Perovskite thin film annealing process and equipment

By using annealing equipment that uses a laser to form a temperature gradient on the perovskite film, the problem of small grain size in the existing technology is solved, and the crystallinity and photoelectric conversion efficiency of the perovskite film are improved.

CN118765149APending Publication Date: 2024-10-11陕西众森电能科技有限公司

Patent Information

Application Number
CN202410848567.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The existing perovskite film annealing process is difficult to accurately control the crystallinity and charge carrier mobility, resulting in smaller grain size and affecting the performance of photovoltaic devices.

Method used

An annealing equipment including a preheating platform and a laser light source is used to form a one-dimensional temperature gradient in the length direction on the perovskite film through a strip laser to achieve the growth of the grains along the length direction. The scanning mechanism and laser controller are combined to Ensures even heating and annealing.

Benefits of technology

The growth of larger grain sizes is achieved, the crystallization uniformity and conversion efficiency of the perovskite film are improved, and the trap state density and charge recombination are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118765149A_ABST
    Figure CN118765149A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of perovskite thin films, and mainly relates to a perovskite thin film annealing process and equipment, the annealing equipment comprises a preheating platform and a laser light source which can move relatively, the preheating platform is used for bearing a perovskite thin film and a substrate thereof, the preheating platform is used for heating the perovskite thin film and the substrate thereof, and the laser light source is used for heating the perovskite thin film and the substrate thereof. The laser light source is used for generating strip-shaped laser, and the strip-shaped laser irradiates the perovskite thin film, so that a one-dimensional temperature gradient in the length direction is formed on the perovskite thin film. And finishing the annealing process by using annealing equipment. Strip-shaped laser is used for heating and scanning, and a one-dimensional temperature gradient in the length direction is formed in a crystallization transition area, so that crystal grains can grow in the length direction without size limitation in the length direction, the crystallization uniformity, the crystal grain size and the crystallinity of the perovskite film layer are improved, the trap state density of the perovskite film layer is reduced, charge recombination is further reduced, and the performance of the perovskite film layer is improved. And the photoelectric conversion efficiency of the perovskite thin film is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of perovskite thin films, and mainly relates to a perovskite thin film annealing process and equipment. Background Art

[0002] In recent years, new photovoltaic materials represented by organic-inorganic halide perovskites have developed rapidly. In the past decade, their photoelectric conversion efficiency in the field of photovoltaic devices has increased from 3.8% to more than 26.1%, making them one of the most promising new generation of high-efficiency solar cell materials. According to theoretical calculations, the ultimate photoelectric conversion efficiency of perovskite solar cells is 45%. So far, the photoelectric conversion efficiency of all perovskite solar cells is far lower than this. Therefore, the development of ultra-high conversion efficiency perovskite solar cells has become a new research hotspot. The main reasons for the low photoelectric conversion efficiency are optical loss, body defect-assisted non-radiative recombination loss and ohmic loss. Among them, the main factor affecting the quality of perovskite films is body defect-assisted non-radiative (SRH) recombination loss.

[0003] Studies have shown that the crystallinity of perovskite films is a key factor affecting the performance of photovoltaic devices. Perovskite films with larger grains usually have lower trap state density and higher carrier mobility, which also reduces the carrier recombination of perovskite films. Therefore, the preparation of perovskite films with large grains has become an important means to improve the performance of photovoltaics and LEDs. The generation of grains mainly includes two processes: nucleation and growth. The growth process determines the size of the grains, and the annealing process plays a decisive role in the growth of the grains. However, the commonly used perovskite film annealing process (thermal annealing) today is difficult to accurately control the crystallinity and charge carrier mobility of perovskite films.

[0004] The Chinese patent document with the authorization announcement number CN219660314U discloses a perovskite film annealing device. The return device includes a box; an infrared heating module that can emit infrared spectrum after power is turned on is installed on the inner top surface of the box; an annealing platform for placing the perovskite film is installed below the infrared heating module, and the perovskite film placed on the annealing platform is heated by the infrared heating module; the infrared heating module is a composite layer structure, which includes a substrate, an electro-emissive infrared coating and an infrared transmission layer from bottom to top.

