Polymer and preparation method thereof, gel polymer electrolyte, battery and electric device

By using polymers containing sulfone-based structures as polymer matrix for gel polymer electrolytes in lithium-ion batteries, the problems of insufficient high magnification and low temperature performance of lithium-ion batteries are solved, and higher ionic conductivity and migration efficiency are achieved , improving the overall performance of the battery.

CN118909255AActive Publication Date: 2024-11-08CONTEMPORARY AMPEREX TECHNOLOGY CO LTD

Patent Information

Application Number
CN202310512296.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-11-08
Estimated Expiration
2043-05-08

AI Technical Summary

Technical Problem

Existing lithium-ion batteries have shortcomings in high-rate charging and discharging and low-temperature cycling performance, mainly due to the low ion conductivity and metal-active ion migration efficiency of gel polymer electrolytes.

Method used

Using polymers containing sulfone-based structures as polymer matrix for gel polymer electrolytes, the sulfone-based structures are used as transition sites for metal active ions to improve ion conductivity, and optimize electrolytes through specific polymer molecular weight and dispersion index. The structure enhances the electrolyte's bundling capacity and transfer efficiency.

Benefits of technology

It significantly improves the rate performance and low-temperature cycling performance of lithium-ion batteries, improves the ion conductivity and migration rate of the battery, and reduces the internal impedance and volume expansion rate of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909255A_ABST
    Figure CN118909255A_ABST
Patent Text Reader

Abstract

The invention discloses a polymer and a preparation method thereof, a gel polymer electrolyte, a battery and an electric device, the general formula of the polymer is as shown in the formula (1): # imgabs0 #, R1 comprises substituted or unsubstituted C1-C4 alkyl, R2 and R3 respectively and independently comprise alkyl and / or alkoxy with the carbon atom number smaller than or equal to 3, and the value of n is 200-1000. Therefore, the gel polymer electrolyte containing the polymer has relatively high ionic conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of batteries, and in particular, to polymers and preparation methods thereof, gel polymer electrolytes, batteries, and electrical devices. Background Art

[0002] In recent years, as the application scope of secondary batteries becomes wider and wider, secondary batteries are widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, as well as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields. However, as the application scope of secondary batteries becomes wider and wider, the rate performance of secondary batteries has also been severely challenged. At present, there are still many problems to be solved in the industrial production and application of lithium-ion batteries. Summary of the invention

[0003] In the first aspect of the present application, the present application proposes a polymer, the general formula of the polymer is shown in formula (1):

[0004]

[0005] Among them, R 1 Including substituted or unsubstituted C 1 -C 4 The alkyl group, R 2 and R 3 Each independently comprises an alkyl group and / or an alkoxy group having a carbon number less than or equal to 3, and the value of n is 200 to 1000. Thus, when the metal active ions migrate, the sulfone structure can serve as a transition site in the metal active ion migration process, thereby improving the migration efficiency, and thus making the gel polymer electrolyte containing the polymer have a higher ion conductivity.

[0006] According to an embodiment of the present application, the number of carbon atoms between adjacent sulfone groups is less than or equal to 4. Thus, the distance between adjacent sulfone groups is relatively close, the metal active ion migration efficiency is relatively high, and the migration rate of metal active ions in the gel polymer electrolyte containing the polymer can be improved.

[0007] According to an embodiment of the present application, the number of carbon atoms between adjacent sulfone groups is 1 or 2. Thus, the distance between adjacent sulfone groups is relatively close, and the migration efficiency of metal active ions between adjacent sulfone groups is relatively high.

[0008] According to an embodiment of the present application, the content of sulfone groups in the polymer is 20%-80%. Therefore, the sulfone group content in the polymer is relatively high, which can provide more transition sites for metal ion migration, thereby further improving the migration rate of metal active ions in the gel polymer electrolyte containing the polymer.

[0009] According to an embodiment of the present application, the content of sulfone groups in the polymer is 60%-80%. Therefore, the content of sulfone groups in the polymer is relatively high, which can provide more transition sites for metal ion migration.

[0010] According to an embodiment of the present application, the carbon atom of the alkoxy group is connected to the sulfur atom on the sulfone group, thereby improving the oxidation resistance of the gel polymer electrolyte containing the polymer.

[0011] According to an embodiment of the present application, the number of carbon atoms between the oxygen atom of the alkoxy group and the sulfur atom of the adjacent sulfone group is less than or equal to 4. Thus, the oxygen atoms between the alkoxy groups can serve as transition sites when metal active ions are transferred between adjacent sulfone groups, which can further improve the migration rate of metal active ions in the gel polymer electrolyte containing the polymer.

[0012] According to an embodiment of the present application, the number of carbon atoms between the oxygen atom of the alkoxy group and the sulfur atom of the adjacent sulfone group is 1 or 2. As a result, the distance between the oxygen atom of the alkoxy group and the sulfone group is relatively close, and the migration efficiency of the metal active ion between the oxygen atom of the alkoxy group and the sulfone group is relatively high.

[0013] According to an embodiment of the present application, the polymer includes at least one of the following:

[0014]

[0015]

[0016]

[0017]

[0018] Thereby, the ion conductivity of the gel polymer electrolyte containing the polymer can be further improved.

