Carbon-coated aluminum foil current collector for lithium battery and preparation method of carbon-coated aluminum foil current collector

By coating the conductive carbon material modified graphene oxide layer in the lithium battery cathode current collector, the problem of insufficient adhesion between the aluminum foil and the cathode material is solved, the cycle life and rate performance of the lithium battery are improved, and a higher Conductivity and wear resistance.

CN118763230APending Publication Date: 2024-10-11NANNING IND INVESTMENT ALUMINUM FOIL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410851218.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The existing lithium battery cathode current collector has insufficient adhesion between the aluminum foil and the cathode material, high contact resistance, poor wettability, and low strength, which affects the electrochemical performance of the battery.

Method used

By coating a conductive carbon material modified graphene oxide layer on the surface of the aluminum foil, the cage structure of POSS and the reaction site of the amide compound are used to improve the adhesion, conductivity and wear resistance of the coating, and enhance the lithium ion diffusion rate.

Benefits of technology

It improves the cycle life, energy density and rate performance of lithium batteries, reduces the internal resistance of the battery, and enhances the binding ability of the coating to the positive active material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides a carbon-coated aluminum foil current collector for a lithium battery and a preparation method of the carbon-coated aluminum foil current collector, and belongs to the technical field of lithium batteries, the carbon-coated aluminum foil current collector comprises a matrix aluminum foil and a coating coated on the matrix, and the formula of the coating comprises the following components in percentage by weight: 15-25 parts of polyurethane resin, 5-20 parts of conductive carbon material modified graphene oxide, 0.5-2 parts of a thickening agent and 40-65 parts of a solvent. According to the present invention, the POSS is modified by using the epoxy group-containing substance, such that the reactive group is obtained on the POSS, the reactive group can participate in the reaction with the amide compound and the graphene oxide so as to improve the dispersibility of the graphene oxide in the slurry, and the POSS has characteristics of cage structure, high strength and wear resistance, such that the specific surface can be increased, the adhesion of the coating can be improved, the conductivity is high, and the solvent resistance is provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium batteries, and in particular to a carbon-coated aluminum foil current collector for lithium batteries and a preparation method thereof. Background Art

[0002] Metal aluminum foil is light in weight, low in price, has good mechanical strength and ductility, high electronic conductivity and electrochemical stability, and is therefore widely used in positive current collectors of lithium batteries. However, there are defects such as insufficient adhesion between aluminum foil and the positive electrode material, high contact resistance, poor wettability, low strength, and chemical corrosion resistance, which seriously affect the electrochemical performance of the battery. In order to solve the above-mentioned problems, carbon-coated aluminum foil came into being. By adding a layer of carbon coating on the surface of the aluminum foil, the interface impedance of the current collector can be reduced, polarization can be reduced, and the cycle life and rate performance can be improved. However, the existing coating technology has the problems of limited contact area between conventional aluminum foil and slurry, insufficient adhesion, and low strength, which leads to obstructed electron transmission, powder loss of the pole piece, and affects battery performance.

[0003] Cage-type polysilsesquioxane (POSS) is a type of "organic / inorganic" nanohybrid material prepared by hydrolysis and condensation of siloxane, which has a cage-type rigid structure and organic groups modified on the silicon oxide skeleton. A series of amino-containing POSS with high reactivity can be prepared using amino-containing siloxane. Since the organic group R at the Si vertex in POSS has strong structural designability, it provides great potential and possibility for the preparation of high-performance POSS.

[0004] Therefore, in response to the defects of the carbon-coated aluminum foil mentioned above, this patent develops a positive electrode current collector surface coating with strong adhesion, high conductivity, good mechanical properties, solvent resistance and alkali resistance, which has positive significance for improving the cycle life of lithium batteries, increasing the energy density of lithium batteries, and improving the rate performance of lithium batteries. Summary of the invention