[0005] The above-mentioned ordinary thermal annealing is achieved by heating, melting, cooling and crystallization. The crystallization process is similar to ice forming on the water surface. The crystals grow only in the longitudinal direction, resulting in the grain size of the perovskite film being only 400-800 nanometers. In other words, the scale of the grain growth direction is only on the order of hundreds of nanometers, so it is impossible to grow larger grains. Summary of the invention

[0006] The present invention provides a perovskite film annealing device to solve the problem of small grain size in the perovskite film in the prior art.

[0007] The present invention also provides a perovskite film annealing process to solve the problem of small grain size in the perovskite film in the prior art.

[0008] To solve the above problems, the present invention adopts the following technical solutions:

[0009] A perovskite film annealing device comprises a preheating platform and a laser light source capable of relative movement, wherein the preheating platform is used to carry the perovskite film and its substrate, and the preheating platform heats the perovskite film and its substrate; the laser light source is used to generate strip laser, and the strip laser is irradiated on the perovskite film to form a one-dimensional temperature gradient in the length direction of the perovskite film.

[0010] The method has the following beneficial effects: the annealing process is completed by using strip laser heating scanning, and a one-dimensional temperature gradient in the length direction is formed in the crystallization transition region, so that the grains can grow along the length direction of the perovskite film without size restrictions in the length direction, thereby obtaining a larger perovskite film grain size.

[0011] Furthermore, the length of the strip laser is not less than the width of the perovskite film.

[0012] The invention has the following beneficial effects: the strip laser can completely cover the perovskite film and avoid leaving dead corners.

[0013] Furthermore, the laser intensity at each location of the strip laser is the same.

[0014] The method has the following beneficial effects: the same laser intensity can achieve uniform heating of the perovskite film, ensuring the crystallization uniformity, grain size and crystallinity of the perovskite film layer.

[0015] Furthermore, the annealing equipment also includes a scanning mechanism, which includes a linear drive component, and a moving end of the linear drive component is connected to the laser light source to achieve relative movement between the laser light source and the perovskite film.

[0016] The invention has the following beneficial effects: the scanning mechanism causes relative movement between the laser light source and the perovskite film, so that the strip laser can move on the perovskite film, thereby realizing annealing of the entire perovskite film.

[0017] Furthermore, the annealing equipment also includes a laser controller, which is used to control laser parameters of the laser light source emitting strip lasers and to control the moving speed of the laser light source.

[0018] The invention has the following beneficial effects: the intensity of the laser is controlled by the laser controller, so that the device can adapt to different process requirements.

[0019] Furthermore, the laser parameters include laser wavelength, laser power density and laser width.

[0020] Furthermore, the laser wavelength is 248-1070nm, the laser width is 0.1-1mm, and the laser power density is 0.2-20W / mm 2 .

[0021] A perovskite film annealing process using the annealing device irradiates a preheated perovskite film with a strip laser having a length not less than the width of the perovskite film, and scans the perovskite film in the length direction of the perovskite film to achieve the growth of the perovskite film grains, thereby obtaining a perovskite film containing perovskite grains with large particle sizes.

[0022] The method has the following beneficial effects: the annealing process is completed by using strip laser heating scanning, and a one-dimensional temperature gradient in the length direction is formed in the crystallization transition region, so that the grains can grow along the length direction without size restrictions in the length direction, thereby improving the crystallization uniformity, grain size and crystallinity of the perovskite film layer, reducing the trap state density of the perovskite film layer, and thereby reducing charge recombination, and greatly improving the conversion efficiency of the perovskite film.

[0023] Further, before preheating the perovskite film, the perovskite film is wetted with a perovskite precursor solution.

