Surface-treated zinc oxide particles, dispersion liquid, cosmetic, and method for producing surface-treated zinc oxide particles
By using specific alkylalkoxysilane as a surface treatment agent on zinc oxide particles, controlling the surface area and treatment agent content solves the problem of zinc oxide particle aggregation and achieves excellent usability and ultraviolet shielding effects in cosmetics.
Patent Information
- Application Number
- CN202380023666.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-27
- Filing Date
- 2023-04-25
- Publication Date
- 2024-10-11
AI Technical Summary
Surface-treated zinc oxide particles tend to agglomerate during the treatment process, resulting in a rough feeling and making it impossible to obtain an excellent use feel in cosmetics.
By using an alkylalkoxysilane with a carbon number of 6 to 10 as a surface treatment agent, the zinc oxide particles are surface treated to control the BET specific surface area to be 1.5m2/g or more and 8m2/g or less. Surface treatment The content of the agent is between 0.70% and below 0.92%, and heat treatment and crushing are performed to inhibit aggregation.
Surface-treated zinc oxide particles that suppress roughness are obtained and are suitable for use in cosmetics, providing excellent usability, transparency, and ultraviolet shielding properties.
Smart Images

Figure BDA0005010037320000061 
Figure BDA0005010037320000261
Abstract
Description
Technical Field
[0001] The present invention relates to surface treated zinc oxide particles, dispersion, cosmetics and a method for producing the surface treated zinc oxide particles.
[0002] This application claims priority based on Japanese Patent Application No. 2022-073189 filed in Japan on April 27, 2022, the contents of which are incorporated herein by reference. Background Art
[0003] Zinc oxide particles with UV shielding properties are used in cosmetics such as sunscreen and foundation cream.
[0004] When zinc oxide particles are applied to cosmetics, in order to make the surface state of the zinc oxide particles match the properties of the cosmetics or to suppress the catalytic activity of the zinc oxide particles, the surface treatment of the zinc oxide particles is performed. As the surface treatment agent of such zinc oxide particles, for example, metal soaps such as magnesium stearate, silicone oils such as polydimethylsiloxane and hydrogenated polydimethylsiloxane, and alkylalkoxysilanes such as octyltriethoxysilane are used (for example, refer to Patent Documents 1, 2, and 3).
[0005] Among them, the zinc oxide particles surface-treated with the alkylalkoxysilane described above have high stability because the alkylalkoxysilane is chemically bonded to the surface of the zinc oxide particles.
[0006] Furthermore, regarding the zinc oxide particles described above, the properties of the particle surfaces can be easily changed by using a surface treatment agent having a different substituent.
[0007] Thus, the zinc oxide particles surface-treated with alkylalkoxysilane (hereinafter, sometimes abbreviated as "surface-treated zinc oxide particles") can be directly blended into a cosmetic, or can be blended into a cosmetic in the form of a dispersion dispersed in a dispersion medium.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2002-362925
[0011] Patent Document 2: Japanese Patent Application Publication No. 2001-181136
[0012] Patent Document 3: Japanese Patent Application Laid-Open No. 08-104606 Summary of the invention
[0013] Technical issues to be solved by the invention
[0014] However, the surface-treated zinc oxide particles have a problem that the zinc oxide particles aggregate with each other during the surface treatment process. The aggregated surface-treated zinc oxide particles have a problem that they have a large rough feel and cannot provide a good feeling when blended into cosmetics.
[0015] The present invention is made in view of the above situation, and its purpose is to provide a surface-treated zinc oxide particle with reduced roughness. In addition, its purpose is to provide a dispersion liquid and a cosmetic containing such surface-treated zinc oxide particles. In addition, its purpose is to provide a method for producing such surface-treated zinc oxide particles.
[0016] Means for solving technical problems
[0017] In order to solve the above problems, the surface-treated zinc oxide particles of the first embodiment of the present invention are zinc oxide particles surface-treated with a surface treatment agent, wherein the BET specific surface area of the zinc oxide particles is 1.5 m 2 / g or more and 8m 2 / g or less, the surface treatment agent is an alkylalkoxysilane having an alkyl group with a carbon number of 6 or more and 10 or less, the content of the surface treatment agent is 0.70 mass % or more and 0.92 mass % or less, and the particle size D98 when the cumulative volume percentage of the dry particle size distribution is 98% is 40 μm or less.
[0018] The surface-treated zinc oxide particles according to the first aspect of the present invention may be configured such that the surface treatment agent is at least one of octyltrimethoxysilane and octyltriethoxysilane.
[0019] The dispersion liquid of the second aspect of the present invention contains the surface-treated zinc oxide particles and a dispersion medium.
[0020] The cosmetic according to the third aspect of the present invention contains at least one selected from the group consisting of the surface-treated zinc oxide particles and the dispersion.
[0021] The method for producing the surface-treated zinc oxide particles according to the fourth aspect of the present invention is a method for producing the surface-treated zinc oxide particles, the method comprising the steps of: mixing zinc oxide particles and a surface treatment agent to surface-treat the zinc oxide particles; heat-treating the surface-treated zinc oxide particles; and crushing the surface-treated zinc oxide particles after the heat treatment, wherein the BET specific surface area of the zinc oxide particles is 1.5 m 2 / g or more and 8m 2 / g or less, the surface treatment agent is an alkylalkoxysilane having an alkyl group with 6 to 10 carbon atoms, the mixing amount of the surface treatment agent is 1.2 to 3.5 parts by mass relative to 100 parts by mass of the zinc oxide particles, and in the step of surface-treating the zinc oxide particles, the content of the solvent is 2% by mass or less relative to the total mass of the zinc oxide particles and the surface treatment agent.
[0022] Effects of the Invention
[0023] According to the present invention, it is possible to provide surface-treated zinc oxide particles with reduced roughness. Furthermore, according to the present invention, it is possible to provide a dispersion liquid and a cosmetic containing such surface-treated zinc oxide particles. Furthermore, according to the present invention, it is possible to provide a method for producing such surface-treated zinc oxide particles. DETAILED DESCRIPTION
[0024] Hereinafter, examples of preferred embodiments of the surface-treated zinc oxide particles, the dispersion, the cosmetic, and the method for producing the surface-treated zinc oxide particles of the present invention will be described.
[0025] In addition, in the present embodiment, specific description is given for a better understanding of the purpose of the invention, and unless otherwise specified, the present invention is not limited. For example, as long as there is no special limitation, conditions such as materials, amounts, types, quantities, sizes, ratios, temperatures, etc. may be changed, added, or omitted as needed. Preferred examples may be exchanged or shared between the embodiments described below.
[0026] [Surface treated zinc oxide particles]
[0027] The surface-treated zinc oxide particles of this embodiment are zinc oxide particles surface-treated by a surface treatment agent, wherein the BET specific surface area of the zinc oxide particles is 1.5 m 2 / g or more and 8m 2 / g or less, the surface treatment agent is an alkylalkoxysilane having an alkyl group with a carbon number of 6 or more and 10 or less, the content of the surface treatment agent is 0.70 mass % or more and 0.92 mass % or less, and the particle size D98 (hereinafter sometimes abbreviated as "D98") when the cumulative volume percentage of the dry particle size distribution is 98% is 40 μm or less. The surface treatment in the surface-treated zinc oxide particles of the present embodiment refers to modifying the surface of the zinc oxide particles with a surface treatment agent. That is, the surface treatment in the surface-treated zinc oxide particles of the present embodiment refers to forming a film composed of a surface treatment agent on at least a portion of the surface of the zinc oxide particles, or making the surface treatment agent adhere to at least a portion of the surface of the zinc oxide particles.
[0028] Regarding the surface-treated zinc oxide particles of the present embodiment, the surface-treated zinc oxide particles having a specific BET specific surface area are surface-treated using a specific alkylalkoxysilane at a specific mass ratio without adding a solvent. Therefore, the agglomeration of zinc oxide particles and surface-treated zinc oxide particles can be suppressed, and surface-treated zinc oxide particles with a small D98 can be obtained. In this way, the surface-treated zinc oxide particles with suppressed agglomeration are suitable for use in cosmetics because the roughness when applied to the skin is suppressed.
[0029] Regarding the surface-treated zinc oxide particles of the present embodiment, the Si content is preferably 0.06 mass % or more and 0.30 mass % or less. It can also be 0.07 mass % or more and 0.25 mass % or less, 0.08 mass % or more and 0.20 mass % or less, 0.09 mass % or more and 0.15 mass % or less, 0.10 mass % or more and 0.13 mass % or less, etc. If the Si content is within the range, the surface of the zinc oxide particles is fully hydrophobicized. As a result, when the surface-treated zinc oxide particles of the present embodiment are blended into cosmetics, the use feeling is excellent.
[0030] The surface treated zinc oxide particles of the present embodiment preferably have a hydroxyl treatment rate of 98% by mass or more. When the hydroxyl treatment rate is 98% by mass or more, aggregation of the surface treated zinc oxide particles can be suppressed, and surface treated zinc oxide particles with a small D98 can be obtained.
