit 32. In addition, the outer tank 35 is connected to the circulation line 40. Thus, the etching solution whose temperature, phosphoric acid concentration, and silicon concentration are adjusted is stored in the outer tank 35.

[0206] In the substrate processing apparatus 1A, the etching liquid stored in the outer tank 35 is supplied to the single-sheet processing unit 61 via the supply line 60. The supply line 60 includes a flow rate regulator 60a. The single-sheet processing unit 61 includes a substrate holding unit 62 and a rotating mechanism 63.

[0207] The substrate holding portion 62 holds the wafer W horizontally. The rotating mechanism 63 rotates the substrate holding portion 62 and the wafer W held by the substrate holding portion 62. Then, the etching liquid is sprayed from the outer tank 35 via the supply line 60 to the upper surface of the wafer W held by the substrate holding portion 62, thereby performing the first etching process and the second etching process on the wafer W.

[0208] Furthermore, the single-sheet processing section 61 is connected to a rinse liquid supply section 70 , a pattern shape processing liquid supply section 71 , and a cleaning liquid supply section 72 .

[0209] The rinse liquid supply unit 70 includes a rinse liquid supply source 70 a , a rinse liquid supply line 70 b , and a flow rate regulator 70 c . The rinse liquid supply unit 70 is operated to spray the rinse liquid onto the upper surface of the wafer W held by the substrate holding unit 62 , thereby rinsing the wafer W.

[0210] The pattern processing liquid supply unit 71 includes a pattern processing liquid supply source 71a, a pattern processing liquid supply line 71b, and a flow rate regulator 71c. The pattern processing liquid supply unit 71 is operated to spray the pattern processing liquid onto the upper surface of the wafer W held by the substrate holding unit 62, thereby performing processing and additional processing on the wafer W.

[0211] The cleaning liquid supply unit 72 includes a cleaning liquid supply source 72a, a cleaning liquid supply line 72b, and a flow rate regulator 72c. The cleaning liquid supply unit 72 is operated to spray the cleaning liquid onto the upper surface of the wafer W held by the substrate holding unit 62, thereby cleaning the wafer W.

[0212] Furthermore, the control unit 7 can control the single-sheet processing unit 61 , the flow rate regulators 60 a , 70 c to 72 c , and the like to perform the etching process of the above-described embodiment and various modifications on the wafer W.

[0213] The substrate processing device 1 involved in the embodiment includes a first processing tank (processing tank 18), a second processing tank (processing tank 20), a conveying unit (substrate group conveying unit 5) and a control unit 7. In the first processing tank (processing tank 18), an etching process is performed by immersing a substrate (wafer W) formed with a silicon oxide film SiO2 and a silicon nitride film SiN in an etching liquid. In the second processing tank (processing tank 20), the following processing is performed: a pattern formed by the silicon oxide film SiO2 in the substrate (wafer W) is processed by a pattern shape processing liquid. The conveying unit (substrate group conveying unit 5) conveys the substrate (wafer W) to the first processing tank (processing tank 18) and the second processing tank (processing tank 20). The control unit 7 controls the first processing tank (processing tank 18), the second processing tank (processing tank 20) ​​and the conveying unit (substrate group conveying unit 5). In addition, the control unit 7 controls the conveying unit (substrate group conveying unit 5) to convey the substrate (wafer W) to the first processing tank (processing tank 18), to convey the substrate conveyed to the first processing tank to the second processing tank (processing tank 20), and to convey the substrate conveyed to the second processing tank (processing tank 20) ​​to the first processing tank. Thus, even for the wafer W having a high layer of silicon nitride film SiN and silicon oxide film SiO2 stacked, a good pattern shape of the silicon oxide film SiO2 can be obtained.

[0214] In addition, the substrate processing device 1 involved in the embodiment includes a first processing tank (processing tank 18A), a second processing tank (processing tank 20), a third processing tank (processing tank 18B), a conveying unit (substrate group conveying unit 5) and a control unit 7. In the first processing tank (processing tank 18A), an etching process is performed by immersing a substrate (wafer W) formed with a silicon oxide film SiO2 and a silicon nitride film SiN in an etching solution. In the second processing tank (processing tank 20), the following processing is performed: a pattern formed by the silicon oxide film SiO2 in the substrate (wafer W) is processed by a pattern shape processing liquid. In the third processing tank (processing tank 18B), an etching process is performed by immersing the substrate (wafer W) in an etching solution. The conveying unit (substrate group conveying unit 5) conveys the substrate (wafer W) to the first processing tank (processing tank 18A), the second processing tank (processing tank 20) ​​and the third processing tank (processing tank 18B). The control unit 7 controls the first processing tank (processing tank 18A), the second processing tank (processing tank 20), the third processing tank (processing tank 18B), and the conveying unit (substrate group conveying unit 5). In addition, the control unit 7 controls the conveying unit (substrate group conveying unit 5) to convey the substrate (wafer W) to the first processing tank (processing tank 18A), to convey the substrate conveyed to the first processing tank to the second processing tank (processing tank 20), and to convey the substrate conveyed to the second processing tank to the third processing tank (processing tank 18B). Thus, even for a wafer W having a high layer of silicon nitride film SiN and silicon oxide film SiO2 stacked on top, a good pattern shape of silicon oxide film SiO2 can be obtained.