[0024] Furthermore, the laser wavelength of the strip laser is 248-1070nm, the laser width is 0.1-1mm, and the laser power density is 0.2-20W / mm 2 , scanning speed is 2-200mm / min, and preheating temperature is 25-200℃. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] By reading the following detailed description with reference to the accompanying drawings, the above and other objects, features and advantages of the exemplary embodiments of the present invention will become readily understood. In the accompanying drawings, several embodiments of the present invention are shown in an exemplary and non-limiting manner, and the same or corresponding reference numerals represent the same or corresponding parts, wherein:

[0026] Figure 1 It is a schematic diagram of the structure of the perovskite film annealing equipment;

[0027] Figure 2 Schematic diagram of the structure when a strip laser irradiates the perovskite film.

[0028] Description of reference numerals:

[0029] 1. Laser light source; 2. Strip laser; 3. Perovskite film; 4. Substrate; 5. Preheating platform; 6. Scanning mechanism; 7. Perovskite area to be crystallized; 8. Perovskite area that has been crystallized; 9. Crystallization transition area; 10. Laser heating melting area; 11. Isotherm. DETAILED DESCRIPTION

[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Those skilled in the art should know that the embodiments described below are part of the embodiments of the present disclosure, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.

[0031] Various non-limiting embodiments of the present invention are described in detail below. Any number of elements in the accompanying drawings is for illustration and not for limitation, and any naming is only for distinction and does not have any limiting meaning. It should be noted that, in the absence of conflict, the embodiments in this application and the features in the embodiments can be combined with each other.

[0032] Perovskite film annealing equipment embodiment 1

[0033] like Figure 1 As shown, a perovskite film annealing device includes a laser light source 1, a preheating platform 5 and a scanning mechanism 6, wherein the laser light source 1 is used to generate a strip laser 2, and the strip laser 2 is used to irradiate the perovskite film 3, so that a one-dimensional temperature gradient in the length direction is formed on the perovskite film 3. The laser light source 1 in this embodiment can be the laser line irradiation described in the authorization announcement number CN109477970B, thereby generating the strip laser 2; wherein the one-dimensional temperature gradient refers to a temperature gradient in the length direction of the perovskite film 3, and the length direction refers to the movement direction of the laser light source 1 relative to the generated perovskite film 3. The preheating platform 5 is used to carry the perovskite film 3 and its substrate 4, and the perovskite film 3 and its substrate 4 can also be heated by the preheating platform 5. The scanning mechanism 6 is used to drive the laser light source 1 to move linearly to achieve relative movement between the laser light source 1 and the perovskite film 3. The position of the laser light source 1 is relatively easier to move, more energy-saving, and faster.

[0034] like Figure 1-Figure 2 As shown, when the strip laser 2 is irradiated onto the perovskite film 3, four regions are formed on the perovskite film 3: a perovskite region 7 to be crystallized, a perovskite region 8 that has been crystallized, a crystallization transition region 9, and a laser-heated melting region 10, and the boundary between adjacent regions is an isotherm 11.

[0035] There are many descriptions in the prior art about how the scanning mechanism 6 drives the laser light source 1 or the preheating platform 5 to move. For example, the scanning mechanism 6 may include a linear drive member, which may be a lead screw nut mechanism, and the laser light source 1 or the preheating platform 5 is mounted on the lead screw nut mechanism, thereby driving the laser light source 1 to move; or the linear drive member may be a cylinder, a hydraulic cylinder or an electric push rod, which directly drives the laser light source 1 to move. The scanning mechanism 6 causes relative movement between the laser light source 1 and the perovskite film 3, so that the strip laser 2 can move on the perovskite film 3, thereby realizing annealing of the entire perovskite film 3.

[0036] The length of the strip laser 2 generated by the laser light source 1 is not less than the width of the perovskite film 3 , so that the strip laser 2 can completely cover the perovskite film 3 and avoid leaving unannealed dead corners on the perovskite film 3 .