[0005] The purpose of the present invention is to provide a carbon-coated aluminum foil current collector for lithium batteries and a preparation method thereof, so as to solve the technical problems mentioned in the background technology. A carbon-coated aluminum foil current collector for lithium batteries with high bonding strength and high surface and a preparation method thereof are provided, and the POSS with a cage structure is first modified to provide chemical sites for subsequent reaction with graphene oxide. By modifying graphene oxide, a highly conductive carbon material-modified graphene oxide is obtained, which increases its dispersibility in the carbon-coated slurry, increases the specific surface area and corrosion resistance, improves the wear resistance and adhesion of the coating, and facilitates the subsequent combination with the positive electrode active material, improves the conductivity and energy density of the material, and increases the lithium ion diffusion rate.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0007] A carbon-coated aluminum foil current collector for lithium battery comprises an aluminum foil substrate and a coating coated on the substrate. The coating comprises, by weight percentage, 15-25 parts of a polyurethane resin, 5-20 parts of conductive carbon material-modified graphene oxide, 0.5-2 parts of a thickener and 40-65 parts of a solvent.

[0008] Further, the conductive carbon material modified graphene oxide is prepared by the following steps:

[0009] (1) Preparation of octaamine-based POSS;

[0010] (2) Preparation of octaamine POSS aminated compounds;

[0011] (3) Preparation of graphene oxide;

[0012] (4) Preparation of amide compounds;

[0013] (5) Conductive carbon material modified graphene oxide is prepared by using octaamine-based POSS amine compound, graphene oxide and amide compound in the presence of a catalyst.

[0014] Furthermore, the specific process of preparing the octaamino POSS in step (1) is as follows: 30 ml of APTES and 240 ml of anhydrous methanol are added to a 500 ml three-necked flask, stirring is started at a speed of 800 rpm, and then 41 ml of HCl is added dropwise to the solution for reaction. The reaction time is 2 days, and stirring is stopped after a white precipitate appears. The reaction is allowed to stand for 5-10 days to stop. Finally, the suspension is filtered and washed with anhydrous methanol to obtain a white powder product, the octaamino POSS, with a yield of 75-85%.

[0015] Furthermore, the specific process for preparing the octaamino POSS amine compound in step (2) is as follows: octaamino POSS and an epoxy group-containing compound are added into a flask at a mass ratio of 1:1.1-1.2, and then an alkali catalyst DBU is added in an amount of 0.5% of the total reactants and an organic solvent is added in an amount of 1.3-1.5 times of the total reactants. After stirring for 0.5-1h, the epoxy group-containing compound is added, and the stirring reaction is continued at room temperature for 1-2h to obtain the product octaamino POSS amine compound.

[0016] Furthermore, the specific process of preparing graphene oxide in step (3) is as follows: 80 ml of concentrated sulfuric acid is added to a three-necked flask placed in an ice water bath, and then 3 g of natural graphite and 2 g of NaNO are added while stirring. 3 , keep the system temperature below 5°C, and then add 8g KMnO in small amounts to the reaction several times. 4, and then continue to react at below 5°C for 2h, heat the system to 35-40°C, react for 3-5h, add 300ml of deionized water several times, and heat the system to 90-100°C, react for 30min, cool to room temperature, add 10ml of hydrogen peroxide, continue stirring for 20min and then end the reaction to obtain graphene oxide, then pour all the system substances into a beaker, add 300ml of deionized water to dilute, precipitate several times, centrifuge, measure the pH value close to 7, dig out the solid and put it in a culture dish, put it in a vacuum oven to dry for 24h and set aside.

[0017] Furthermore, the specific process for preparing the amide compound in step (4) is as follows: adding a methacrylate compound and a basic amino acid in a mass ratio of 2-2.4:1 to a reaction bottle, and then adding a catalyst in an amount of 0.1-0.3% of the total reactants and an excess of ethanol solvent, and performing an addition reaction at room temperature for 48-60 hours to obtain an amide compound;

[0018] The specific process for preparing the conductive carbon material modified graphene oxide in step (5) is as follows: the product amide compound obtained in step (4) and the product octaamino POSS amine compound obtained in step (2) are added to a reaction bottle, and then deionized water is added to make the solution concentration 1-1.5%, after ultrasonic treatment for 30-45 minutes, an acid-base buffer solution is added to adjust the pH value to 4.5-5.3, and then an EDC / NHS activator is added, and stirred at room temperature for at least 24 hours to obtain a solution A for standby use;

[0019] Add the graphene oxide product obtained in step (3) into a reaction bottle, then add deionized water in an amount of 6-8 times the mass of the substance and stir evenly to obtain solution B for later use;

[0020] Then, solution A and solution B were mixed, stirred at room temperature for 24 hours, and then the reaction was stopped. Then, the solution was dialyzed with DPBS buffer and acidic deionized water for 12 hours, respectively, and the pH range of the acidic deionized water was between 4 and 5. Then, the solution was freeze-dried to obtain conductive carbon material modified graphene oxide.