[0019] According to an embodiment of the present application, the number average molecular weight of the polymer is 40000-80000. Therefore, the polymer has a good ability to bind electrolyte, and can improve the ionic conductivity and liquid content of the gel polymer electrolyte containing the polymer.

[0020] According to an embodiment of the present application, the number average molecular weight of the polymer is 55000-65000. Therefore, the polymer has a better ability to bind electrolyte.

[0021] According to an embodiment of the present application, the polymer dispersity index of the polymer is 1.5-2.5. Therefore, the polymer has high molecular weight uniformity, high internal structure consistency, and high transfer efficiency of metal active ions between adjacent sulfone groups.

[0022] According to an embodiment of the present application, the polymer dispersibility index of the polymer is 1.7-2.2. Thus, the transfer efficiency of metal active ions between adjacent sulfone groups is high.

[0023] In a second aspect of the present application, the present application proposes a method for preparing a polymer, comprising: adding a monomer and an initiator to a solvent, and performing a heating treatment to obtain the polymer, wherein the monomer comprises an alkane substituted with a sulfone group containing an unsaturated bond, and the alkane comprises a substituted or unsubstituted C 1 -C 4 The unsaturated bond comprises at least one of a double bond and a triple bond. Thus, a polymer that can effectively improve the ionic conductivity of the gel polymer electrolyte can be obtained by a relatively simple synthesis method.

[0024] According to an embodiment of the present application, the alkane includes at least two sulfone groups, and the number of carbon atoms between adjacent sulfone substituents is less than or equal to 4. Thus, the sulfone content of the obtained polymer can be increased.

[0025] According to an embodiment of the present application, the alkane further includes an ether bond, and the number of carbon atoms between the oxygen atom of the ether bond and the sulfur atom of the adjacent sulfone group is less than or equal to 4. Thus, the ionic conductivity of the gel polymer electrolyte containing the obtained polymer can be further improved.

[0026] According to an embodiment of the present application, the initiator includes at least one of azobisisoheptanenitrile, 2,2″-azabis(2-imidazoline) dihydrochloride, 2,2′-azobisisobutylamidine dihydrochloride, benzoyl peroxide, tert-butyl benzoyl peroxide, and methyl ethyl ketone peroxide. Thus, the yield of the polymer can be improved.

[0027] In the third aspect of the present application, the present application proposes a gel polymer electrolyte, comprising a polymer matrix, wherein the polymer matrix comprises the aforementioned polymer; and / or a polymer prepared by the aforementioned method. Therefore, the gel polymer electrolyte has all the characteristics and advantages of the aforementioned polymer and the aforementioned method, which will not be described in detail here.

[0028] According to an embodiment of the present application, the electrolyte includes a plasticizer and a metal salt, and the plasticizer includes a sulfone plasticizer, thereby improving the ionic conductivity of the gel polymer electrolyte.

[0029] According to an embodiment of the present application, the sulfone plasticizer includes at least one of sulfolane, dimethyl sulfone, ethyl methyl sulfone, ethyl isopropyl sulfone, and 3-methylcyclosulfone, thereby further improving the ionic conductivity of the gel polymer electrolyte.

[0030] According to an embodiment of the present application, the sulfone plasticizer includes sulfolane, thereby further improving the ionic conductivity of the gel polymer electrolyte.

[0031] According to an embodiment of the present application, the mass fraction of the polymer matrix in the gel polymer electrolyte is 10%-80%, thereby improving the mechanical strength of the gel polymer electrolyte.

[0032] According to an embodiment of the present application, the mass fraction of the plasticizer in the gel polymer electrolyte is 20%-60%, thereby improving the ionic conductivity of the gel polymer electrolyte and reducing the cost.

[0033] According to an embodiment of the present application, the mass fraction of the metal salt in the gel polymer electrolyte is 5%-30%, thereby reducing the cost of the gel polymer electrolyte.

[0034] In a fourth aspect of the present application, the present application proposes a battery, comprising the aforementioned gel polymer electrolyte. Thus, the battery has all the characteristics and advantages of the aforementioned gel polymer electrolyte, and the battery has better rate performance and low-temperature cycle performance.

[0035] In the fifth aspect of the present application, the present application proposes an electrical device, comprising the aforementioned gel polymer electrolyte and / or the aforementioned battery. Therefore, the electrical device has all the features and advantages of the aforementioned gel polymer electrolyte and battery, which will not be described in detail here. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0037] Figure 1 A schematic diagram of the structure of a battery according to an embodiment of the present application is shown;

[0038] Figure 2 A schematic diagram of a battery according to an embodiment of the present application is shown;

[0039] Figure 3 yes Figure 2 An exploded view of a battery according to an embodiment of the present application is shown;

[0040] Figure 4 A schematic diagram of a battery module according to an embodiment of the present application is shown;

[0041] Figure 5 A schematic diagram of a battery pack according to an embodiment of the present application is shown;

[0042] Figure 6 yes Figure 5An exploded view of a battery pack according to an embodiment of the present application is shown;

[0043] Figure 7 A schematic diagram of an electric device using a battery as a power source according to an embodiment of the present application is shown.