[0037] In order to achieve uniform heating of the perovskite film 3 and ensure the crystallization uniformity, grain size and crystallinity of the perovskite film layer, the laser intensity of the strip laser 2 needs to be the same at all locations.

[0038] Specifically, the annealing equipment also includes a laser controller, which is used to control the laser parameters of the laser light source 1 emitting the strip laser 2 and to control the moving speed of the laser light source 1, wherein the laser parameters include laser wavelength, laser power density and laser width, the laser wavelength is 248-1070nm, the laser width is 0.1-1mm, and the laser power density is 0.2-20W / mm 2 The intensity of the laser is controlled by a laser controller, so that the device can adapt to different process requirements.

[0039] The annealing process is completed by heating and scanning with a strip laser 2, and a one-dimensional temperature gradient is formed in the length direction in the crystallization transition region 9, so that the grains can grow along the length direction without size restrictions in the length direction, thereby improving the crystallization uniformity, grain size and crystallinity of the perovskite film layer, reducing the trap state density of the perovskite film layer, and further reducing charge recombination, so that the photoelectric conversion efficiency of the perovskite film 3 is greatly improved.

[0040] Perovskite film annealing equipment embodiment 2

[0041] The difference between this embodiment and embodiment 1 is that the scanning mechanism 6 in this embodiment drives the preheating platform 5 to move linearly, that is, the moving end of the linear driving member is connected to the preheating platform 5 to achieve relative movement between the laser light source 1 and the perovskite film 3.

[0042] Perovskite film annealing equipment embodiment 3

[0043] The difference between this embodiment and embodiment 1 is that the scanning mechanism 6 in this embodiment can simultaneously drive the laser light source 1 and the preheating platform 5 to move linearly, and the scanning mechanism 6 has two linear driving components, a moving end of one linear driving component is connected to the laser light source 1, and a moving end of the other linear driving component is connected to the preheating platform 5, so as to realize the relative movement between the laser light source 1 and the perovskite film 3.

[0044] Perovskite film annealing equipment embodiment 4

[0045] The difference between this embodiment and embodiment 1 is that the length of the strip laser 2 generated by the laser light source 1 in this embodiment is smaller than the width of the perovskite film 3, that is, in order to achieve annealing of the perovskite film 3 and promote the growth of grains in the perovskite film 3, the laser light source 1 needs to scan the perovskite film 3 multiple times.

[0046] Perovskite film annealing process example 1

[0047] A perovskite film annealing process using the annealing device in the above embodiment specifically comprises the following steps:

[0048] Step 1: First, place the substrate 4 on the preheating platform 5, then spray the perovskite precursor solution onto the substrate 4, then place the perovskite film 3 onto the substrate 4 containing the perovskite precursor solution, and finally use the preheating platform 5 to heat the substrate 4 and the perovskite film 3, wherein the heating temperature is 25° C. The perovskite precursor solution in this embodiment can be the perovskite precursor solution disclosed in the patent application document with publication number CN114122267A.

[0049] Step 2: Start the laser light source 1 to generate the strip laser 2, and irradiate the strip laser 2 onto the perovskite film 3, wherein the laser wavelength of the strip laser 2 generated by the laser controller is 350nm, the laser width is 0.5mm, and the laser power density is 11W / mm 2 .

[0050] Step 3: The scanning mechanism 6 drives one of the laser light source 1 or the preheating platform 5 to move. The relative movement speed of the laser light source 1 and / or the preheating platform 5 is 185 mm / min. The movement direction of the laser light source 1 and / or the preheating platform 5 is perpendicular to the extension direction of the strip laser 2, thereby completing the annealing of the perovskite film 3 and obtaining a perovskite film 3 containing large-size perovskite grains.