[0021] Furthermore, in step (2), the epoxy group-containing compound is one of glycidyl ether, 1,4-butanediol diglycidyl ether, resorcinol diglycidyl ether, and ethylene glycol diglycidyl ether, and the organic solvent is one of ethanol, tetrahydrofuran, chloroform, toluene, and acetone.

[0022] Furthermore, in step (4), the methacrylate compound is at least one of alkyl methacrylate, 2-aminoethyl methacrylate hydrochloride, methacryloylethyl sulfobetaine, and methacryloyloxyethyl phosphorylcholine, the basic amino acid is one of histidine, arginine, and lysine, and the basic catalyst is one of triethylamine, tetraethyl lead, and phenylphosphine.

[0023] Furthermore, in step (5), the weight ratio of the amide compound: the product octaamino POSS amine compound obtained in step (2): the EDC / NHS activator is 0.6-0.7: 0.4-0.5: 0.05: 0.03, and the mass ratio of EDC and NHS in the EDC / NHS activator is 1:1;

[0024] The solvent is one of ethanol, methanol, isopropanol and N-methylpyrrolidone, and the thickener is one or more of sodium carboxymethyl cellulose, gelatin and sodium alginate.

[0025] A carbon-coated aluminum foil current collector for lithium battery and a preparation method thereof. The carbon-coated aluminum foil slurry is prepared by stirring evenly according to a proportion, and the slurry is coated on one side of the aluminum foil by a micro-concave roller. After pressurization, it is dried at a temperature of 100-180°C. Similarly, the slurry is coated on the other side of the aluminum foil and dried. The thickness of the base aluminum foil is 12-30μm, and the thickness of the single-sided coating is 1-8μm.

[0026] The present invention has the following beneficial effects due to the adoption of the above technical solution:

[0027] (1) The present invention uses a substance containing an epoxy group to modify POSS, so that reactive groups are obtained on the POSS, which can react with amide compounds and graphene oxide, thereby improving the dispersibility of graphene oxide in the slurry. Due to the cage structure, high strength and wear resistance of the POSS, the specific surface area can be increased, and the adhesion, high conductivity and solvent resistance of the coating can be improved.

[0028] (2) Using an acrylate containing at least a positive ion to react with an amino acid to obtain an amide compound, thereby creating a reaction site for further reaction and further improving the conductive properties of the carbon-coated current collector. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, preferred embodiments are given below to further describe the present invention in detail. However, it should be noted that many details listed in the specification are only for the purpose of enabling the reader to have a thorough understanding of one or more aspects of the present invention, and these aspects of the present invention can be implemented even without these specific details.

[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Unless otherwise specifically stated, the numerical value set forth in these embodiments does not limit the scope of the present invention. The technology and method known to those of ordinary skill in the relevant art may not be discussed in detail, but in appropriate cases, the technology and method should be considered as a part of the specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values.

[0032] The experimental methods in the following examples without specifying specific conditions are usually measured according to national standards; if there is no corresponding national standard, it is carried out according to the general international standards or the standard requirements proposed by relevant enterprises. Unless otherwise specified, all parts are by weight and all percentages are by weight.

[0033] A carbon-coated aluminum foil current collector for lithium battery comprises an aluminum foil substrate and a coating coated on the substrate. The coating comprises, by weight percentage, 15-25 parts of a polyurethane resin, 5-20 parts of conductive carbon material-modified graphene oxide, 0.5-2 parts of a thickener and 40-65 parts of a solvent.