[0044] Description of reference numerals:

[0045] Battery pack 1, upper box 2, lower box 3, battery module 4, battery 5,

[0046] Positive electrode sheet 10 , positive electrode current collector 11 , positive electrode active material layer 12 , negative electrode sheet 20 , negative electrode current collector 21 , negative electrode active material layer 22 , separator 30 , gel polymer electrolyte 40 , shell 51 , electrode assembly 52 , top cover assembly 53 . DETAILED DESCRIPTION

[0047] The embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application.

[0048] In the description of the present application, it should be understood that the terms "length", "width", "thickness", "up", "down", "front", "back", "left", "right", etc., indicating the orientation or position relationship are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.

[0049] In the description of the present application, "A and / or B" may include the case of A alone, the case of B alone, or any of the cases of A and B, where A and B are only used for examples and may be any technical feature connected by "and / or" in the present application.

[0050] In the description of the present application, “plurality” means two or more.

[0051] Unless otherwise specified, all scientific and technological terms used in this application have the same meaning as those commonly understood by those skilled in the art to which this application belongs. All patents and publications related to this application are incorporated herein by reference in their entirety. The term "comprising" or "including" is an open expression, i.e., including the content specified in this application, but does not exclude the content of other aspects.

[0052] In the description of this application, regardless of whether the words "about" or "approximately" are used, all the numbers disclosed herein are approximate values. The value of each number may differ by less than 10% or a reasonable difference considered by those skilled in the art, such as 1%, 2%, 3%, 4% or 5%.

[0053] Taking lithium-ion batteries as an example, the rate charge and discharge performance of a battery is an important indicator to measure the capacity retention ability of a lithium-ion battery under rapid charge and discharge conditions. The rate charge and discharge performance of a battery depends on the mobility of lithium ions in the active material, the ionic conductivity of lithium ions in the electrolyte, and the ionic mobility of lithium ions at the electrode-electrolyte interface, among which the ionic conductivity of lithium ions in the electrolyte and the ionic mobility of lithium ions at the electrode-electrolyte interface are closely related to the composition and properties of the electrolyte inside the battery 5.

[0054] The electrolyte includes at least one of an organic liquid electrolyte, a solid polymer electrolyte, and a gel polymer electrolyte. The gel polymer electrolyte is a semi-solid electrolyte mixed with a liquid and a solid. The polymer molecules in the gel polymer electrolyte present a cross-linked spatial network structure, and the pores in the structure are filled with a liquid plasticizer. The lithium salt is dissolved in the polymer and the plasticizer, and the polymer matrix and the plasticizer are both continuous phases. By using a gel polymer electrolyte to replace or partially replace the organic liquid electrolyte, the production safety problems such as electrode corrosion and oxidative combustion caused by leakage of the organic liquid electrolyte can be effectively reduced.

[0055] In this application, lithium salt is taken as an example, and the metal active ion of lithium salt is Li + , Li + When dissolved in plasticizer, it will be solvated, thus + A solvated shell is formed on the surface, while the anions of the lithium salt are hardly solvated, making Li + The solvation effect of Li + The migration speed of the gel polymer electrolyte is also reduced. Due to the high viscosity of the gel polymer electrolyte, the transfer mode of the solvated metal active ions between the plasticizers is a hopping transfer, which in turn causes the lithium ions to encounter greater resistance when migrating between the positive electrode plate 10 and the negative electrode plate 20, ultimately resulting in the room temperature ion conductivity of the gel polymer electrolyte being only a fraction or even a few tens of percent of that of the organic liquid electrolyte, resulting in poor high rate charge and discharge performance and low temperature performance of the battery using the gel polymer electrolyte.

[0056] In the present application, a polymer containing a sulfone structure is used as the polymer matrix of the gel polymer electrolyte. When the metal active ions migrate between the positive electrode plate 10 and the negative electrode plate 20, the sulfone structure can serve as a transition site for the metal active ions in the process of migration between the positive electrode plate 10 and the negative electrode plate 20, providing a relatively close contact site for the hopping transfer of the metal active ions, and constructing a fast transmission channel for the metal active ions, so that the solvated metal active ions can be coordinated and combined with the sulfone group after being separated from the plasticizer, and then solvated after the sulfone group transition to participate in subsequent transfer. By using a polymer containing a sulfone structure as the polymer matrix of the gel polymer electrolyte, the ionic conductivity of the gel polymer electrolyte is effectively improved, thereby improving the rate performance and low-temperature cycle performance of the battery containing the gel polymer electrolyte.

[0057] As an example, the metal active ions may include at least one of lithium ions, sodium ions, and magnesium ions.

[0058] The battery disclosed in the embodiment of the present application can be used in, but not limited to, electrical devices such as vehicles, ships or aircraft. A power supply system having the battery, electrical devices, etc. disclosed in the present application can be used.

[0059] The present application embodiment provides an electric device using a battery and / or a battery as a power source, and the electric device includes but is not limited to a mobile phone, a tablet, a laptop, an electric toy, an electric tool, a battery car, an electric car, a ship, a spacecraft, etc. Among them, the electric toy may include a fixed or mobile electric toy, such as a game console, an electric car toy, an electric ship toy, and an electric airplane toy, etc., and the spacecraft may include an airplane, a rocket, a space shuttle, and a spacecraft, etc.

[0060] It should be understood that the technical solutions described in the embodiments of the present application are not limited to the batteries and electrical devices described above, but can also be applied to all electrical devices using batteries. However, for the sake of simplicity, the following embodiments are described using electric vehicles as examples.