[0051] The sprayed perovskite precursor solution can be used for the growth of perovskite film 3 grains during the annealing process; at the same time, the strip laser 2 is used for heating scanning to complete the annealing process, forming a one-dimensional temperature gradient in the length direction in the crystallization transition region 9, so that the grains can grow along the length direction without size restrictions in the length direction, thereby improving the crystallization uniformity, grain size and crystallinity of the perovskite film layer, reducing the trap state density of the perovskite film layer, and then reducing charge recombination, so that the photoelectric conversion efficiency of the perovskite film 3 is greatly improved.

[0052] Perovskite film annealing process example 2

[0053] A perovskite film annealing process specifically comprises the following steps:

[0054] Step 1: First, place the substrate 4 on the preheating platform 5, then spray the perovskite precursor solution onto the substrate 4, then place the perovskite film 3 on the substrate 4 containing the perovskite precursor solution, and finally use the preheating platform 5 to heat the substrate 4 and the perovskite film 3, wherein the heating temperature is 56°C.

[0055] Step 2: Start the laser light source 1 to generate the strip laser 2, and irradiate the strip laser 2 onto the perovskite film 3, wherein the laser wavelength of the strip laser 2 generated by the laser controller is 550nm, the laser width is 0.7mm, and the laser power density is 17W / mm 2 .

[0056] Step 3: The scanning mechanism 6 drives one of the laser light source 1 or the preheating platform 5 to move. The relative movement speed of the laser light source 1 and / or the preheating platform 5 is 200 mm / min. The movement direction of the laser light source 1 and / or the preheating platform 5 is perpendicular to the extension direction of the strip laser 2, thereby completing the annealing of the perovskite film 3.

[0057] The sprayed perovskite precursor solution can be used for the growth of perovskite film 3 grains during the annealing process; at the same time, the strip laser 2 is used for heating scanning to complete the annealing process, forming a one-dimensional temperature gradient in the length direction in the crystallization transition region 9, so that the grains can grow along the length direction without size restrictions in the length direction, thereby improving the crystallization uniformity, grain size and crystallinity of the perovskite film layer, reducing the trap state density of the perovskite film layer, and then reducing charge recombination, and the conversion efficiency of the perovskite film 3 is greatly improved.

[0058] Perovskite film annealing process example 3

[0059] A perovskite film annealing process specifically comprises the following steps:

[0060] Step 1: First, place the substrate 4 on the preheating platform 5, then spray the perovskite precursor solution onto the substrate 4, then place the perovskite film 3 on the substrate 4 containing the perovskite precursor solution, and finally use the preheating platform 5 to heat the substrate 4 and the perovskite film 3, wherein the heating temperature is 90°C.

[0061] Step 2: Start the laser light source 1 to generate the strip laser 2, and make the strip laser 2 irradiate the perovskite film 3, wherein the laser wavelength of the strip laser 2 generated by the laser controller is 650nm, the laser width is 0.9mm, and the laser power density is 20W / mm 2 .

[0062] Step 3: The scanning mechanism 6 drives one of the laser light source 1 or the preheating platform 5 to move. The relative movement speed of the laser light source 1 and / or the preheating platform 5 is 2 mm / min. The movement direction of the laser light source 1 and / or the preheating platform 5 is perpendicular to the extension direction of the strip laser 2, thereby completing the annealing of the perovskite film 3.

[0063] The sprayed perovskite precursor solution can be used for the growth of perovskite film 3 grains during the annealing process; at the same time, the strip laser 2 is used for heating scanning to complete the annealing process, forming a one-dimensional temperature gradient in the length direction in the crystallization transition region 9, so that the grains can grow along the length direction without size restrictions in the length direction, thereby improving the crystallization uniformity, grain size and crystallinity of the perovskite film layer, reducing the trap state density of the perovskite film layer, and then reducing charge recombination, and the conversion efficiency of the perovskite film 3 is greatly improved.

[0064] Perovskite film annealing process example 4

[0065] A perovskite film annealing process specifically comprises the following steps:

[0066] Step 1: First, place the substrate 4 on the preheating platform 5, then spray the perovskite precursor solution onto the substrate 4, then place the perovskite film 3 on the substrate 4 containing the perovskite precursor solution, and finally use the preheating platform 5 to heat the substrate 4 and the perovskite film 3, wherein the heating temperature is 130°C.