[0031] In this specification, the "BET specific surface area" refers to a value measured by the BET method using a specific surface area measuring device (for example, a fully automatic specific surface area measuring device (trade name: Macsorb HM Model-1201, manufactured by MOUNTECH Co., Ltd.)).
[0032] In the present specification, "the content of the surface treatment agent" is calculated according to the following general formula (1).
[0033] Content of surface treatment agent = (heat loss - drying loss) × molecular weight of surface treatment agent / molecular weight of alkyl group of surface treatment agent ... (1)
[0034] In this specification, "loss on drying" means loss on drying at 105°C for 2 hours, and can be obtained by the following method.
[0035] First, 2 g of surface-treated zinc oxide particles are prepared. The surface-treated zinc oxide particles are preferably particles stored under dry conditions. The particles can be heated in a dryer set at 105° C. for 2 hours, and the mass after heating is measured, and the mass reduction rate is taken as the drying loss (mass %).
[0036] That is, the loss on drying can be obtained by the following formula (2) using the above measurement results.
[0037] Drying loss of surface-treated zinc oxide particles (mass %) = (mass of surface-treated zinc oxide particles before heating - mass of surface-treated zinc oxide particles after heating) / mass of surface-treated zinc oxide particles before heating × 100 ... (2)
[0038] In this specification, "heat reduction" means heat reduction at 500° C. for 4 hours, and can be obtained by the following method.
[0039] First, 2 g of surface-treated zinc oxide particles are prepared. The surface-treated zinc oxide particles are preferably particles stored under dry conditions. The particles can be heated in an electric furnace set at 500° C. for 4 hours, and the mass after heating is measured, and the mass reduction rate is taken as the strong heat loss (mass %).
[0040] That is, the heat loss can be obtained by the following formula (3) using the above measurement results.
[0041] Heat loss of surface-treated zinc oxide particles (mass %) = (mass of surface-treated zinc oxide particles before heating - mass of surface-treated zinc oxide particles after heating) / mass of surface-treated zinc oxide particles before heating × 100 ... (3)
[0042] If octyltriethoxysilane is used as the surface treatment agent, the molecular weight of the surface treatment agent, that is, the molecular weight of octyltriethoxysilane, is 276.49. Moreover, the molecular weight of the alkyl group of octyltriethoxysilane is 113.08. By using this molecular weight ratio in formula (1), the content of the surface treatment agent can be calculated.
[0043] The loss on drying can be considered to be a mass reduction caused by impurities other than the surface-treated zinc oxide particles, such as water contained in the surface-treated zinc oxide particles and unreacted surface treatment agent, which are removed by heating at 105°C.
[0044] The heat loss is considered to be a mass loss caused by the removal of the impurities and the removal of the alkyl groups in the alkylalkoxysilane attached to the zinc oxide particles by heating at 500°C.
[0045] Therefore, in the present embodiment, the content of the surface treatment agent calculated by the above general formula (1) is regarded as the content of the surface treatment agent actually attached to the zinc oxide particles by the surface treatment.
[0046] In this specification, the "Si content" refers to a value measured by the following method using a spectroscopic analyzer (for example, an ICP emission spectroscopic analyzer ICP-AES 700-ES (manufactured by Varian)).
[0047] 0.2g of the surface-treated zinc oxide particles of the object to be measured is placed in a platinum crucible, and the temperature is gradually raised to 700°C in an electric furnace to ashed the surface-treated zinc oxide particles. 2g of lithium tetraborate is added to the ashed sample, and heated to 925°C in an electric furnace to melt it. Then, the molten sample is placed in a 100mL tall beaker together with the platinum crucible. Then, 70mL of warm water and 8mL of nitric acid are added to the tall beaker, and the sample is heated and stirred with a heating stirrer to dissolve the sample. The dissolved solution is transferred to a 200mL volumetric flask and fixed to volume, and it is used as a detection solution. The detection solution can be appropriately diluted. Y standard solution is added to the detection solution as an internal standard substance to make Y reach 1000ppm. A calibration curve is prepared using an element standard solution of known concentration. In addition, y, lithium tetraborate and nitric acid as internal standard substances are also added to the element standard solution used for the preparation of the calibration curve to reach the same concentration as the detection solution. The detection solution is measured with an ICP emission spectrometer and quantified by the calibration curve method.
[0048] Since the surface treatment agent used in the present embodiment is alkylalkoxysilane, the content of the surface treatment agent attached to the zinc oxide particles can also be measured based on the Si content.
[0049] In this specification, "D98" means a value when the cumulative volume percentage is 98% when the volume particle size distribution is measured by dry method using a particle size distribution analyzer (for example, a laser diffraction particle size distribution analyzer (model: Mastersizer 3000, manufactured by Malvern)).
[0050] In this specification, the "hydroxyl group treatment rate" is measured using a red pigment that absorbs light having a wavelength of about 545 nm represented by the following general formula (4).
[0051] [Chemical formula 1]
[0052]
[0053] The red pigment in the general formula (4) can be produced by the following method.
[0054] 1 mmol of 2,2'-dihydroxyazobenzene, 1 mmol of diphenyltin (IV) oxide as a metal source, and 30 mL of acetone were mixed to prepare a mixed solution.
[0055] Next, the mixed liquid was stirred at 70° C. for 3 hours to carry out a dehydration reaction, thereby coordinating diphenyltin oxide and 2,2′-dihydroxyazobenzene.
[0056] The mixed liquid after the dehydration reaction is filtered, the filtrate is recovered, and the solvent is distilled off from the filtrate, thereby obtaining a red pigment represented by the general formula (4).
[0057] The red pigment represented by the above-mentioned general formula (4) is selectively adsorbed on the hydroxyl present on the surface of zinc oxide particles, and does not react with hydroxyl groups such as water or alcohol. Therefore, the amount of the metal hydroxyl contained in zinc oxide particles and surface-treated zinc oxide particles can be qualitatively and quantitatively evaluated without being affected by moisture. That is, by investigating the adsorption amount of the red pigment by the zinc oxide particles before the surface treatment and the adsorption amount of the red pigment by the surface-treated zinc oxide particles, the hydrophobic degree on the surface of zinc oxide particles can be investigated. That is, it refers to that the hydroxyl treatment rate on the surface of zinc oxide particles is higher, indicating that the hydroxyl present on the surface of zinc oxide particles is surface-treated and hydrophobized.
[0058] Specifically, the hydroxyl group treatment rate (%) of the red pigment can be measured by the following method.
[0059] 5×10 -5 mol / L evaluation solution C1. The absorbance C2 of solution C1 at a wavelength of 545 nm was measured.
[0060] xg of zinc oxide particles before surface treatment were added to the evaluation solution C1, and the mixture was stirred and mixed at 60°C for 4 hours to prepare a mixed solution. -3 The zinc oxide particles were removed from the mixed solution by centrifugal separation to obtain a mixed solution A1 for evaluation. The absorbance A2 of the mixed solution A1 at a wavelength of 545 nm was measured.
[0061] yg of the surface-treated zinc oxide particles to be measured were added to the evaluation solution C1, and the mixture was stirred and mixed at 60°C for 4 hours to prepare a mixed solution. -3 The surface treated zinc oxide particles were removed from the mixed solution by centrifugal separation to obtain a mixed solution B1 for evaluation. The absorbance B2 of the mixed solution B1 at a wavelength of 545 nm was measured.
[0062] The adsorption amount (mol / m 2 ).
[0063] Adsorption amount A3 = ((A2-C2) / C2) × 250 × 10 -9(mol) / x(g)……(5)
[0064] The adsorption amount (mol / m 2 ).
[0065] Adsorption amount B3 = ((B2-C2) / C2) × 250 × 10 -9 (mol) / y(g)……(6)
[0066] In general formulas (5) and (6), a decrease in absorbance indicates adsorption of the dye. Therefore, the adsorption amount of the red dye was calculated based on the idea that the decrease rate of absorbance = the adsorption rate of the dye can be converted.
[0067] The hydroxyl group treatment rate can be calculated by the following general formula (7).
[0068] Hydroxyl treatment rate (%) = 100 - ((B3 / A3) × 100) ... (7)
[0069] (BET specific surface area of surface treated zinc oxide particles)
[0070] The BET specific surface area of the surface treated zinc oxide particles can be arbitrarily selected, but is preferably 1.5 m 2 / g or more, more preferably 2.5m 2 / g or more, more preferably 3.0m 2 / g or more, particularly preferably 3.5m 2 / g or more. In addition, the BET specific surface area of the surface-treated zinc oxide particles is preferably 8 m 2 / g or less, and preferably 8.0m 2 / g or less, more preferably 7.5m 2 / g or less, more preferably 7m 2 If necessary, the BET specific surface area of the surface-treated zinc oxide particles can be 6.5 m 2 / g or less, and can also be 6.0m 2 The above upper limit value and lower limit value of the BET specific surface area of the surface-treated zinc oxide particles may be combined arbitrarily.