[0034] Conductive carbon material modified graphene oxide is prepared by the following steps:

[0035] (1) Preparation of octaamino POSS. 30 ml of APTES and 240 ml of anhydrous methanol were added to a 500 ml three-necked flask, and stirring was started at 800 rpm. Then 41 ml of HCl was added dropwise to the solution for reaction. The reaction time was 2 days. Stirring was stopped after a white precipitate appeared, and the reaction was stopped after standing for 5-10 days. Finally, the suspension was filtered and washed with anhydrous methanol to obtain a white powder product, octaamino POSS, with a yield of about 80%, which was set aside.

[0036] (3) Preparation of graphene oxide. Add 80 ml of concentrated sulfuric acid to a three-necked flask placed in an ice-water bath, then add 3 g of natural graphite and 2 g of NaNO3 while stirring, keep the system temperature below 5 °C, then add 8 g of KMnO4 to the reaction in small amounts several times, and then continue to react at below 5 °C for 2 hours, raise the system temperature to 35-40 °C, react for 3-5 hours, add 300 ml of deionized water several times, and raise the system temperature to 90-100 °C and react for 30 minutes. After cooling to room temperature, add 10 ml of hydrogen peroxide, continue stirring for 20 minutes, and then terminate the reaction to obtain graphene oxide. Then pour all the system substances into a beaker and add 300 ml of deionized water to dilute. After multiple precipitations and centrifugation, the pH value is measured to be close to 7, dig out the solid and place it in a petri dish, place it in a vacuum oven to dry for 24 hours and set aside.

[0037] Example 1

[0038] (2) Preparation of octaamino POSS amine compound. Octaamino POSS and glycidyl ether were added into a flask at a mass ratio of 1:1.1, and then 0.5% of the total reactant base catalyst DBU and 1.3 times of the total reactant tetrahydrofuran were added. After stirring for 0.5 h, glycidyl ether was added, and the reaction was continued at room temperature for 1 h to obtain the product octaamino POSS amine compound.

[0039] (4) Preparation of amide compounds. A methacrylate compound (methacrylate alkyl ester and methacrylate-2-aminoethyl ester hydrochloride mixed in a ratio of 1:1) and a basic amino acid histidine in a mass ratio of 2:1 were added to a reaction flask, and then a catalyst triethylamine in an amount of 0.1% of the total reactants and an excess of ethanol solvent were added, and the addition reaction was carried out at room temperature for 48 hours to obtain an amide compound.

[0040] (5) Preparation of conductive carbon material modified graphene oxide. The amide compound obtained in step (4) and the octaamino POSS amine compound obtained in step (2) are added to a reaction bottle, and then deionized water is added to make the solution concentration 1-1.5%. After ultrasonic treatment for 30 minutes, an acid-base buffer solution is added to adjust the pH value to 4.5-5.3. Then, an EDC / NHS activator is added and stirred at room temperature for at least 24 hours to obtain a solution A for standby use.

[0041] The graphene oxide product obtained in step (3) is added to a reaction bottle, and then deionized water in an amount of 6-8 times the mass of the substance is added and stirred evenly to obtain a solution B for later use.

[0042] Then, solution A and solution B were mixed, and the reaction was stopped after stirring at room temperature for 24 hours. Then, the mixture was dialyzed with DPBS buffer and acidic deionized water (pH range between 4-5) for 12 hours, respectively, and then freeze-dried to obtain conductive carbon material modified graphene oxide.

[0043] Prepare a carbon-coated aluminum foil current collector for lithium battery. The coating includes, by weight percentage: 20 parts of polyurethane resin, 10 parts of conductive carbon material modified graphene oxide, 40 parts of solvent ethanol, and 0.5 parts of thickener sodium carboxymethyl cellulose. Stir to obtain a carbon-coated aluminum foil slurry; apply the slurry on one side of the aluminum foil by a micro-concave roller, pressurize, and dry at a temperature of 140°C; similarly, apply the above slurry on the other side of the aluminum foil and dry. The thickness of the base aluminum foil is 13μm; the thickness of the single-sided coating is 1μm.

[0044] Example 2

[0045] (2) Preparation of octaamino POSS amine compound. Octaamino POSS and 1,4-butanediol diglycidyl ether were added to a flask at a mass ratio of 1:1.2, and then 0.5% of the total reactant base catalyst DBU and 1.5 times of the total reactant tetrahydrofuran were added. After stirring for 0.5 h, 1,4-butanediol diglycidyl ether was added, and the reaction was continued at room temperature for 1 h to obtain the product octaamino POSS amine compound.