[0067] Step 2: Start the laser light source 1 to generate the strip laser 2, and irradiate the strip laser 2 onto the perovskite film 3, wherein the laser wavelength of the strip laser 2 generated by the laser controller is 850nm, the laser width is 1mm, and the laser power density is 0.2W / mm 2 .

[0068] Step 3: The scanning mechanism 6 drives one of the laser light source 1 or the preheating platform 5 to move. The relative movement speed of the laser light source 1 and / or the preheating platform 5 is 20 mm / min. The movement direction of the laser light source 1 and / or the preheating platform 5 is perpendicular to the extension direction of the strip laser 2, thereby completing the annealing of the perovskite film 3.

[0069] The sprayed perovskite precursor solution can be used for the growth of perovskite film 3 grains during the annealing process; at the same time, the strip laser 2 is used for heating scanning to complete the annealing process, forming a one-dimensional temperature gradient in the length direction in the crystallization transition region 9, so that the grains can grow along the length direction without size restrictions in the length direction, thereby improving the crystallization uniformity, grain size and crystallinity of the perovskite film layer, reducing the trap state density of the perovskite film layer, and then reducing charge recombination, and the conversion efficiency of the perovskite film 3 is greatly improved.

[0070] Perovskite film annealing process example 5

[0071] A perovskite film annealing process specifically comprises the following steps:

[0072] Step 1: First, place the substrate 4 on the preheating platform 5, then spray the perovskite precursor solution onto the substrate 4, and then place the perovskite film 3 on the substrate 4 containing the perovskite precursor solution, and finally use the preheating platform 5 to heat the substrate 4 and the perovskite film 3, wherein the heating temperature is 175°C.

[0073] Step 2: Start the laser light source 1 to generate the strip laser 2, and make the strip laser 2 irradiate the perovskite film 3, wherein the laser wavelength of the strip laser 2 generated by the laser controller is 1070nm, the laser width is 0.1mm, and the laser power density is 2W / mm 2 .

[0074] Step 3: The scanning mechanism 6 drives one of the laser light source 1 or the preheating platform 5 to move. The relative movement speed of the laser light source 1 and / or the preheating platform 5 is 70 mm / min. The movement direction of the laser light source 1 and / or the preheating platform 5 is perpendicular to the extension direction of the strip laser 2, thereby completing the annealing of the perovskite film 3.

[0075] The sprayed perovskite precursor solution can be used for the growth of perovskite film 3 grains during the annealing process; at the same time, the strip laser 2 is used for heating scanning to complete the annealing process, forming a one-dimensional temperature gradient in the length direction in the crystallization transition region 9, so that the grains can grow along the length direction without size restrictions in the length direction, thereby improving the crystallization uniformity, grain size and crystallinity of the perovskite film layer, reducing the trap state density of the perovskite film layer, and then reducing charge recombination, and the conversion efficiency of the perovskite film 3 is greatly improved.

[0076] Perovskite film annealing process example 6

[0077] A perovskite film annealing process specifically comprises the following steps:

[0078] Step 1: First, place the substrate 4 on the preheating platform 5, then spray the perovskite precursor solution onto the substrate 4, then place the perovskite film 3 on the substrate 4 containing the perovskite precursor solution, and finally use the preheating platform 5 to heat the substrate 4 and the perovskite film 3, wherein the heating temperature is 200°C.

[0079] Step 2: Start the laser light source 1 to generate the strip laser 2, and make the strip laser 2 irradiate the perovskite film 3, wherein the laser wavelength of the strip laser 2 generated by the laser controller is 248nm, the laser width is 0.2mm, and the laser power density is 6W / mm 2 .