[0071] If the BET specific surface area of the surface treated zinc oxide particles is 1.5 m 2 / g or more and 8m 2 / g or less, when blended in cosmetics, the transparency and ultraviolet shielding properties are excellent.
[0072] In addition, the value of the BET specific surface area of the zinc oxide particles before the surface treatment and the BET specific surface area of the surface-treated zinc oxide particles after the surface treatment do not change significantly.
[0073] (Average primary particle size of surface treated zinc oxide particles)
[0074] The average primary particle size of the surface-treated zinc oxide particles of the present embodiment is preferably 130 nm or more, more preferably 150 nm or more, and further preferably 200 nm or more. In addition, the average primary particle size of the surface-treated zinc oxide particles of the present embodiment is preferably 300 nm or less, more preferably 270 nm or less, and further preferably 250 nm or less.
[0075] When the surface-treated zinc oxide particles have an average primary particle size of 130 nm or more and 300 nm or less, the particles are excellent in transparency and ultraviolet shielding properties when incorporated into a cosmetic.
[0076] The average primary particle size of the surface-treated zinc oxide particles can be calculated by the following general formula (8) using the BET specific surface area of the surface-treated zinc oxide particles.
[0077] Average primary particle size (nm) = 6000 / (BET specific surface area (m 2 / g)×ρ(g / cm 3 )……(8)
[0078] (where ρ is the density of zinc oxide particles, i.e. 5.61 g / cm 3 . )
[0079] Alternatively, the average primary particle size of the surface-treated zinc oxide particles can also be obtained by the following method. That is, when the surface-treated zinc oxide particles are observed using a transmission electron microscope (TEM) or the like, a predetermined number (e.g., 200 or 100) of surface-treated zinc oxide particles are selected. Furthermore, the longest straight line portion (maximum major diameter) of each of these surface-treated zinc oxide particles is measured, and these measured values are arithmetic averaged.
[0080] In the case where the surface-treated zinc oxide particles are aggregated, the aggregate particle size of the aggregate is not measured. A predetermined number of surface-treated zinc oxide particles (primary particles) constituting the aggregate are measured and the average primary particle size is taken as the average primary particle size.
[0081] (Zinc Oxide Particles)
[0082] The BET specific surface area of the zinc oxide particles in this embodiment is 1.5 m 2 / g or more and 8m 2 / g or less, preferably 2.5m 2 / g or more and 7.0m 2 The BET specific surface area of zinc oxide particles can be 3.5 m 2 / g or above and 6.5m2 / g or less, and can also be 4.5m 2 / g or more and 6.0m 2 When the BET specific surface area of the zinc oxide particles is less than the lower limit, the transparency will decrease when mixed into the cosmetic, so it is not preferred. If the BET specific surface area of the zinc oxide particles exceeds the upper limit, when the surface-treated zinc oxide particles are contained in the cosmetic at a high concentration, the particles are sometimes easily agglomerated, so it is not preferred.
[0083] As described above, the BET specific surface area of the zinc oxide particles in the present embodiment refers to a value measured by the BET method using a specific surface area measuring device (for example, a fully automatic specific surface area measuring device (trade name: Macsorb HM Model-1201, manufactured by MOUNTECH Co., Ltd.)).
[0084] The average primary particle size of the zinc oxide particles in this embodiment is preferably 130 nm or more, more preferably 150 nm or more, and further preferably 200 nm or more. Also, the average primary particle size of the zinc oxide particles in this embodiment is preferably 300 nm or less, more preferably 270 nm or less, and further preferably 250 nm or less.
[0085] When the zinc oxide particles have an average primary particle size of 130 nm or more and 300 nm or less, the particles have excellent transparency and ultraviolet shielding properties when incorporated into a cosmetic.
[0086] The average primary particle size of the zinc oxide particles can be calculated by the general formula (8) using the BET specific surface area of the zinc oxide particles, similarly to the BET-converted particle size of the surface-treated zinc oxide particles.
[0087] In addition, the average primary particle size of the zinc oxide particles can also be measured using a transmission electron microscope, similar to the average primary particle size of the surface-treated zinc oxide particles.
[0088] In the present embodiment, by surface-treating the zinc oxide particles, the BET specific surface area of the surface-treated zinc oxide particles tends to be smaller than the BET specific surface area of the zinc oxide particles before the surface treatment, but the BET specific surface area of the surface-treated zinc oxide particles and the BET specific surface area of the zinc oxide particles before the surface treatment are substantially the same in size. Similarly, by surface-treating the zinc oxide particles, the average primary particle size of the surface-treated zinc oxide particles tends to be larger than the average primary particle size of the zinc oxide particles before the surface treatment, but the average primary particle size of the surface-treated zinc oxide particles and the average primary particle size of the zinc oxide particles before the surface treatment are substantially the same in size. Here, substantially the same means that the difference in the BET specific surface area of the zinc oxide particles and the surface-treated zinc oxide particles is 5 m 2 / g or less.
[0089] From the viewpoint of improving dispersion stability in cosmetics, the zinc oxide particles in the present embodiment are preferably high-purity zinc oxide particles.
[0090] (Surface treatment agent)
[0091] The surface treatment agent in the present embodiment is an alkylalkoxysilane having an alkyl group having 6 to 10 carbon atoms, and among the silane coupling agents represented by the following general formula (9), silane coupling agents that can be used in cosmetics can be preferably used.
[0092] R 1 n Si(OR 2 ) 4-n ……(9)
[0093] (Among them, R 1 represents an alkyl group having 6 to 10 carbon atoms, R 2 represents an alkyl group having 1 to 4 carbon atoms, and n represents 1 to 3. )
[0094] R 1 An alkyl group having 7 to 9 carbon atoms is preferred, and an alkyl group having 8 carbon atoms is more preferred.
[0095] R 2 An alkyl group having 1 to 3 carbon atoms is preferred, and an alkyl group having 1 to 2 carbon atoms is more preferred.
[0096] n is preferably 1 or more and 2 or less, and n is more preferably 1.
[0097] Specifically, in the present embodiment, as the surface treatment agent, for example, alkyl alkoxysilanes such as hexyltrimethoxysilane, hexyltriethoxysilane, heptyltrimethoxysilane, heptyltriethoxysilane, octyltrimethoxysilane, octyltriethoxysilane (triethoxyoctylsilane), nonyltrimethoxysilane, nonyltriethoxysilane, decyltrimethoxysilane, and decyltriethoxysilane can be cited. Among these, alkyl alkoxysilanes having an octyl group in the molecule are preferred.
[0098] Specifically, the polarity of the functional group is moderate, and octyltriethoxysilane and octyltrimethoxysilane are preferred, since they can cope with oil phases having a wide range of polarities, from natural oils and ester oils to silicone oils. Octyltriethoxysilane is particularly preferred.
[0099] The surface treatment using the surface treatment agent is preferably carried out by mixing the surface treatment agent in an amount of 1.2 parts by mass or more and 3.5 parts by mass or less relative to 100 parts by mass of the zinc oxide particles. The amount may be 1.5 parts by mass or more and 3.3 parts by mass or less, 1.8 parts by mass or more and 3.0 parts by mass or less, 2.0 parts by mass or more and 2.8 parts by mass or less, etc.
[0100] In the method described later, when the surface treatment is performed in such a manner that the surface treatment agent is 1.2 mass parts or more and 3.5 mass parts or less relative to 100 mass parts of zinc oxide particles, the content of the surface treatment agent calculated by the general formula (1) is 0.70 mass % or more and 0.92 mass % or less. The content of the surface treatment agent is preferably 0.72 mass % or more and 0.90 mass % or less, and more preferably 0.75 mass % or more and 0.85 mass % or less.
[0101] Furthermore, when the total amount of the surface-treated zinc oxide particles is 100 mass %, the Si content measured by the ICP emission spectrometer is 0.06 mass % or more and 0.30 mass % or less.
[0102] By the content of the surface treatment agent contained in the surface-treated zinc oxide particles being within the above range, the surface of the above-mentioned zinc oxide particles is fully hydrophobized. As a result, when the surface-treated zinc oxide particles of the present embodiment are blended into cosmetics, the use feeling is excellent. When the content of the surface treatment agent contained in the surface-treated zinc oxide particles is lower than the above lower limit, the surface of the zinc oxide particles cannot be fully hydrophobized, and the untreated surfaces of the zinc oxide particles are easily agglomerated with each other, resulting in D98 becoming larger, so it is not preferred. In addition, since the touch of the surface-treated zinc oxide particles deteriorates, it is not preferred. If the content of the surface treatment agent contained in the surface-treated zinc oxide particles exceeds the above upper limit, the surface-treated zinc oxide particles are easily agglomerated with each other due to the excess surface treatment agent, resulting in D98 becoming larger, so it is not preferred. In addition, since the touch of the surface-treated zinc oxide particles deteriorates, it is not preferred.