[0046] (4) Preparation of amide compounds. A methacrylate compound (methyl methacrylate and methacryloylethyl sulfobetaine mixed in a ratio of 1:1) and a basic amino acid histidine were added to a reaction flask in a mass ratio of 2.2:1, and then a catalyst triethylamine in an amount of 0.2% of the total reactants and an excess of ethanol solvent were added, and the addition reaction was carried out at room temperature for 48 hours to obtain an amide compound.

[0047] (5) Preparation of conductive carbon material modified graphene oxide. The amide compound obtained in step (4) and the octaamino POSS amine compound obtained in step (2) are added to a reaction bottle, and then deionized water is added to make the solution concentration 1-1.5%. After ultrasonic treatment for 30 minutes, an acid-base buffer solution is added to adjust the pH value to 4.5-5.3. Then, an EDC / NHS activator is added and stirred at room temperature for at least 24 hours to obtain a solution A for standby use.

[0048] The graphene oxide product obtained in step (3) is added to a reaction bottle, and then deionized water in an amount of 6-8 times the mass of the substance is added and stirred evenly to obtain a solution B for later use.

[0049] Then, solution A and solution B were mixed, and the reaction was stopped after stirring at room temperature for 24 hours. Then, the mixture was dialyzed with DPBS buffer and acidic deionized water (pH range between 4-5) for 12 hours, respectively, and then freeze-dried to obtain conductive carbon material modified graphene oxide.

[0050] Prepare a carbon-coated aluminum foil current collector for lithium battery. The coating includes, by weight percentage: 25 parts of polyurethane resin, 12 parts of conductive carbon material modified graphene oxide, 55 parts of solvent ethanol, and 1.5 parts of thickener sodium alginate. Stir to obtain a carbon-coated aluminum foil slurry; apply the slurry on one side of the aluminum foil by a micro-concave roller, pressurize, and dry at a temperature of 140°C; similarly, apply the above slurry on the other side of the aluminum foil and dry. The thickness of the base aluminum foil is 13μm; the thickness of the single-sided coating is 1μm.

[0051] Example 3

[0052] (2) Preparation of octaamino POSS amine compound. Octaamino POSS and glycidyl ether were added to a flask at a mass ratio of 1:1.2, and then 0.5% of the total reactant was added as a base catalyst DBU and 1.4 times of the total reactant was added as tetrahydrofuran. After stirring for 1 hour, glycidyl ether was added, and the reaction was continued at room temperature with stirring for 1 hour to obtain the product octaamino POSS amine compound.

[0053] (4) Preparation of amide compounds. A methacrylate compound (methacryloylethyl sulfobetaine and methacryloyloxyethyl phosphorylcholine mixed in a ratio of 1:1) and a basic amino acid arginine were added to a reaction flask in a mass ratio of 2.4:1, and then a catalyst phenylphosphine in an amount of 0.3% of the total reactants and an excess of ethanol solvent were added, and the addition reaction was carried out at room temperature for 60 hours to obtain an amide compound.

[0054] (5) Preparation of conductive carbon material modified graphene oxide. The amide compound obtained in step (4) and the octaamino POSS amine compound obtained in step (2) are added to a reaction bottle, and then deionized water is added to make the solution concentration 1-1.5%. After ultrasonic treatment for 30 minutes, an acid-base buffer solution is added to adjust the pH value to 4.5-5.3. Then, an EDC / NHS activator is added and stirred at room temperature for at least 24 hours to obtain a solution A for standby use.

[0055] The graphene oxide product obtained in step (3) is added to a reaction bottle, and then deionized water in an amount of 6-8 times the mass of the substance is added and stirred evenly to obtain a solution B for later use.

[0056] Then, solution A and solution B were mixed, and the reaction was stopped after stirring at room temperature for 24 hours. Then, the mixture was dialyzed with DPBS buffer and acidic deionized water (pH range between 4-5) for 12 hours, respectively, and then freeze-dried to obtain conductive carbon material modified graphene oxide.