[0080] Step 3: The scanning mechanism 6 drives one of the laser light source 1 or the preheating platform 5 to move. The relative movement speed of the laser light source 1 and / or the preheating platform 5 is 120 mm / min. The movement direction of the laser light source 1 and / or the preheating platform 5 is perpendicular to the extension direction of the strip laser 2, thereby completing the annealing of the perovskite film 3.

[0081] The sprayed perovskite precursor solution can be used for the growth of perovskite film 3 grains during the annealing process; at the same time, the strip laser 2 is used for heating scanning to complete the annealing process, forming a one-dimensional temperature gradient in the length direction in the crystallization transition region 9, so that the grains can grow along the length direction without size restrictions in the length direction, thereby improving the crystallization uniformity, grain size and crystallinity of the perovskite film layer, reducing the trap state density of the perovskite film layer, and then reducing charge recombination, and the conversion efficiency of the perovskite film 3 is greatly improved.

Claims

1. A perovskite thin film annealing device, characterized in that: The invention comprises a preheating platform (5) and a laser light source (1) capable of relative movement. The preheating platform (5) is used to carry a perovskite film (3) and a substrate (4) thereof. The preheating platform (5) heats the perovskite film (3) and the substrate (4) thereof. The laser light source (1) is used to generate a strip laser (2). The strip laser (2) irradiates the perovskite film (3) to form a one-dimensional temperature gradient in the length direction of the perovskite film (3).

2. A perovskite thin film annealing device according to claim 1, characterized in that: The length of the strip laser (2) is not less than the width of the perovskite film (3).

3. A perovskite thin film annealing device according to claim 2, characterized in that: The laser intensity at each location of the strip laser (2) is the same.

4. A perovskite thin film annealing device according to any one of claims 1 to 3, characterized in that: The annealing device also includes a scanning mechanism (6), wherein the scanning mechanism (6) includes a linear drive component, and a moving end of the linear drive component is connected to the laser light source (1) to achieve relative movement between the laser light source (1) and the perovskite film (3).

5. A perovskite thin film annealing device according to claim 4, characterized in that: The annealing equipment also includes a laser controller, which is used to control the laser parameters of the laser light source (1) emitting the strip laser (2) and to control the moving speed of the laser light source.

6. The perovskite thin film annealing device according to claim 5, characterized in that: The laser parameters include laser wavelength, laser power density and laser width.

7. A perovskite thin film annealing device according to claim 6, characterized in that: The laser wavelength is 248-1070nm, the laser width is 0.1-1mm, and the laser power density is 0.2-20W / mm 2 .

8. A perovskite thin film annealing process using the annealing device according to any one of claims 1 to 7, characterized in that: A strip laser (2) having a length not less than the width (3) of the perovskite film is irradiated onto the preheated perovskite film (3), and the strip laser (2) is scanned on the perovskite film (3) in the length direction of the perovskite film (3) to achieve the growth of the perovskite film (3) grains, thereby obtaining a perovskite film (3) containing perovskite grains with large grain sizes.

9. A perovskite thin film annealing process according to claim 8, characterized in that: Before preheating the perovskite film (3), the perovskite film (3) is wetted with a perovskite precursor solution.

10. A perovskite thin film annealing process according to claim 9, characterized in that: The laser wavelength of the strip laser (2) is 248-1070nm, the laser width is 0.1-1mm, and the laser power density is 0.2-20W / mm 2 , scanning speed is 2-200mm / min, and preheating temperature is 25-200℃.

Citation Information

Patent Citations

  • Laser line illumination

    CN109477970A

  • Preparation method of perovskite precursor solution and perovskite thin film

    CN114122267A

  • Perovskite film annealing device

    CN219660314U

Cited By

  • Perovskite photovoltaic device and annealing method, preparation method and application thereof

    CN119562744A

  • A perovskite photovoltaic device and its annealing method, preparation method and application

    CN119562744B

  • Method for preparing perovskite thin film

    CN119630250A

  • A method for preparing a perovskite thin film

    CN119630250B