[0103] The surface treated zinc oxide particles of the present embodiment have a BET specific surface area of 1.5 m 2 / g or more and 8m 2 / g or less, the content of the surface treatment agent is 0.70 mass % to 0.92 mass % when the total mass of the surface-treated zinc oxide particles is 100 mass %, and it is important that the amount of the surface treatment agent is small.
[0104] The BET specific surface area is 1.5 m 2 / g or more and 8m 2 The zinc oxide particles having a surface area of less than 100 g are treated with a small amount of the above-mentioned surface treatment agent without adding a solvent. * a * b * b in the chromaticity diagram of the color system * The increase of is suppressed, and surface-treated zinc oxide particles with D98 of 40 μm or less can be obtained.
[0105] Regarding the surface-treated zinc oxide particles of the present embodiment, the red pigment of the general formula (4) is used, and the hydroxyl treatment rate calculated by the general formula (7) is preferably 98% or more, more preferably 99% or more, and further preferably 99.5% or more. For example, it can be 98.5% or more by mass, 99.0% or more by mass, or 99.9% or more by mass.
[0106] By setting the hydroxyl group treatment ratio within the above range, the surface of the zinc oxide particles is appropriately surface-treated and hydrophobized, and therefore the surface-treated zinc oxide particles can be easily blended into an oily cosmetic.
[0107] The surface treated zinc oxide particles of this embodiment have a * a * b * b in the chromaticity diagram of the color system* It is preferably 6.3 or less.
[0108] b * The lower limit of is preferably 0, but may be 2.0 or more, 3.0 or more, 4.0 or more, or 5.0 or more.
[0109] By making the L of the surface treated zinc oxide particles * a * b * b in the chromaticity diagram of the color system * When the surface-treated zinc oxide particles are blended into cosmetics, unintentional coloring can be suppressed.
[0110] As the L of the surface treated zinc oxide particles * a * b * b in the chromaticity diagram of the color system * The method may be a known method such as a spectrocolorimeter. For example, a spectrocolorimeter (manufactured by NIPPON DENSHOKU INDUSTRIES Co., Ltd., Spectro Color Meter SE7700) may be used.
[0111] The surface treated zinc oxide particles of the present embodiment have a D98 of 40 μm or less, preferably 38 μm or less, more preferably 36 μm or less, and further preferably 34 μm or less.
[0112] When D98 exceeds 40 μm, the roughness of the surface-treated zinc oxide particles becomes noticeable, and when the surface-treated zinc oxide particles are blended into cosmetics, it is difficult to obtain a cosmetic with excellent feel during use.
[0113] Furthermore, the zinc oxide particles may be surface-treated using a surface treatment agent for cosmetics other than the alkylalkoxysilane as long as the properties of the surface-treated zinc oxide particles of the present embodiment are not impaired.
[0114] As the surface treatment agent other than the alkylalkoxysilane, for example, inorganic materials such as silica and alumina, and organic materials such as silicone compounds, fatty acids, fatty acid soaps, fatty acid esters, and organic titanate compounds can be used.
[0115] The surface treated zinc oxide particles of the present embodiment are surface treated zinc oxide particles preferably produced by a production method without adding a solvent described later, using a specific surface treatment agent at a specific mass ratio, with D98 being 40 μm or less. Therefore, regarding the surface treated zinc oxide particles of the present embodiment, the surface of the zinc oxide particles is sufficiently hydrophobicized, the roughness is suppressed, and b * The increase of is suppressed, and the feeling of use when mixed into cosmetics is excellent.
[0116] [Method for producing surface-treated zinc oxide particles]
[0117] The method for producing surface-treated zinc oxide particles of the present embodiment includes: a step of mixing zinc oxide particles and a surface treatment agent to surface-treat the zinc oxide particles (hereinafter referred to as the "surface treatment step"); a step of heat-treating the surface-treated zinc oxide particles (hereinafter referred to as the "heat treatment step"); and a step of crushing the surface-treated zinc oxide particles after the heat treatment (hereinafter referred to as the "crushing step"). The BET specific surface area of the zinc oxide particles is 1.5 m 2 / g or more and 8m 2 / g or less, the surface treatment agent is an alkylalkoxysilane having an alkyl group with a carbon number of 6 or more and 10 or less, and the mixing amount of the surface treatment agent is 1.2 or more and 3.5 or less parts by mass relative to 100 parts by mass of the zinc oxide particles. In the surface treatment step, the content of the solvent is set to 2% by mass or less relative to the total mass of the zinc oxide particles and the surface treatment agent.
[0118] Here, setting the content of the solvent to 2% by mass or less in the surface treatment process means that, although there is a solvent produced by side reactions such as adsorbed water contained in the zinc oxide particles and alcohol produced in the hydrolysis reaction of the surface treatment agent, no water or organic solvent is added for the surface treatment reaction. In other words, it means that no solvent is added in the surface treatment process of this embodiment, and even if added, it is only a very small amount. "The content of the solvent is 2% by mass or less", in other words, "the amount of solvent added is 0% by mass".
[0119] Regarding the zinc oxide particles and the surface treatment agent, the same zinc oxide particles and the surface treatment agent as those described above can be used.
[0120] In order to uniformly perform surface treatment on the surface of the particles, a wet method is generally used. Even when a dry method is used, a method of adding a small amount of an organic solvent such as alcohol to perform surface treatment is generally used.
[0121] The present inventors also added a solvent such as water or alcohol and carried out surface treatment of zinc oxide particles in a dry manner.
[0122] However, the present inventors have found that zinc oxide particles are likely to aggregate with each other during the process of removing the solvent.
[0123] Therefore, the surface treatment is performed by a method without adding water or an organic solvent. However, if water or an organic solvent is not added, the surface of the zinc oxide particles cannot be sufficiently hydrophobized.
[0124] As a result of repeated trial and error, the inventors found that if a BET specific surface area of 1.5 m 2 / g or more and 8m 2 When zinc oxide particles having a surface area of 1.0-1.5 mm2 / g or less are surface-treated with 1.2 to 3.5 parts by mass of the alkylalkoxysilane based on 100 parts by mass of the zinc oxide particles, the surface treatment can be sufficiently performed without adding an organic solvent such as alcohol or water, thereby suppressing aggregation of the surface-treated zinc oxide particles.
[0125] Since zinc oxide particles used in cosmetics require high transparency, most of them have a BET specific surface area of 20 m 2 However, the present inventors have found that by using zinc oxide particles having a BET specific surface area of 1.5 m 2 / g or more and 8m 2 When the surface-treated zinc oxide particles have a surface area of 1000 Å or less and agglomeration of the surface-treated zinc oxide particles is suppressed, not only the transparency and ultraviolet shielding properties are excellent when mixed in cosmetics, but also the rough feeling is suppressed.
[0126] In the method for producing surface-treated zinc oxide particles of the present embodiment, preferably, an organic solvent such as alcohol is not added in the surface treatment step, and more preferably, neither water nor an organic solvent is added.
[0127] It is difficult to completely remove the moisture absorbed from the atmosphere. If the adsorbed water is 0, the surface treatment reaction will not be able to proceed, so water is inevitably contained in the zinc oxide particles. And, when the hydrolysis reaction of the surface treatment agent is carried out, alcohols derived from alkoxysilane will be produced. However, in the surface treatment process, if water or an organic solvent is added, it is necessary to remove their process, so that the surface-treated zinc oxide particles will agglomerate due to the removal process. Therefore, in the method for manufacturing surface-treated zinc oxide particles of the present embodiment, in the surface treatment process, the content of the solvent is set to 2% by mass or less relative to the total mass of the zinc oxide particles and the surface treatment agent. If the content of the solvent is 2% by mass or less, then in the above-mentioned heat treatment process, the agglomeration of the surface-treated zinc oxide particles can be suppressed. The amount of the organic solvent added is 0% by mass, and the amount of water and the organic solvent added is also 0% by mass. In other words, in all the processes of the method for manufacturing surface-treated zinc oxide particles of the present embodiment, the amount of water and the organic solvent added is 0% by mass. That is, it means that the content of solvents other than alcohol generated by adsorbed water of zinc oxide particles and hydrolysis reaction of the surface treatment agent is 0 mass %, and does not exclude additives, catalysts, and inevitably contained impurities added to the extent that they do not affect the effects of the present invention.
[0128] In the surface treatment step, the raw material having a BET specific surface area of 1.5 m 2 / g or more and 8m 2 The alkylalkoxysilane is added to the zinc oxide particles by droplets or spraying while the zinc oxide particles having a weight of 100 g or less are stirred in a mixer such as a Henschel mixer or a super mixer. Thereafter, the zinc oxide particles and the alkylalkoxysilane are stirred at a high speed for a predetermined time.
[0129] The stirring may be performed at room temperature, or may be performed at an arbitrarily selected temperature, for example, 30°C to 100°C.
[0130] The stirring speed is not particularly limited as long as it is a speed at which the zinc oxide particles and the alkylalkoxysilane are mixed and the surface treatment reaction proceeds, and for example, the stirring can be performed at a peripheral speed of 5 m / s to 60 m / s.