[0057] Prepare a carbon-coated aluminum foil current collector for lithium battery. The coating includes, by weight percentage: 18 parts of polyurethane resin, 8 parts of conductive carbon material modified graphene oxide, 60 parts of solvent ethanol, and 2 parts of thickener sodium alginate. Stir to obtain a carbon-coated aluminum foil slurry; apply the slurry on one side of the aluminum foil by a micro-concave roller, pressurize, and dry at a temperature of 140°C; similarly, apply the above slurry on the other side of the aluminum foil and dry. The thickness of the base aluminum foil is 13μm; the thickness of the single-sided coating is 1μm.

[0058] Example 4

[0059] (2) Preparation of octaamino POSS amine compound. Octaamino POSS 1,4-butanediol diglycidyl ether was added to octaamino POSS in a mass ratio of 1:1.2 into a flask, and then 0.5% of the total reactant amount of base catalyst DBU and 1.5 times of the total reactant amount of chloroform were added. After stirring for 1 hour, glycidyl ether was added, and the reaction was continued at room temperature for 2 hours to obtain the product octaamino POSS amine compound.

[0060] (4) Preparation of amide compounds. A methacrylate compound (methyl methacrylate: methacrylate-2-aminoethyl ester hydrochloride 1:1.2) and a basic amino acid histidine were added to a reaction flask at a mass ratio of 2.4:1, and then a catalyst triethylamine in an amount of 0.3% of the total reactants and an excess of ethanol solvent were added, and the addition reaction was carried out at room temperature for 48 hours to obtain an amide compound.

[0061] (5) Preparation of conductive carbon material modified graphene oxide. The amide compound obtained in step (4) and the octaamino POSS amine compound obtained in step (2) are added to a reaction bottle, and then deionized water is added to make the solution concentration 1-1.5%. After ultrasonic treatment for 30 minutes, an acid-base buffer solution is added to adjust the pH value to 4.5-5.3. Then, an EDC / NHS activator is added and stirred at room temperature for at least 24 hours to obtain a solution A for standby use.

[0062] The graphene oxide product obtained in step (3) is added to a reaction bottle, and then deionized water in an amount of 6-8 times the mass of the substance is added and stirred evenly to obtain a solution B for later use.

[0063] Then, solution A and solution B were mixed, and the reaction was stopped after stirring at room temperature for 24 hours. Then, the mixture was dialyzed with DPBS buffer and acidic deionized water (pH range between 4-5) for 12 hours, respectively, and then freeze-dried to obtain conductive carbon material modified graphene oxide.

[0064] Prepare a carbon-coated aluminum foil current collector for lithium battery. The coating includes, by weight percentage: 15 parts of polyurethane resin, 7 parts of conductive carbon material modified graphene oxide, 40 parts of solvent isopropyl alcohol, and 1.5 parts of thickener sodium carboxymethyl cellulose. Stir to obtain a carbon-coated aluminum foil slurry; apply the slurry on one side of the aluminum foil by a micro-concave roller, pressurize, and dry at a temperature of 140°C; similarly, apply the above slurry on the other side of the aluminum foil and dry. The thickness of the base aluminum foil is 13μm; the thickness of the single-sided coating is 1μm.

[0065] Comparative Example 1

[0066] The plain aluminum foil current collector produced by our company was used for relevant performance tests.

[0067] Comparative Example 2

[0068] The carbon-coated aluminum foil current collector for lithium battery is prepared. The coating includes, by weight percentage: 20 parts of polyurethane resin, 10 parts of unmodified graphene oxide, 40 parts of solvent ethanol, and 0.5 parts of thickener sodium carboxymethyl cellulose. Stirring to obtain carbon-coated aluminum foil slurry; applying the slurry on one side of the aluminum foil by a micro-concave roller, applying pressure, and drying at a temperature of 140°C; similarly, applying the above slurry on the other side of the aluminum foil and drying. The thickness of the base aluminum foil is 13μm; the thickness of the single-sided coating is 1μm.

[0069] The graphene oxide is prepared according to step (3).