[0061] In the first aspect of the present application, the present application proposes a polymer, the general formula of the polymer is shown in formula (1):

[0062]

[0063] Among them, R 1 Including substituted or unsubstituted C 1 -C 4 The alkyl group, R 2 and R 3Each independently includes an alkyl group and / or an alkoxy group having a carbon number less than or equal to 3. The gel polymer electrolyte containing the polymer can provide a fast transmission channel for the transfer of metal active ions, effectively improve the ionic conductivity of the gel polymer electrolyte, and improve the rate performance and low-temperature cycle performance of the battery containing the gel polymer electrolyte.

[0064] As an example, R 2 It may include at least one of a methyl group, an ethyl group, a propyl group, a methoxy group, an ethoxy group, and a propoxy group.

[0065] As an example, R 3 It may include at least one of a methyl group, an ethyl group, a propyl group, a methoxy group, an ethoxy group, and a propoxy group.

[0066] As an example, R 1 It may include at least one of a substituted or unsubstituted methyl group, a substituted or unsubstituted ethyl group, a substituted or unsubstituted n-propyl group, a substituted or unsubstituted isopropyl group, a substituted or unsubstituted n-butyl group, a substituted or unsubstituted sec-butyl group, a substituted or unsubstituted isobutyl group, and a substituted or unsubstituted tert-butyl group.

[0067] In some embodiments, R 1 Including substituted or unsubstituted C 1 -C 4 The alkyl group, R 1 The substituents may include a sulfone group.

[0068] By selecting sulfone-substituted R 1 The group can effectively increase the sulfone content in the polymer, and a higher sulfone content in the polymer can provide more transition sites for the transfer of metal active ions, thereby effectively improving the ionic conductivity of the gel polymer electrolyte containing the polymer.

[0069] In some embodiments, the number of carbon atoms between adjacent sulfone groups is less than or equal to 4. Optionally, the number of carbon atoms between adjacent sulfone groups is 1 or 2.

[0070] As an example, the spacing between adjacent sulfone groups is R 1 The group may be substituted or unsubstituted C 1 -C 4The alkyl group is an alkyl group in which the number of carbon atoms between adjacent sulfone groups can be 1, 2, 3 or 4. When the number of carbon atoms between adjacent sulfone groups is less than or equal to 4, the distance between adjacent sulfone groups is shorter. Compared with the two sulfone groups located at the para position of the benzene ring, the adjacent sulfone groups have smaller steric hindrance and better molecular chain flexibility, which can provide a faster lithium ion transmission speed. After the metal active ions separated from the solvation are combined with the sulfone groups, the metal active ions can also be transferred between the sulfone groups through the adjacent sulfone groups. After the metal active ions are separated from the sulfone groups, they can participate in the subsequent transfer through ion solvation. The transfer of metal active ions between adjacent sulfone groups is achieved through reversible coordination bonds, with high transfer efficiency, which can effectively improve the ionic conductivity of the gel polymer electrolyte.

[0071] In some embodiments, the position of the sulfone group can be adjusted accordingly according to the structure of the polymer. As long as the total number of carbon atoms between adjacent sulfone groups is less than or equal to 4, that is, as long as the sum of the number of main chain carbon atoms and the number of side chain carbon atoms between adjacent sulfone groups is less than or equal to 4, the transfer efficiency of metal active ions between adjacent sulfone groups can be improved, and the ionic conductivity of the gel polymer electrolyte can be effectively improved.

[0072] As an example, two adjacent sulfone groups can be located on the main chain of the polymer; as another example, one of the two adjacent sulfone groups can be located on the main chain of the polymer, and the other sulfone group can be located on the side chain of the polymer; as another example, two adjacent sulfone groups can be located on the side chain of the polymer.

[0073] As an example, adjacent sulfone groups may be separated by substituted or unsubstituted C 1 -C 4 Compared with the benzene ring, the substituted or unsubstituted C 1 -C 4 The alkyl group has less steric hindrance, and the resistance to the transfer of metal active ions between adjacent sulfone groups is smaller.

[0074] In some embodiments, the content of sulfone groups in the polymer may be 20%-80%. Alternatively, the content of sulfone groups in the polymer may be 60%-80%.

[0075] As an example, the content of sulfone groups in the polymer may be 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80%.

[0076] The content of sulfone groups in a polymer refers to the percentage of the mass of sulfone groups (O=S=O structure) in the polymer to the total mass of the polymer.

[0077] As an example, the content of sulfone groups in polymers can be determined by infrared spectroscopy. For example, a standard solution is first prepared with a sulfone group substance with a known sulfone group content, and the absorbance of the standard solution is measured. A standard curve is drawn according to the relationship between absorbance and content. Then the absorbance of the sample to be tested is measured, and the sulfone group content of the sample to be tested is obtained according to the standard curve. Specifically, the test method for sulfone group content is as follows: first, polymers with different sulfone group contents are synthesized, and then 1g of polymers with different sulfone group contents are dissolved in 15ml of acetonitrile solvent respectively to prepare a standard solution. Different absorption peak intensities are obtained by infrared spectroscopy testing, and a linear standard curve is drawn according to the relationship between peak intensity and sulfone group content. Then, the polymer with unknown sulfone content is also subjected to infrared testing according to the above-mentioned operating procedure, and the obtained absorption peak intensity is brought into the standard curve, and the sulfone group content can be known by comparative calculation.