[0131] The stirring time is not particularly limited as long as it is a time for mixing the zinc oxide particles and the alkylalkoxysilane and performing the surface treatment reaction, and for example, the stirring time may be 1 minute to 1 hour, and preferably about 10 minutes to 30 minutes.
[0132] The mixing amount of the alkylalkoxysilane is 1.2 parts by mass or more and 3.5 parts by mass or less relative to 100 parts by mass of the zinc oxide particles. The mixing amount of the alkylalkoxysilane is preferably 1.4 parts by mass or more and 3.0 parts by mass or less, more preferably 1.6 parts by mass or more and 2.5 parts by mass or less, and further preferably 1.8 parts by mass or more and 2.3 parts by mass or less.
[0133] In the above-mentioned heat treatment process, as long as the surface of the zinc oxide particles is hydrophobized at a temperature and time that is appropriately performed. For example, a heat treatment of 30 minutes to 24 hours can be performed at a temperature of 70° C. to 200° C. The atmosphere in the heat treatment is not particularly limited as long as it does not hinder the surface treatment, and can be any of an atmospheric atmosphere, an oxygen atmosphere, an inert atmosphere, a reduced pressure atmosphere or a vacuum atmosphere.
[0134] The heat treatment step can be performed while stirring.
[0135] The crushing step is not particularly limited as long as the crushing method can reduce the D98 of the surface-treated zinc oxide particles after the heat treatment to 40 μm or less.
[0136] The surface-treated zinc oxide particles after heat treatment can be crushed, for example, using a known crusher, such as an atomizer, a hammer mill, a jet mill, an impeller mill, a pin mill, and the like.
[0137] According to the method for producing surface-treated zinc oxide particles of this embodiment, with respect to a BET specific surface area of 1.5 m 2 / g or more and 8m 2 100 parts by mass of zinc oxide particles having a carbon number of 6 to 10 are mixed with 1.2 parts by mass or more and 3.5 parts by mass or less of an alkylalkoxysilane having an alkyl group having a carbon number of 6 to 10, and the surface treatment is performed in such a manner that the content of the solvent is 2% by mass or less relative to the total mass of the zinc oxide particles and the surface treatment agent, thereby obtaining surface-treated zinc oxide particles in which aggregation is suppressed.
[0138] [Dispersion liquid]
[0139] The dispersion liquid of the present embodiment contains the surface-treated zinc oxide particles of the present embodiment and a dispersion medium.
[0140] Furthermore, the dispersion liquid of the present embodiment also includes a paste-like dispersion having a high viscosity.
[0141] The dispersion medium is not particularly limited as long as it can be used in a cosmetic formulation and can disperse the surface-treated zinc oxide particles.
[0142] As the dispersion medium, for example, water, alcohols, esters, ethers, natural oils, ester oils, silicone oils, etc. are preferably used.
[0143] Examples of the alcohols include methanol, ethanol, n-propanol, isopropanol, n-butanol, 2-butanol, octanol, and glycerol.
[0144] Examples of the esters include ethyl acetate, butyl acetate, ethyl lactate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, and γ-butyrolactone.
[0145] Examples of the ethers include diethyl ether, ethylene glycol monomethyl ether (methyl cellosolve), ethylene glycol monoethyl ether (ethyl cellosolve), ethylene glycol monobutyl ether (butyl cellosolve), diethylene glycol monomethyl ether, and diethylene glycol monoethyl ether.
[0146] Furthermore, as other dispersion media, ketones, aromatic hydrocarbons, cyclic hydrocarbons, amides, chain polysiloxanes, cyclic polysiloxanes, modified polysiloxanes, hydrocarbon oils, ester oils, silicone oils, higher fatty acids, higher alcohols, and the like can be used.
[0147] Examples of ketones include acetone, methyl ethyl ketone, methyl isobutyl ketone, acetylacetone, and cyclohexanone.
[0148] Examples of the aromatic hydrocarbon include benzene, toluene, xylene, and ethylbenzene.
[0149] Examples of the cyclic hydrocarbon include cyclohexane and the like.
[0150] Examples of the amides include dimethylformamide, N,N-dimethylacetoacetamide, and N-methylpyrrolidone.
[0151] Examples of the chain polysiloxanes include dimethyl polysiloxane, methylphenyl polysiloxane, and diphenyl polysiloxane.
[0152] Examples of cyclic polysiloxanes include octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, dodecamethylcyclohexasiloxane, etc. Examples of modified polysiloxanes include amino-modified polysiloxane, polyether-modified polysiloxane, alkyl-modified polysiloxane, and fluorine-modified polysiloxane.
[0153] Examples of the hydrocarbon oil include liquid paraffin, squalane, isoparaffin, branched light paraffin, vaseline, and ozokerite.
[0154] Examples of the ester oil include isopropyl myristate, cetyl isooctanoate, and tricaprylin.
[0155] Examples of the silicone oil include decamethylcyclopentasiloxane, dimethylpolysiloxane, and methylphenylpolysiloxane.
[0156] Examples of the higher fatty acid include lauric acid, myristic acid, palmitic acid, and stearic acid.
[0157] Examples of the higher alcohol include lauryl alcohol, cetyl alcohol, stearyl alcohol, hexyldodecanol, and isostearyl alcohol.
[0158] The above-mentioned dispersion media may be used alone or in combination of two or more.
[0159] The dispersion liquid of the present embodiment may contain commonly used additives within a range that does not impair its characteristics.
[0160] As additives, for example, preservatives, dispersants, dispersing aids, stabilizers, water-soluble binders, thickeners, oil-soluble drugs, oil-soluble pigments, oil-soluble proteins, UV absorbers and the like are preferably used.
[0161] The particle size (D50) of the surface-treated zinc oxide particles when the cumulative volume percentage of the particle size distribution in the dispersion of the present embodiment is 50% can be arbitrarily selected, but is preferably 600 nm or less, more preferably 500 nm or less, and further preferably 400 nm or less.
[0162] The lower limit of D50 is not particularly limited, and may be, for example, 130 nm or more, 140 nm or more, or 150 nm or more. The upper limit and lower limit of D50 may be arbitrarily combined.
[0163] The particle size (D90) of the surface-treated zinc oxide particles when the cumulative volume percentage of the particle size distribution in the dispersion of this embodiment is 90% can be arbitrarily selected, but is preferably 1 μm or less, more preferably 900 nm or less, and further preferably 800 nm or less.
[0164] The lower limit of D90 is not particularly limited, and may be, for example, 150 nm or more, 200 nm or more, or 250 nm or more. The upper limit and lower limit of D90 may be arbitrarily combined.
[0165] When the D50 of the dispersion is 600 nm or less, when the cosmetic prepared using the dispersion is applied to the skin, the surface-treated zinc oxide particles are easily evenly distributed, thereby improving the ultraviolet shielding effect, which is preferred. In addition, when the D90 of the dispersion is 1 μm or less, the transparency of the dispersion is high, and the transparency of the cosmetic prepared using the dispersion is also high, which is preferred.
[0166] That is, when D50 and D90 in the dispersion of the present embodiment are within the above ranges, a dispersion having excellent transparency and excellent ultraviolet shielding properties can be obtained. Furthermore, a cosmetic prepared using the dispersion also has excellent transparency and ultraviolet shielding properties.
[0167] The cumulative volume percentage of the particle size distribution in the dispersion can be measured using a dynamic light scattering particle size distribution measuring apparatus.
[0168] The content of the surface-treated zinc oxide particles in the dispersion of the present embodiment may be appropriately adjusted according to desired properties.
[0169] When the dispersion of the present embodiment is used in a cosmetic, the content of the surface-treated zinc oxide particles in the dispersion can be arbitrarily selected, but is preferably 10% by mass or more, more preferably 20% by mass or more, and further preferably 30% by mass or more. In addition, the content of the surface-treated zinc oxide particles in the dispersion is preferably 90% by mass or less, more preferably 85% by mass or less, and further preferably 80% by mass or less. The upper limit and lower limit of the content of the surface-treated zinc oxide particles in the dispersion can be arbitrarily combined.
[0170] By setting the content of the surface-treated zinc oxide particles in the dispersion to be within the above range, the surface-treated zinc oxide particles can be contained at a high concentration, thereby increasing the degree of freedom in formulation and setting the viscosity of the dispersion to a level that is easy to handle.
[0171] The viscosity of the dispersion of this embodiment can be arbitrarily selected, but is preferably 5 Pa·s or more, more preferably 8 Pa·s or more, further preferably 10 Pa·s or more, and most preferably 15 Pa·s or more. In addition, the viscosity of the dispersion is preferably 300 Pa·s or less, more preferably 100 Pa·s or less, further preferably 80 Pa·s or less, and most preferably 60 Pa·s or less. The upper limit and lower limit of the viscosity of the dispersion can be arbitrarily combined.
[0172] By setting the viscosity of the dispersion liquid to be within the above range, a dispersion liquid that is easy to handle can be obtained even if the dispersion liquid contains a high concentration of solid content (surface-treated zinc oxide particles).