[0070] Comparative Example 3

[0071] Prepare a carbon-coated aluminum foil current collector for lithium battery. The coating includes, by weight percentage: 20 parts of polyurethane resin, 10 parts of conductive carbon material modified graphene oxide, 40 parts of solvent ethanol, and 0.5 parts of thickener sodium carboxymethyl cellulose. Stir to obtain a carbon-coated aluminum foil slurry; apply the slurry on one side of the aluminum foil by a micro-concave roller, pressurize, and dry at a temperature of 140°C; similarly, apply the above slurry on the other side of the aluminum foil and dry. The thickness of the base aluminum foil is 13μm; the thickness of the single-sided coating is 1μm.

[0072] The preparation of the conductive carbon material modified graphene oxide is different from that in Example 1 in that no amide compound is added for the reaction.

[0073] The surface resistance, peel strength, solvent resistance and wetting tension performance of the coatings prepared on the aluminum foil current collector of the above embodiments and comparative examples were tested, and the test results are shown in Table 1. The surface resistance was tested using a two-probe resistance tester; the peel strength test was measured according to GB / T 2792-2014; the solvent resistance test was performed by wiping the surfaces of the coatings of the above embodiments and comparative examples with cotton swabs soaked in water and DMC respectively until the number of times the aluminum foil substrate was exposed; the wetting tension was tested using a dyne pen.

[0074] Table 1 Examples and Comparative Examples Data

[0075]

[0076] It can be seen from the performance test data of the embodiment that the POSS is modified by using a substance containing an epoxy group, and reacts with an amide compound and graphene oxide to improve the dispersibility of graphene oxide in the slurry. Due to the cage structure, high strength and wear resistance of the POSS, the specific surface area of ​​the conductive carbon material graphene oxide is increased, the adhesion between the coating and the aluminum foil is improved, and the conductivity is high and solvent-resistant. At the same time, by comparing Examples 1-4 and Comparative Example 3, the amide compound containing positive ions can further improve the conductivity of the carbon-coated current collector, reduce the internal resistance of the battery, and then improve the battery cycle life.

[0077] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A carbon-coated aluminum foil current collector for lithium battery, characterized in that: The invention comprises a base aluminum foil and a coating coated on the base. The coating comprises, by weight percentage, 15-25 parts of a polyurethane resin, 5-20 parts of conductive carbon material-modified graphene oxide, 0.5-2 parts of a thickener and 40-65 parts of a solvent.

2. The carbon-coated aluminum foil current collector for lithium battery according to claim 1, characterized in that: Conductive carbon material modified graphene oxide is prepared by the following steps: (1) Preparation of octaamine-based POSS; (2) Preparation of octaamine POSS aminated compounds; (3) Preparation of graphene oxide; (4) Preparation of amide compounds; (5) Conductive carbon material modified graphene oxide is prepared by using octaamine-based POSS amine compound, graphene oxide and amide compound in the presence of a catalyst.

3. The carbon-coated aluminum foil current collector for lithium battery according to claim 2, characterized in that: The specific process of preparing the octaamino POSS in step (1) is as follows: 30 ml of APTES and 240 ml of anhydrous methanol are added to a 500 ml three-necked flask, stirring is started at a speed of 800 rpm, and then 41 ml of HCl is added dropwise to the solution to react for 2 days until a white precipitate appears, stirring is stopped, and the reaction is stopped after standing for 5-10 days. Finally, the suspension is filtered and washed with anhydrous methanol to obtain a white powder product, the octaamino POSS, with a yield of 75-85%.

4. The carbon-coated aluminum foil current collector for lithium battery according to claim 2, characterized in that: The specific process for preparing the octaamino POSS amine compound in step (2) is as follows: octaamino POSS and an epoxy group-containing compound are added to a flask at a mass ratio of 1:1.1-1.2, and then an alkali catalyst DBU is added in an amount of 0.5% of the total reactants and an organic solvent is added in an amount of 1.3-1.5 times of the total reactants. After stirring for 0.5-1h, the epoxy group-containing compound is added, and the stirring reaction is continued at room temperature for 1-2h to obtain the product octaamino POSS amine compound.