[0078] When the content of sulfone groups in the polymer is 20%-80%, the polymer can provide more jumping sites for metal active ions, and the ionic conductivity of the gel polymer electrolyte containing the polymer is significantly improved; and the viscosity and rigidity of the gel polymer electrolyte containing the polymer are moderate, so that the ionic conductivity of the gel polymer electrolyte is relatively high.

[0079] In some embodiments, the carbon atom of the alkoxy group is attached to the sulfur atom of the sulfone group.

[0080] As an example, when R 2 and / or R 3 When including an alkoxy group with a carbon number less than or equal to 3, the carbon atom of the alkoxy group is connected to the sulfur atom on the sulfone group, that is, the oxygen atom of the alkoxy group is not directly connected to the sulfur atom of the adjacent sulfone group. Due to the low strength of the SO bond and poor oxidation resistance, when the oxygen atom of the alkoxy group is directly connected to the sulfur atom of the adjacent sulfone group, the oxidation resistance of the polymer is poor. In addition, since the surface of the positive electrode plate is highly oxidizing, the highly oxidizing positive electrode will cause the gel polymer electrolyte to undergo electrochemical side reactions on the surface of the positive electrode plate during the cycle process, resulting in a high volume expansion rate of the battery, a significant increase in internal impedance, and a significant decrease in capacity retention.

[0081] In some embodiments, the number of carbon atoms between the oxygen atom of the alkoxy group and the sulfur atom of the adjacent sulfone group is less than or equal to 4. Optionally, the number of carbon atoms between the oxygen atom of the alkoxy group and the sulfur atom of the adjacent sulfone group is 1 or 2.

[0082] As an example, when R 2 and / or R 3When an alkoxy group having a carbon number less than or equal to 3 is included, the number of carbon atoms between the oxygen atom of the alkoxy group and the sulfur atom of the adjacent sulfone group may be 1, 2, 3 or 4. When the number of carbon atoms between the oxygen atom of the alkoxy group and the sulfur atom of the adjacent sulfone group is less than or equal to 4, the distance between the oxygen atoms between the sulfone group and the alkoxy group is shorter, and the oxygen atoms between the alkoxy groups can serve as transition sites when metal active ions are transferred between adjacent sulfone groups, thereby improving the transfer efficiency of metal active ions and further improving the ionic conductivity of the gel polymer electrolyte.

[0083] In some embodiments, the polymer may include at least one of the following:

[0084]

[0085]

[0086]

[0087]

[0088] In some embodiments, when the degree of polymerization n of the polymer is 200-1000, the number average molecular weight of the polymer may be 40000-80000, and optionally, the number average molecular weight of the polymer may be 55000-65000. When the molecular weight of the polymer is 40000-80000, the polymer has a good liquid binding ability, and when the polymer is used as the polymer matrix of the gel polymer electrolyte, the polymer matrix has a good capacity to accommodate the electrolyte, which is beneficial to improve the migration number of metal active ions; at the same time, the viscosity of the gel polymer electrolyte containing the polymer is moderate, which can improve the ionic conductivity of the gel polymer electrolyte.

[0089] As an example, the number average molecular weight of the polymer can be 40,000, 42,000, 45,000, 48,000, 50,000, 52,000, 55,000, 58,000, 60,000, 62,000, 65,000, 68,000, 70,000, 72,000, 75,000, 78,000, 80,000.

[0090] The number average molecular weight measures the molecular weight of a polymer based on the number fraction. The number average molecular weight is numerically equal to the molecular weight of each component of the polymer multiplied by the mole fraction of the corresponding component.

[0091] As an example, the colligative properties of a polymer solution at extremely low concentrations are the same as those of an ideal solution, and the number average molecular weight of the polymer can be tested based on the colligative properties of the boiling point of the solution, that is, the boiling point elevation method. After a non-volatile polymer is added to a pure solvent to form a polymer solution, the vapor pressure of the solution decreases, resulting in a higher boiling point of the solution than the boiling point of the pure solvent, and a lower freezing point of the solution than the freezing point of the pure solvent. Specifically, it can be calculated according to the following formula:

[0092]

[0093] Among them, △T b =T 2 -T 1 , T 1 is the boiling point of the pure solvent, T 2 is the boiling point of the polymer solution; M n is the number average molecular weight of the polymer; c is the concentration of the polymer solution; K b It is a characteristic constant of a pure solvent and can be measured by the boiling point rise of a compound of known molecular weight.

[0094] In some embodiments, the dispersibility index of the polymer may be 1.5-2.5, and optionally, the dispersibility index of the polymer may be 1.7-2.2. Specifically, the dispersibility index of the polymer may be 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4 or 2.5. When the dispersibility index of the polymer is 1.5-2.5, the molecular weight distribution of the polymer is narrow, the consistency of the internal structure of the polymer is high, and the metal active ions have more sulfone structures with close distances when transferred inside the polymer, which can be used as transition sites, thereby having a higher transfer efficiency.