[0173] The method for producing the dispersion of the present embodiment is not particularly limited, and for example, a method of mechanically dispersing the surface-treated zinc oxide particles of the present embodiment and the dispersion medium using a known dispersing device can be used.
[0174] The dispersing device can be selected as needed, and examples thereof include a stirrer, a rotation and revolution mixer, a homomixer, an ultrasonic homogenizer, a sand mill, a ball mill, a roll mill and the like.
[0175] The dispersion liquid of the present embodiment can be used for coating materials or the like having an ultraviolet shielding function or a gas permeation suppressing function, in addition to cosmetics.
[0176] According to the dispersion of the present embodiment, since the surface-treated zinc oxide particles of the present embodiment are included, when the dispersion is blended into a cosmetic, the rough feeling is suppressed and the dispersion has excellent transparency and ultraviolet shielding properties.
[0177] [Composition]
[0178] The composition of the present embodiment contains the surface-treated zinc oxide particles of the present embodiment, a resin, and a dispersion medium.
[0179] The content of the surface-treated zinc oxide particles in the composition of the present embodiment may be appropriately adjusted according to desired properties and is, for example, preferably 10% by mass or more and 40% by mass or less, and more preferably 20% by mass or more and 30% by mass or less.
[0180] When the content of the surface-treated zinc oxide particles in the composition is within the above range, the composition contains a high concentration of solid components (surface-treated zinc oxide particles), thereby sufficiently obtaining the properties of the surface-treated zinc oxide particles and obtaining a composition in which the surface-treated zinc oxide particles are uniformly dispersed.
[0181] The resin is not particularly limited as long as it is a resin generally used for industrial purposes, and examples thereof include acrylic resins, epoxy resins, urethane resins, polyester resins, silicone resins, and the like.
[0182] The content of the resin in the composition of the present embodiment is not particularly limited and can be appropriately adjusted according to the properties of the target composition.
[0183] The dispersion medium is not particularly limited as long as it is a dispersion medium generally used in industrial applications, and examples thereof include water, alcohols such as methanol, ethanol, and propanol, methyl acetate, ethyl acetate, toluene, methyl ethyl ketone, and methyl isobutyl ketone.
[0184] The content of the dispersion medium in the composition of the present embodiment is not particularly limited and can be appropriately adjusted according to the properties of the target composition.
[0185] The composition of the present embodiment may contain commonly used additives within a range that does not impair the properties thereof.
[0186] Examples of the additive include a polymerization initiator, a dispersant, and an antiseptic.
[0187] The method for producing the composition of the present embodiment is not particularly limited, and an example thereof includes a method of mechanically mixing the surface-treated zinc oxide particles of the present embodiment, a resin, and a dispersion medium using a known mixing device.
[0188] Furthermore, there can be mentioned a method of mechanically mixing the dispersion and the resin using a known mixing device.
[0189] Examples of the mixing device include a stirrer, a rotation-revolution mixer, a homomixer, and an ultrasonic homogenizer.
[0190] The composition of the present embodiment is applied to an arbitrarily selected substrate (e.g., a plastic substrate such as a polyester film) by a common coating method such as a roller coating method, a flow coating method, a spray coating method, a screen printing method, a brush coating method, a dipping method, etc., thereby forming a coating film. These coating films can be used for arbitrarily selected purposes, such as as an ultraviolet shielding film or a gas barrier film.
[0191] According to the composition of the present embodiment, since the surface-treated zinc oxide particles of the present embodiment are included, the composition can be easily mixed with a resin and can exhibit excellent transparency and ultraviolet shielding properties.
[0192] [Cosmetics]
[0193] The cosmetic material of one embodiment of the present embodiment contains at least one selected from the group consisting of the surface-treated zinc oxide particles of the present embodiment and the dispersion of the present embodiment. Alternatively, the cosmetic material of one embodiment of the present embodiment contains at least one selected from the group consisting of the surface-treated zinc oxide particles of the present embodiment, the dispersion of the present embodiment, and the composition of the present embodiment.
[0194] A cosmetic material of another embodiment contains a cosmetic base material and at least one selected from the group consisting of the surface-treated zinc oxide particles of this embodiment and the dispersion of this embodiment. Alternatively, a cosmetic material of another embodiment contains a cosmetic base material and at least one selected from the group consisting of the surface-treated zinc oxide particles of this embodiment, the dispersion of this embodiment, and the composition of this embodiment.
[0195] Cosmetic base raw materials refer to various raw materials that form the main body of cosmetics. Examples of cosmetic base raw materials include oily raw materials, water-based raw materials, surfactants, powder raw materials, and the like.
[0196] The oily raw material can be arbitrarily selected, and examples thereof include fats and oils, higher fatty acids, higher alcohols, and ester oils.
[0197] The aqueous raw material can be arbitrarily selected, and examples thereof include purified water, alcohol, and a thickener.
[0198] The powder raw material can be arbitrarily selected, and examples thereof include color pigments, white pigments, pearlescent agents, and extender pigments.
[0199] The cosmetic material of the present embodiment can be obtained, for example, by blending the dispersion of the present embodiment into a cosmetic base material such as emulsion, face cream, foundation cream, lipstick, blush, eye shadow, etc. according to a conventional method.
[0200] The cosmetic of the present embodiment can be obtained, for example, by blending the surface-treated zinc oxide particles of the present embodiment into an oil phase or a water phase to prepare an O / W type or W / O type emulsion, and then blending the emulsion with a cosmetic base material.
[0201] The content of the surface-treated zinc oxide particles in the cosmetic of the present embodiment can be appropriately adjusted according to the desired characteristics. For example, the lower limit of the content of the surface-treated zinc oxide particles can be 0.01% by mass or more, 0.1% by mass or more, or 1% by mass or more. In addition, the upper limit of the content of the surface-treated zinc oxide particles can be 50% by mass or less, 40% by mass or less, or 30% by mass or less. The upper limit and lower limit of the content of the surface-treated zinc oxide particles in the cosmetic can be arbitrarily combined.
[0202] Hereinafter, the sunscreen cosmetics will be described in detail.
[0203] In sunscreen cosmetics, in order to effectively shield ultraviolet rays (especially long-wavelength ultraviolet rays (UVA)) and obtain a good feel of use with less powdery and astringent feeling, it is also preferred to adjust the content of surface-treated zinc oxide particles. For example, the lower limit of the content of surface-treated zinc oxide particles in sunscreen cosmetics is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and further preferably 1% by mass or more. In addition, the upper limit of the content of surface-treated zinc oxide particles in sunscreen cosmetics can be 50% by mass or less, 40% by mass or less, or 30% by mass or less. The upper limit and lower limit of the content of surface-treated zinc oxide particles in sunscreen cosmetics can be arbitrarily combined. In addition, within the above range, preferred ranges such as 5% by mass to 15% by mass, 10% by mass to 20% by mass can be arbitrarily selected.
[0204] As necessary, the sunscreen cosmetic may contain inorganic microparticles or inorganic pigments other than the surface-treated zinc oxide particles, hydrophobic dispersion media, hydrophilic dispersion media, oils and fats, surfactants, moisturizers, thickeners, pH adjusters, nutrients, antioxidants, fragrances, preservatives, dispersants, defoamers, colorants, cosmetic ingredients, polymer substances, bio-derived ingredients, plant-derived ingredients, antibacterial agents, bactericides, mildew preventers, aqueous ingredients, oily ingredients, vitamins, emulsifiers, stabilizers, solubilizers, pearlescent agents, fat-enhancing substances, and the like.
[0205] Examples of the hydrophobic dispersion medium include hydrocarbon oils, ester oils, silicone oils, higher fatty acids, and higher alcohols.
[0206] Examples of the hydrocarbon oil include liquid paraffin, squalane, isoparaffin, branched light paraffin, vaseline, and ozokerite.
[0207] Examples of the ester oil include isopropyl myristate, cetyl isooctanoate, and tricaprylin.
[0208] Examples of the silicone oil include decamethylcyclopentasiloxane, dimethylpolysiloxane, and methylphenylpolysiloxane.
[0209] Examples of the higher fatty acid include lauric acid, myristic acid, palmitic acid, and stearic acid.
[0210] Examples of the higher alcohol include lauryl alcohol, cetyl alcohol, stearyl alcohol, hexyldodecanol, and isostearyl alcohol.
[0211] Examples of inorganic fine particles or inorganic pigments other than the surface-treated zinc oxide particles contained in cosmetics include calcium carbonate, calcium phosphate (apatite), magnesium carbonate, calcium silicate, magnesium silicate, aluminum silicate, kaolin, talc, titanium oxide, aluminum oxide, yellow iron oxide, γ-iron oxide, cobalt titanate, cobalt violet, silicon oxide, and the like.
[0212] The sunscreen cosmetic may further contain at least one organic ultraviolet absorber. Cosmetics containing both surface-treated zinc oxide particles and an organic ultraviolet absorber are preferred because they can increase the ultraviolet shielding area and enhance the ultraviolet shielding property through the reinforcing effect.