[0215] In addition, in the substrate processing apparatus 1 according to the embodiment, the third processing tanks (processing tanks 18B) are provided in a larger number than the first processing tanks (processing tanks 18A), so that the wafer W can be smoothly etched without waiting for processing in the substrate processing apparatus 1.

[0216] <Details of etching process>

[0217] Next, refer to Fig.14 and Fig.15 Details of the etching process performed by the substrate processing apparatus 1 according to the embodiment will be described. Fig.14 Detailed description of the invention is provided herein.

[0218] First, the control unit 7 uses a predetermined etching liquid to perform a first etching process on the wafer W (step S101). Next, the control unit 7 uses a predetermined rinsing liquid to perform a rinsing process on the wafer W (step S102). Then, the control unit 7 uses a predetermined pattern shape processing liquid to perform a processing process on the wafer W (step S103).

[0219] Next, the control unit 7 performs a second etching process on the wafer W using a predetermined etching liquid (step S104 ). Then, the control unit 7 performs a rinsing process on the wafer W using a predetermined rinsing liquid (step S105 ).

[0220] Next, the control unit 7 uses a predetermined cleaning liquid to perform a cleaning process on the wafer W (step S106 ). Finally, the control unit 7 uses a predetermined rinse liquid to perform a rinse process on the wafer W (step S107 ), and the process is completed.

[0221] Fig.15 This is a flowchart showing a processing procedure of an etching process according to Modification 1 of the embodiment.

[0222] First, the control unit 7 uses a predetermined etching liquid to perform a first etching process on the wafer W (step S201). Next, the control unit 7 uses a predetermined rinsing liquid to perform a rinsing process on the wafer W (step S202). Then, the control unit 7 uses a predetermined pattern shape processing liquid to perform a processing process on the wafer W (step S203).

[0223] Next, the control unit 7 performs a second etching process on the wafer W using a predetermined etching liquid (step S204 ). Then, the control unit 7 performs a rinsing process on the wafer W using a predetermined rinsing liquid (step S205 ).

[0224] Next, the control unit 7 performs additional processing on the wafer W using a predetermined pattern processing liquid (step S206 ). Then, the control unit 7 performs cleaning processing on the wafer W using a predetermined cleaning liquid (step S207 ).

[0225] Finally, the control unit 7 performs a rinsing process on the wafer W using a predetermined rinsing liquid (step S208 ), and the process is completed.

[0226] The substrate processing method involved in the embodiment includes a first etching process, a processing process, and a second etching process. In the first etching process, a substrate (wafer W) formed with a silicon oxide film SiO2 and a silicon nitride film SiN is etched by an etching liquid. In the processing process, a pattern formed by the silicon oxide film SiO2 in the substrate (wafer W) is processed by a pattern shape processing liquid after the first etching process. In the second etching process, the substrate (wafer W) is etched by an etching liquid after the processing process. Thus, even for a wafer W with a high layer of silicon nitride film SiN and silicon oxide film SiO2, a good pattern shape of the silicon oxide film SiO2 can be obtained.

[0227] In the substrate processing method according to the embodiment, the pattern processing liquid has no etching capability or low etching capability for the silicon nitride film SiN, thereby being able to maintain the shape of the silicon nitride film SiN during processing.

[0228] In addition, in the substrate processing method according to the embodiment, the first etching step is performed until the front end E of the pattern formed by the silicon oxide film SiO2 is exposed, and the processing step processes the exposed front end E. Thus, it is possible to prevent the bulk oxide film filling the storage hole M from being erroneously etched in the processing after the first etching process.

[0229] In addition, in the substrate processing method according to the embodiment, the temperature of the etching solution in the first etching step is set lower than the temperature of the etching solution in the second etching step. Thus, by reducing the etching rate of SiN in the first etching step, the increase in local silicon concentration can be suppressed in the initial stage, thereby suppressing the deposition of silicon oxide R.

[0230] In the substrate processing method according to the embodiment, the silicon concentration of the etching solution in the first etching step is set lower than the silicon concentration of the etching solution in the second etching step. This can suppress the deposition of silicon oxide R on the surface of the silicon oxide film SiO2 during the first etching process.

[0231] In addition, the substrate processing method according to the embodiment further includes an additional processing step of processing the pattern formed by the silicon oxide film SiO2 using a pattern shape processing liquid after the second etching step. Thus, the silicon oxide R deposited on the surface of the front end E of the silicon oxide film SiO2 can be removed after the second etching process.