[0095] Polymer dispersity index (PDI) is used to describe the molecular weight distribution of polymers, where the ratio of the weight average molecular weight of the polymer to the number average molecular weight of the polymer is the polydispersity index, and the value of PDI is greater than 1. When the PDI is larger, the molecular weight distribution of the polymer is wider; when the PDI is smaller, the molecular weight distribution of the polymer is narrower.

[0096] As an example, the polymer dispersibility index of a polymer can be tested by gel permeation chromatography: Gel permeation chromatography (GPC), also known as size exclusion chromatography, can separate polymer molecules by utilizing their different molecular volumes. Specifically, first calibrate with a standard substance of known molecular weight, and draw a standard curve between elution volume and molecular weight. When an unknown sample enters the chromatographic column, the current molecular weight of the sample can be calculated by measuring the elution volume and comparing it with the standard curve. By recording the size and distribution of the molecular weight at each moment, the polymer dispersibility index PDI can be calculated.

[0097] In a second aspect of the present application, the present application provides a method for preparing a polymer, comprising: adding a monomer and an initiator to a solvent, and performing a heating treatment to obtain a polymer, wherein the monomer comprises an alkane substituted with a sulfone group containing an unsaturated bond, and the alkane comprises a substituted or unsubstituted C 1 -C 4 The alkane, the unsaturated bond includes at least one of a double bond and a triple bond. The above preparation method can be used to easily obtain a polymer that can effectively improve the ionic conductivity of the gel polymer electrolyte.

[0098] As an example, a monomer is a small molecule that can be linked to other molecules of the same or other species through covalent bonds to form a polymer.

[0099] As an example, substituted or unsubstituted C 1 -C 4 The alkane may include at least one of substituted or unsubstituted methane, substituted or unsubstituted ethane, substituted or unsubstituted n-propane, substituted or unsubstituted isopropane, substituted or unsubstituted n-butane, substituted or unsubstituted sec-butane, substituted or unsubstituted isobutane, and substituted or unsubstituted tert-butane.

[0100] According to an embodiment of the present application, the alkane includes at least two sulfone groups, and the number of carbon atoms between adjacent sulfone substituents is less than or equal to 4.

[0101] As an example, an alkane may include two sulfone substituents. When the alkane is a substituted or unsubstituted C 1 -C 4 When the alkane is an alkane, the number of carbon atoms between adjacent sulfone groups can be 1, 2, 3 or 4.

[0102] As an example, the monomer may include at least one of bis(vinylsulfone)methane, bis(vinylsulfone)ethane, 1,3-bis(vinylsulfone)-2-propanol, 2,2'-[methylenebissulfonyl]diethanol, 1,4-bis(vinylsulfonyl)butane, vinyl sulfone, bis(vinylsulfone)propane, 2,2'-sulfonyldiethanol, 1,3'-bis(chloroethylsulfone)propanol, and 1,3'-bis(hydroxyethylsulfone)propanol.

[0103] In some embodiments, the alkane further comprises an ether bond, and the number of carbon atoms between the oxygen atom of the ether bond and the sulfur atom of the adjacent sulfone group is less than or equal to 4.

[0104] As an example, the number of carbon atoms separating the oxygen atom of the ether bond and the sulfur atom of the adjacent sulfone group may be 1, 2, 3 or 4.

[0105] As an example, an alkane containing an ether bond may include an alkoxy group.

[0106] In some embodiments, the initiator may include at least one of azobisisoheptanenitrile, 2,2″-azabis(2-imidazoline) dihydrochloride, 2,2′-azobisisobutylamidine dihydrochloride, benzoyl peroxide, tert-butyl benzoyl peroxide, and methyl ethyl ketone peroxide.

[0107] Initiators, also known as free radical initiators, are a class of compounds that are easily decomposed into free radicals (i.e., primary free radicals) by heat. They can be used to initiate free radical polymerization and copolymerization reactions of olefin and diene monomers, and can also be used for cross-linking and curing of unsaturated polyesters and polymer cross-linking reactions.

[0108] As an example, the temperature of the heat treatment may be 40° C.-80° C. For example, the temperature of the heat treatment may be 40° C., 45° C., 50° C., 55° C., 60° C., 65° C., 70° C., 75° C., or 80° C.

[0109] As an example, the solvent for the polymerization reaction may include tetrahydrofuran (THF).

[0110] In some specific embodiments, the polymer of formula I-1 can be prepared by referring to the route of reaction formula I-1:

[0111]

[0112] Specifically, bis(vinylsulfone)methane and azobisisobutyronitrile (AIBN) were placed in a single-mouth bottle, the single-mouth bottle was placed in liquid nitrogen to solidify the reactants, and vacuum was evacuated for a period of time, then the reactants were melted and filled with argon, and this was repeated several times, and finally the reactants were heated and stirred at 70°C for a period of time. After the reaction was completed, the product was added dropwise to n-hexane for precipitation, and a solid precipitate appeared, which was filtered to obtain a solid product, namely polymer I-1.