[0213] Examples of the organic ultraviolet absorber include benzotriazole ultraviolet absorbers, benzoylmethane ultraviolet absorbers, benzoic acid ultraviolet absorbers, anthranilic acid ultraviolet absorbers, salicylic acid ultraviolet absorbers, cinnamic acid ultraviolet absorbers, silicone cinnamic acid ultraviolet absorbers, and triazine ultraviolet absorbers.
[0214] Examples of the benzotriazole-based ultraviolet absorber include 2,2′-hydroxy-5-methylphenylbenzotriazole, 2-(2′-hydroxy-5′-tert-octylphenyl)benzotriazole, and 2-(2′-hydroxy-5′-methylphenyl)benzotriazole.
[0215] Examples of the benzoylmethane ultraviolet absorber include benzylhydrazine, anisylmethane, 4-tert-butyl-4′-methoxydibenzoylmethane, 1-(4′-isopropylphenyl)-3-phenylpropane-1,3-dione, and 5-(3,3′-dimethyl-2-norbornylene)-3-pentan-2-one.
[0216] Examples of the benzoic acid-based ultraviolet absorber include para-aminobenzoic acid (PABA), PABA monoglyceride, N,N-dipropoxy PABA ethyl ester, N,N-diethoxy PABA ethyl ester, N,N-dimethyl PABA ethyl ester, N,N-dimethyl PABA butyl ester, and N,N-dimethyl PABA methyl ester.
[0217] Examples of the anthranilic acid-based ultraviolet absorber include homomenthyl N-acetylanthranilate.
[0218] Examples of the salicylic acid-based ultraviolet absorber include amyl salicylate, menthyl salicylate, homomenthyl salicylate, octyl salicylate, phenyl salicylate, benzyl salicylate, and p-2-propanolphenyl salicylate.
[0219] Examples of the cinnamic acid-based ultraviolet absorber include octyl methoxycinnamate (ethylhexyl methoxycinnamate), di-p-methoxycinnamic acid-mono-2-ethylhexanoic acid glyceryl ester, octyl cinnamate, ethyl 4-isopropylcinnamate, methyl 2,5-diisopropylcinnamate, ethyl 2,4-diisopropylcinnamate, methyl 2,4-diisopropylcinnamate, propyl p-methoxycinnamate, isopropyl p-methoxycinnamate, isoamyl p-methoxycinnamate, octyl p-methoxycinnamate (2-ethylhexyl p-methoxycinnamate), 2-ethoxyethyl p-methoxycinnamate, cyclohexyl p-methoxycinnamate, ethyl α-cyano-β-phenylcinnamate, 2-ethylhexyl α-cyano-β-phenylcinnamate, and glyceryl mono-2-ethylhexanoyl-di-p-methoxycinnamate.
[0220] Examples of the silicone cinnamic acid ultraviolet absorber include [3-bis(trimethylsilyloxy)methylsilyl-1-methylpropyl]-3,4,5-trimethoxycinnamate, [3-bis(trimethylsilyloxy)methylsilyl-3-methylpropyl]-3,4,5-trimethoxycinnamate, [3-bis(trimethylsilyloxy)methylsilylpropyl]-3,4,5-trimethoxycinnamate, [3-bis(trimethylsilyloxy)methylsilylbutyl]-3,4,5-trimethoxycinnamate, [3-tris(trimethylsilyloxy)silylbutyl]-3,4,5-trimethoxycinnamate, and [3-tris(trimethylsilyloxy)silyl-1-methylpropyl]-3,4-dimethoxycinnamate.
[0221] Examples of the triazine-based ultraviolet absorber include bis-ethylhexyloxyphenol methoxyphenyl triazine, ethylhexyl triazone, methylenebisbenzotriazolyl tetramethylbutylphenol, terphenyl triazine, and diethylhexylbutyrylamino triazone.
[0222] Examples of organic ultraviolet absorbers other than the above include 3-(4'-methylbenzylidene)-d,l-camphor, 3-benzylidene-d,l-camphor, imidazole acrylic acid, imidazole ethyl acrylate, 2-phenyl-5-methylbenzoxazole, 5-(3,3'-dimethyl-2-nitrobornyl)-3-pentan-2-one, silicone-modified ultraviolet absorbers, fluorine-modified ultraviolet absorbers, etc. The above ultraviolet absorbers may be used alone or in combination of two or more.
[0223] The critical wavelength of the cosmetic of this embodiment is preferably 370 nm or more. When the critical wavelength of the cosmetic is 370 nm or more, a wide range of ultraviolet rays including long-wavelength ultraviolet rays (UVA) and short-wavelength ultraviolet rays (UVB) can be shielded.
[0224] According to the cosmetic of this embodiment, it contains at least one selected from the group consisting of the surface-treated zinc oxide particles of this embodiment, the dispersion of this embodiment, and the composition of this embodiment. Therefore, it is possible to obtain a cosmetic having excellent transparency and ultraviolet shielding properties, in which the roughness of the surface-treated zinc oxide particles is suppressed and which has a good feel when used.
[0225] Example
[0226] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples, but the present invention is not limited to the following Examples.
[0227] [Example 1]
[0228] "Preparation of surface-treated zinc oxide particles"
[0229] Zinc oxide particles A1 (BET specific surface area: 5 m 2 / g, manufactured by SUMITOMO OSAKA CEMENT Co., Ltd.) and 1.5 parts by mass of octyltriethoxysilane (trade name: Silquest A-137, manufactured by Momentive Performance Materials, Inc.) were mixed in a Henschel mixer heated to 60° C. at a peripheral speed of 15 m / s.
[0230] Next, the mixture was heat-treated at 95° C. for 6 hours under reduced pressure.
[0231] Next, the obtained dried product was crushed by a hammer mill at 16,000 revolutions to obtain surface-treated zinc oxide particles B1 of Example 1.
[0232] (Content of Octyltriethoxysilane)
[0233] The drying loss of 2 g of the surface-treated zinc oxide particles of Example 1 at 105° C. for 2 hours and the heat loss of 2 g of the surface-treated zinc oxide particles of Example 1 at 500° C. for 4 hours were measured, and the content of octyltriethoxysilane was calculated using the above general formulas (1) to (3). The results are shown in Table 1.
[0234] (Si content)
[0235] The Si content in the surface-treated zinc oxide particles of Example 1 was measured by the following method using an ICP emission spectrometer (trade name: ICP-AES 700-ES, manufactured by Varian).
[0236] 0.2 g of the surface treated zinc oxide particles of Example 1 were placed in a platinum crucible and gradually heated to 700° C. in an electric furnace to ashed the surface treated zinc oxide particles. 2 g of lithium tetraborate was added to the ashed sample and heated to 925° C. in an electric furnace to melt the sample.
[0237] Next, the molten sample was placed in a 100 mL tall beaker together with the platinum crucible.
[0238] Then, add 70mL of warm water and 8mL of nitric acid to the tall beaker, heat and stir with a heating stirrer to dissolve the sample. The dissolved solution is transferred to a 200mL volumetric flask and constant to volume, which is used as a detection solution. Y standard solution is added to the detection solution as an internal standard substance, so that Y reaches 1000ppm, as a detection solution for determination. The detection solution is measured with an ICP emission spectrometer, and the Si content in the surface-treated zinc oxide particles is quantified by a calibration curve method. In addition, about the calibration curve, Y, lithium tetraborate and nitric acid as internal standard substances are added to the element standard solution of known concentration to reach the same concentration as the detection solution, and the solution is used to make it.
[0239] (Determination of particle size distribution)
[0240] The volume particle size distribution of the surface-treated zinc oxide particles of Example 1 was measured in a dry manner using a laser diffraction particle size analyzer (trade name: Mastersizer 3000, manufactured by Malvern Panalytical Ltd.) equipped with a dry dispersion unit (trade name: AeroS, manufactured by Malvern Panalytical Ltd.).
[0241] (Determination of Hydroxyl Treatment Rate)
[0242] “Production of Red Pigment”
[0243] 1 mmol of 2,2'-dihydroxyazobenzene, 1 mmol of diphenyltin(IV) oxide, and 30 mL of acetone were mixed to prepare a mixed solution.
[0244] Next, the mixed liquid was stirred at 70° C. for 3 hours to carry out a dehydration reaction, thereby coordinating diphenyltin oxide and 2,2′-dihydroxyazobenzene.
[0245] The mixed liquid after the dehydration reaction is filtered, the filtrate is recovered, and the solvent is distilled off from the filtrate to obtain a red pigment represented by the above general formula (4).
[0246] "Preparation of Evaluation Solution"
[0247] 250 nmol (0.12 mg) of the obtained red pigment was dissolved in toluene to make 5 mL, and 5×10 -5 The absorbance C2 of the evaluation solution C1 at 545 nm was measured.
[0248] 4.0 mg of zinc oxide particles A1 were added to solution C1, and the mixture was stirred and mixed at 60° C. for 4 hours to prepare a mixed solution. The mixed solution was filtered with a syringe filter (0.2 μm), and the absorbance A2 of the filtrate at 545 nm was measured.