[0232] In addition, in the substrate processing method according to the embodiment, the etching solution includes phosphoric acid and an additive for suppressing the redeposition of silicon oxide R. Thus, the silicon nitride film SiN can be etched with a high selectivity relative to the silicon oxide film SiO2, and the deposition of silicon oxide R on the silicon oxide film SiO2 can be suppressed.

[0233] In the substrate processing method according to the embodiment, the processing time in the additional processing step is set to the time for processing only the silicon oxide R formed on the surface of the silicon oxide film SiO2. This can prevent the pattern shape of the silicon oxide film SiO2 from being excessively etched.

[0234] In addition, in the additional processing step, as a method of processing only the silicon oxide R formed on the surface of the silicon oxide film SiO2, the etching rate of the patterning liquid can be reduced, and the additional processing step can be performed using a patterning liquid with a high silicon concentration.

[0235] The above is a description of the embodiments of the present disclosure, but the present disclosure is not limited to the above embodiments, and various changes can be made without departing from the main purpose. For example, in the above embodiments, an example of using a solution obtained by adding a silicon-containing compound to a phosphoric acid aqueous solution to adjust the silicon concentration is shown as an etching solution, but a SiO2 deposition inhibitor or the like may also be added to the etching solution.

[0236] It should be considered that all the aspects of the embodiments disclosed this time are illustrative and not restrictive. In fact, the above embodiments can be specifically implemented in many ways. In addition, the above embodiments can also be omitted, replaced, and changed in various ways without departing from the attached claims and their main purpose.

[0237] Description of Reference Numerals

[0238] 1, 1A: substrate processing device; 5: substrate group transport unit (an example of a transport unit); 7: control unit; 18, 18A: processing tank (an example of a first processing tank); 18B, 18B1~18B3: processing tank (an example of a third processing tank); 20: processing tank (an example of a second processing tank); W, W1~W3: wafer (an example of a substrate); SiN: silicon nitride film; SiO2: silicon oxide film.

Claims

1. A substrate processing method, comprising: A first etching step of etching a portion of the silicon nitride film in a substrate on which a silicon oxide film and a silicon nitride film are stacked with an etching solution; a processing step of processing a pattern formed by the silicon oxide film in the substrate by a pattern shape processing liquid after the first etching step, so as to etch a front end portion of the silicon oxide film or silicon oxide formed on the silicon oxide film in the first etching step; as well as a second etching step of etching, after the processing step, a portion of the silicon nitride film on the substrate that was not etched in the first etching step using an etching solution, The pattern processing liquid has no etching ability or low etching ability for the silicon nitride film, and the pattern processing liquid is a phosphoric acid treatment liquid with a high phosphoric acid concentration. The first etching step is performed until the front end of the pattern formed by the silicon oxide film is exposed, The processing step processes the exposed front end portion.

2. The substrate processing method according to claim 1, characterized in that: The front end portion after processing is etched so that the entrance area is expanded in a rectangular or trapezoidal shape compared with the inner area.

3. The substrate processing method according to claim 1, characterized in that: The temperature of the etching solution in the first etching step is set lower than the temperature of the etching solution in the second etching step.

4. The substrate processing method according to claim 1, characterized in that: The silicon concentration of the etching solution in the first etching step is set lower than the silicon concentration of the etching solution in the second etching step.

5. The substrate processing method according to claim 1, characterized in that: The etching solution includes phosphoric acid and an additive for inhibiting redeposition of silicon oxide.

6. The substrate processing method according to claim 1, characterized in that: The first etching step, the second etching step, and the processing step are performed in at least one groove.

7. A substrate processing device comprising: The first processing tank, the second processing tank and the third processing tank, in which the substrate having a high-layer stack of silicon oxide film and silicon nitride film is immersed in an etching solution to perform etching treatment, the etching treatment comprising: a first etching process for etching a portion of the silicon nitride film in the substrate; and a second etching process for etching a portion of the silicon nitride film in the substrate that was not etched in the first etching process, wherein a processing process for processing a pattern formed by the silicon oxide film in the substrate by a pattern shape processing liquid is further performed in the first processing tank, the second processing tank, and the third processing tank, wherein the processing process is for etching a front end portion of the silicon oxide film or silicon oxide formed on the silicon oxide film in the first etching process; A conveying unit, which conveys the substrate to the first processing tank, the second processing tank, and the third processing tank; as well as a control unit that controls the first processing tank, the second processing tank, the third processing tank, and the conveying unit, wherein the control unit controls the conveying unit to convey the substrate to the first processing tank, the second processing tank, and the third processing tank to perform the first etching treatment, the second etching treatment, and the processing treatment, The pattern processing liquid has no etching ability or low etching ability for the silicon nitride film, and the pattern processing liquid is a phosphoric acid treatment liquid with a high phosphoric acid concentration. performing the first etching process until the front end of the pattern formed by the silicon oxide film is exposed, The processing is to process the exposed front end portion.