[0113] In some specific embodiments, the polymer of formula I-2 can be prepared by referring to the route of reaction formula I-2:

[0114]

[0115] Reaction formula I-2,

[0116] Specifically, sodium hydride and anhydrous THF are placed in a three-necked flask, and argon is used for protection. The reactant is cooled to 0°C, and a tetrahydrofuran solution of 2,2'-[methylenebissulfonyl]diethanol is added dropwise. After the addition is complete, the reaction is stirred at 0°C, and the tetrahydrofuran solution of 2,2'-[methylenebissulfonyl]diethanol is added dropwise again. After the addition is complete, the temperature is restored to room temperature and stirred, and finally the reactant is stirred at 70°C for a period of time. After the reaction is completed, the THF is removed by concentration under reduced pressure, and the product is then added dropwise to n-hexane for precipitation. A solid precipitate appears, and a solid product is obtained by suction filtration, which is polymer I-2.

[0117] In some specific embodiments, the polymer of formula I-5 can be prepared by referring to the route of reaction formula I-5:

[0118]

[0119] It should be noted that the relevant parameters in the above-mentioned method for preparing a polymer can refer to part or all of the technical features in the aforementioned embodiments. The parts not described in the relevant embodiments of the method for preparing a polymer can also refer to the aforementioned embodiments and related drawings, which will not be repeated here.

[0120] The above description of various embodiments tends to emphasize the differences between the various embodiments. The same or similar aspects can be referenced to each other, and for the sake of brevity, they will not be repeated herein.

[0121] In the third aspect of the present application, the present application proposes a gel polymer electrolyte, comprising a polymer matrix, the polymer matrix comprising the aforementioned polymer; and / or a polymer prepared by the aforementioned method. Therefore, the gel polymer electrolyte has all the characteristics and advantages of the aforementioned polymer and the aforementioned method, which will not be repeated here.

[0122] In some embodiments, the electrolyte includes a plasticizer and a metal salt, and the plasticizer includes a sulfone plasticizer.

[0123] As an example, the plasticizer can be a liquid plasticizer. The conduction of metal active ions in the gel polymer electrolyte is mainly conducted in the liquid plasticizer, and the liquid plasticizer can act as a solvent in the electrolyte, thereby helping to improve the ionic conductivity of the gel polymer electrolyte.

[0124] As an example, sulfone plasticizers contain sulfone groups, which can coordinate with metal active ions. The metal active ions can be transferred between adjacent sulfone groups of the plasticizer, and can also be transferred between the sulfone groups of the plasticizer and the sulfone groups of the polymer matrix, thereby effectively improving the transfer rate of the metal active ions.

[0125] In some embodiments, the sulfone plasticizer may include at least one of sulfolane, dimethyl sulfone, ethyl methyl sulfone, ethyl isopropyl sulfone, and 3-methylcyclosulfone.

[0126] As an example, sulfone plasticizers such as sulfolane (SL), dimethyl sulfone (DMS), ethyl methyl sulfone (EMS), ethyl isopropyl sulfone (EiPS), and 3-methylcyclosulfone (MSL) can provide more sulfone groups to the electrolyte and enhance the transfer effect of metal active ions.

[0127] In some embodiments, the sulfone plasticizer may include sulfolane. Sulfolane has a higher solubility of metal salts and a higher oxidative stability. In addition, the conformation of sulfolane is relatively limited. Compared with chain-structured sulfone plasticizers such as ethyl methyl sulfone, sulfolane has a faster Li + The ligand exchange rate can effectively improve the cycle performance and rate performance of the battery.

[0128] Conformation refers to different temporary and changeable spatial structural forms formed by the free rotation of a certain atom (group) in a molecule around the CC single bond. Different conformations can transform into each other. Among various conformational forms, the one with the lowest potential energy and the most stable one is the dominant one.

[0129] In some embodiments, the mass fraction of the polymer matrix in the gel polymer electrolyte is 10%-80%.

[0130] As an example, the mass fraction of the polymer matrix in the gel polymer electrolyte can be 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80%.

[0131] When the mass fraction of the polymer matrix in the gel polymer electrolyte is 10%-80%, the mechanical strength of the gel polymer electrolyte is better, which can reduce the occurrence of explosion when encountering abnormal usage conditions such as impact, crushing and puncture; the gel polymer electrolyte has good bendability and stretchability and can be used to prepare batteries of various shapes, such as flexible batteries.

[0132] In some embodiments, the mass fraction of the plasticizer in the gel polymer electrolyte is 20%-60%.

[0133] As an example, the mass fraction of the plasticizer in the gel polymer electrolyte may be 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55% or 60%.

[0134] When the mass fraction of the plasticizer in the gel polymer electrolyte is less than 20%, the content of metal salt that can be dissolved in the gel polymer electrolyte is too small, resulting in a significant decrease in the migration number of metal active ions, and the efficiency of the electrolyte in transferring charges between the positive electrode plate 10 and the negative electrode plate 20 is low, which in turn causes excessive anions to accumulate on the surface of the positive electrode plate 10, generating a concentration gradient between the positive electrode plate 10 and the negative electrode plate 20, causing concentration polarization in the ion battery, resulting in a large overpotential, limiting the improvement of the battery's energy density and power density; when the mass fraction of the plasticizer in the gel polymer electrolyte is greater than 60%, the amount of metal salt added to the gel polymer electrolyte needs to be reduced accordingly, resulting in an excessive amount of plasticizer, and the plasticizer cannot provide capacity during the battery's charge and discharge cycle, thereby reducing the battery's volume energy density.

[0135] In some embodiments, the mass fraction of the metal salt in the gel polymer electrolyte is 5%-30%.