[0249] 4.0 mg of the surface-treated zinc oxide particles B1 of Example 1 was added to the solution C1, and the mixture was stirred and mixed at 60° C. for 4 hours to prepare a mixed solution. The mixed solution was filtered with a syringe filter (0.2 μm), and the absorbance B2 of the filtrate at 545 nm was measured.
[0250] The adsorption amount of the red pigment by the zinc oxide particles and the surface-treated zinc oxide particles was calculated by the above formulas (5) and (6).
[0251] The adsorption amount of the pigment of the surface-treated zinc oxide particles B3 = ((B2-C2) / C2) × 250 × 10 -9 (mol) / 4×10 -3 (g)……(6)
[0252] The adsorption amount of the pigment of the zinc oxide particles A3 = ((A2-C2) / C2) × 250 × 10 -9 (mol) / 4×10 -3 (g)……(5)
[0253] The hydroxyl group treatment rate of Example 1 was calculated by the above formula (7). The results are shown in Table 1.
[0254] Hydroxyl treatment rate = 100-(B3 / A3×100)……(7)
[0255] (Evaluation of hydrophobicity based on the limiting ethanol method)
[0256] The limiting ethanol method is a method of adding a sample to a solution formed by mixing water and ethanol to observe whether the sample is precipitated. In addition, the limiting ethanol method is a method in which if the sample does not precipitate, the ethanol ratio is increased, and when the sample precipitates, the water ratio is increased, thereby evaluating the hydrophobicity of the surface of the zinc oxide particles with the ethanol ratio required for the sample precipitation. The higher the ethanol ratio, the higher the surface hydrophobicity of the zinc oxide particles, and the higher the metal hydroxyl treatment rate.
[0257] The surface treated zinc oxide particles of Example 1 were evaluated by the limiting ethanol method. As a result, it was confirmed that 10 or more particles precipitated when the ethanol ratio was 40%. Table 1 shows the ethanol concentration when 10 or more surface treated zinc oxide particles precipitated.
[0258] (b * )
[0259] The b of the surface-treated zinc oxide particles of Example 1 was measured using a spectrocolorimeter (trade name: Spectro Color Meter SE7700, manufactured by NIPPON DENSHOKU INDUSTRIES Co., Ltd.). * The measurement was performed under the conditions of reflection (light 2 degree field of view) with a measurement diameter of 10 mm and using D65 light source as the light source.
[0260] Regarding the measurement sample, 10 g of the surface-treated zinc oxide particles of Example 1 were placed in a 30 mL spiral tube, which was tapped 30 times on a table, and the bottom surface of the spiral tube was used as the measurement surface.
[0261] (Evaluation of the feeling of use (touch))
[0262] The touch of the surface-treated zinc oxide particles of Example 1 was evaluated as follows. The surface-treated zinc oxide particles were taken out with the thumb and index finger, and the roughness was evaluated when rubbed. The surface-treated zinc oxide particles without roughness were evaluated as "○" (good), the surface-treated zinc oxide particles with a slight roughness were evaluated as "△" (acceptable), and the surface-treated zinc oxide particles with a roughness were evaluated as "×" (unacceptable). The results are shown in Table 1.
[0263] The less roughness the surface-treated zinc oxide particles have, the better the touch. Therefore, the degree of good touch is indicated by "○", "△", and "×" in order.
[0264] [Example 2]
[0265] Surface-treated zinc oxide particles of Example 2 were obtained in the same manner as in Example 1 except that 100 parts by mass of zinc oxide particles and 2.0 parts by mass of octyltriethoxysilane were used.
[0266] The content of the surface treatment agent, particle size distribution, hydroxyl treatment rate, hydrophobicity, b * The results are shown in Table 1.
[0267] [Example 3]
[0268] Surface-treated zinc oxide particles of Example 3 were obtained in the same manner as in Example 1 except that 100 parts by mass of zinc oxide particles and 3.0 parts by mass of octyltriethoxysilane were used.
[0269] The content of the surface treatment agent, particle size distribution, hydroxyl treatment rate, hydrophobicity, b * The results are shown in Table 1.
[0270] [Comparative Example 1]
[0271] Surface-treated zinc oxide particles of Comparative Example 1 were obtained in the same manner as in Example 1 except that 100 parts by mass of zinc oxide particles and 0.5 parts by mass of octyltriethoxysilane were used.
[0272] In the same manner as in Example 1, the content of the surface treatment agent, particle size distribution, hydroxyl treatment rate, hydrophobicity, b * The results are shown in Table 1.
[0273] [Comparative Example 2]
[0274] Surface-treated zinc oxide particles of Comparative Example 2 were obtained in the same manner as in Example 1 except that 100 parts by mass of zinc oxide particles and 1.0 parts by mass of octyltriethoxysilane were used.
[0275] The content of the surface treatment agent, particle size distribution, hydroxyl treatment rate, hydrophobicity, b * The results are shown in Table 1.
[0276] [Comparative Example 3]
[0277] Surface-treated zinc oxide particles of Comparative Example 3 were obtained in the same manner as in Example 1 except that 100 parts by mass of zinc oxide particles and 4.0 parts by mass of octyltriethoxysilane were used.
[0278] The content of the surface treatment agent, particle size distribution, hydroxyl treatment rate, hydrophobicity, b *The results are shown in Table 1.
[0279] [Comparative Example 4]
[0280] Surface-treated zinc oxide particles of Comparative Example 4 were obtained in the same manner as in Example 1 except that 100 parts by mass of zinc oxide particles and 5.0 parts by mass of octyltriethoxysilane were used.
[0281] The content of the surface treatment agent, particle size distribution, hydroxyl treatment rate, hydrophobicity, b * The results are shown in Table 1.
[0282] [Comparative Example 5]
[0283] Surface-treated zinc oxide particles of Comparative Example 5 were obtained in the same manner as in Example 1 except that 100 parts by mass of zinc oxide particles, 2.0 parts by mass of octyltriethoxysilane, and 36.0 parts by mass of isopropyl alcohol were used.
[0284] The content of the surface treatment agent, particle size distribution, hydroxyl treatment rate, hydrophobicity, b * The results are shown in Table 1.
[0285] [Table 1]
[0286]
[0287] By comparing Examples 1 to 3 with Comparative Examples 1 to 5, it was confirmed that the BET specific surface area was 1.5 m 2 / g or more and 8m 2 The surface-modified zinc oxide particles prepared by mixing zinc oxide particles with octyltriethoxysilane in a mass ratio of 100:1.2 to 100:3.5 have high hydrophobicity and a suppressed rough feeling. * Small.
[0288] Industrial Applicability
[0289] The present invention provides surface-treated zinc oxide particles with reduced roughness, a dispersion liquid and a cosmetic containing the surface-treated zinc oxide particles, and a method for producing the surface-treated zinc oxide particles. The surface-treated zinc oxide particles of the present invention are excellent in color and feel of use. Therefore, the surface-treated zinc oxide particles of the present invention can easily ensure the design quality when applied to dispersion liquids, compositions, coatings, and cosmetics, and have great industrial value.
Claims
1. A surface-treated zinc oxide particle, which is a zinc oxide particle surface-treated by a surface treatment agent, wherein: The BET specific surface area of the zinc oxide particles is 1.5 m 2 / g or more and 8m 2 / g or less, the surface treatment agent is an alkylalkoxysilane having an alkyl group with 6 to 10 carbon atoms, The content of the surface treatment agent is 0.70 mass % or more and 0.92 mass % or less, The particle size D98 when the cumulative volume percentage of the dry particle size distribution is 98% is 40 μm or less.
2. The surface-treated zinc oxide particles according to claim 1, wherein The surface treatment agent is at least one of octyltrimethoxysilane and octyltriethoxysilane. 3 . A dispersion comprising the surface-treated zinc oxide particles according to claim 1 or 2 and a dispersion medium. 4 . A cosmetic comprising at least one selected from the group consisting of the surface-treated zinc oxide particles according to claim 1 or 2 and the dispersion according to claim 3 .
5. A method for producing surface-treated zinc oxide particles, which is a method for producing the surface-treated zinc oxide particles according to claim 1 or 2, the method for producing the surface-treated zinc oxide particles comprising the following steps: mixing zinc oxide particles and a surface treatment agent to surface treat the zinc oxide particles; heat-treating the surface-treated zinc oxide particles; and The surface-treated zinc oxide particles after heat treatment are crushed. The BET specific surface area of the zinc oxide particles is 1.5 m 2 / g or more and 8m 2 / g or less, the surface treatment agent is an alkylalkoxysilane having an alkyl group with 6 to 10 carbon atoms, The mixing amount of the surface treatment agent is 1.2 parts by mass or more and 3.5 parts by mass or less relative to 100 parts by mass of the zinc oxide particles. In the step of surface-treating the zinc oxide particles, the content of the solvent is set to 2% by mass or less relative to the total mass of the zinc oxide particles and the surface treatment agent.