5. The carbon-coated aluminum foil current collector for lithium battery according to claim 2, characterized in that: The specific process for preparing graphene oxide in step (3) is as follows: 80 ml of concentrated sulfuric acid is added to a three-necked flask placed in an ice water bath, and then 3 g of natural graphite and 2 g of NaNO3 are added while stirring, the system temperature is kept below 5 ° C, and then 8 g of KMnO4 is added to the reaction in small amounts several times, and then the reaction is continued at below 5 ° C for 2 h, the system is heated to 35-40 ° C, and after reacting for 3-5 h, 300 ml of deionized water is added several times, and the system is heated to 90-100 ° C, reacted for 30 min, cooled to room temperature, 10 ml of hydrogen peroxide is added, and the reaction is terminated after continuous stirring for 20 min to obtain graphene oxide, and then all the system substances are poured into a beaker, 300 ml of deionized water is added for dilution, and after multiple precipitations and centrifugation, the pH value is measured to be close to 7, the solid is dug out and placed in a culture dish, and placed in a vacuum oven for drying for 24 h for use.

6. The carbon-coated aluminum foil current collector for lithium battery according to claim 2, characterized in that: The specific process of preparing the amide compound in step (4) is as follows: adding a methacrylate compound and a basic amino acid in a mass ratio of 2-2.4:1 to a reaction bottle, and then adding a catalyst in an amount of 0.1-0.3% of the total reactants and an excess of ethanol solvent, and performing an addition reaction at room temperature for 48-60 hours to obtain an amide compound; The specific process for preparing the conductive carbon material modified graphene oxide in step (5) is as follows: the product amide compound obtained in step (4) and the product octaamino POSS amine compound obtained in step (2) are added to a reaction bottle, and then deionized water is added to make the solution concentration 1-1.5%, after ultrasonic treatment for 30-45 minutes, an acid-base buffer solution is added to adjust the pH value to 4.5-5.3, and then an EDC / NHS activator is added, and stirred at room temperature for at least 24 hours to obtain a solution A for standby use; Add the graphene oxide product obtained in step (3) into a reaction bottle, then add deionized water in an amount of 6-8 times the mass of the substance and stir evenly to obtain solution B for later use; Then, solution A and solution B were mixed, stirred at room temperature for 24 hours, and then the reaction was stopped. Then, the solution was dialyzed with DPBS buffer and acidic deionized water for 12 hours, respectively, and the pH range of the acidic deionized water was between 4 and 5. Then, the solution was freeze-dried to obtain conductive carbon material modified graphene oxide.

7. The carbon-coated aluminum foil current collector for lithium battery according to claim 4, characterized in that: In step (2), the epoxy group-containing compound is one of glycidyl ether, 1,4-butanediol diglycidyl ether, resorcinol diglycidyl ether, and ethylene glycol diglycidyl ether, and the organic solvent is one of ethanol, tetrahydrofuran, chloroform, toluene, and acetone.

8. A carbon-coated aluminum foil current collector for lithium battery according to claim 5, characterized in that: In step (4), the methacrylate compound is at least one of alkyl methacrylate, 2-aminoethyl methacrylate hydrochloride, methacryloylethyl sulfobetaine, and methacryloyloxyethyl phosphorylcholine, the basic amino acid is one of histidine, arginine, and lysine, and the basic catalyst is one of triethylamine, tetraethyl lead, and phenylphosphine.

9. The carbon-coated aluminum foil current collector for lithium battery according to claim 6, characterized in that: In step (5), the weight ratio of the amide compound: the product octaamino POSS amine compound obtained in step (2): EDC / NHS activator is 0.6-0.7:0.4-0.5:0.05:0.03, and the mass ratio of EDC and NHS in the EDC / NHS activator is 1:1; The solvent is one of ethanol, methanol, isopropanol and N-methylpyrrolidone, and the thickener is one or more of sodium carboxymethyl cellulose, gelatin and sodium alginate.

10. A carbon-coated aluminum foil current collector for lithium battery and a preparation method thereof according to any one of claims 1 to 9, characterized in that: The mixture is stirred evenly according to the proportion to obtain a carbon-coated aluminum foil slurry, which is then coated on one side of the aluminum foil by a micro-concave roller. After pressurization, it is dried at a temperature of 100-180°C. Similarly, the slurry is coated on the other side of the aluminum foil and dried. The thickness of the base aluminum foil is 12-30μm, and the thickness of the single-sided coating is 1-8μm.