[0136] As an example, the mass fraction of the metal salt in the gel polymer electrolyte may be 5%, 8%, 10%, 15%, 20%, 25% or 30%.

[0137] As an example, the metal salt in the electrolyte may include a lithium salt, and the lithium salt may include at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorophosphate, lithium difluorobis(oxalatophosphate) and lithium tetrafluorooxalatophosphate.

[0138] In the fourth aspect of the present application, the present application proposes a battery, including the aforementioned gel polymer electrolyte. As a result, the battery has all the characteristics and advantages of the aforementioned gel polymer electrolyte, and the battery has better rate performance and low-temperature cycle performance. Generally, the battery includes a positive electrode sheet 10, a negative electrode sheet 20, an electrolyte and a separator 30, and the electrolyte may include the aforementioned gel polymer electrolyte 40. During the battery charge and discharge process, active ions are embedded and removed back and forth between the positive electrode sheet 10 and the negative electrode sheet 20. The electrolyte plays the role of conducting ions between the positive electrode sheet 10 and the negative electrode sheet 20. The separator 30 is arranged between the positive electrode sheet 10 and the negative electrode sheet 20, mainly to prevent the positive electrode sheet and the negative electrode sheet from short-circuiting, while allowing ions to pass through.

[0139] In the embodiment of the present application, the battery 5 may be a metal battery.

[0140] As an example, the battery 5 may be a sodium metal battery, a lithium metal battery, or the like.

[0141] In some embodiments, reference Figure 3The electrode assembly 52 may be a wound structure. The positive electrode sheet 10 and the negative electrode sheet 20 are wound to form a wound structure.

[0142] In some embodiments, the electrode assembly 52 is a laminate structure.

[0143] As an example, a plurality of positive electrode sheets 10 and a plurality of negative electrode sheets 20 may be provided respectively, and the plurality of positive electrode sheets 10 and the plurality of negative electrode sheets 20 may be alternately stacked.

[0144] As an example, a plurality of positive electrode sheets 10 may be provided, and the negative electrode sheet 20 may be folded to form a plurality of stacked folded segments, with one positive electrode sheet 10 being sandwiched between adjacent folded segments.

[0145] As an example, the positive electrode sheet 10 and the negative electrode sheet 20 are both folded to form a plurality of stacked folded sections.

[0146] In some embodiments, the isolation film 30 is disposed between the positive electrode sheet 10 and the negative electrode sheet 20 , and mainly serves to prevent the positive electrode sheet and the negative electrode sheet from short-circuiting, while allowing ions to pass through.

[0147] As an example, a plurality of separators 30 may be provided, each of which is provided between any adjacent positive electrode sheets 10 or negative electrode sheets 20 .

[0148] As an example, the separator 30 may be disposed continuously, and disposed between any adjacent positive electrode sheets 10 or negative electrode sheets 20 by folding or winding.

[0149] In some embodiments, the shape of the electrode assembly can be cylindrical, flat, or polygonal.

[0150] In some embodiments, the electrode assembly is provided with tabs, which can lead current out of the electrode assembly. The tabs include a positive tab and a negative tab.

[0151] In some embodiments, the positive electrode sheet 10 may include a positive electrode current collector 11 and a positive electrode active material layer 12 disposed on at least one side of the positive electrode current collector 11 .

[0152] As an example, the positive electrode current collector 11 has two surfaces facing each other in its thickness direction, and the positive electrode active material layer 12 is provided on either or both of the two facing surfaces of the positive electrode current collector 11 .

[0153] As an example, the positive electrode current collector 11 can be made of metal foil, foam metal or composite current collector. For example, as the metal foil, aluminum or stainless steel, stainless steel, copper, aluminum, nickel, carbon electrode, carbon, nickel or titanium with silver surface treatment can be used. The composite current collector may include a polymer material base and a metal layer. The foam metal may be foam nickel, foam copper, foam aluminum, foam alloy, or foam carbon. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyethylene, etc.).

[0154] As an example, the positive electrode active material layer may include at least one of optionally doped lithium cobalt oxide, optionally doped lithium manganese oxide, optionally doped nickel-cobalt ternary material, and optionally doped lithium iron phosphate.

[0155] In some embodiments, the negative electrode plate 20 may include a negative electrode current collector 21, and the negative electrode current collector 21 may be a metal foil, a foam metal, or a composite current collector. For example, as the metal foil, aluminum or stainless steel treated with silver, stainless steel, copper, aluminum, nickel, carbon electrode, carbon, nickel or titanium, etc. may be used. The foam metal may be foam nickel, foam copper, foam aluminum, foam alloy, or foam carbon, etc. The composite current collector may include a polymer material base layer and a metal layer, and the composite current collector may be formed by placing a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyethylene, etc.).

[0156] In some embodiments, the negative electrode plate 20 may be a rolled metal foil or a surface-coated inert layer of metal powder coated on a current collector.

[0157] In some embodiments, the negative electrode current collector 21 may be a composite current collector, for example, the composite current collector may include at least one of carbon cloth, carbon film, carbonaceous material, porous current collector, alloyed modified current collector, lithium-philic modified current collector and sodium-philic modified current collector.

[0158] As an example, the silicon-based material may include at least one of simple silicon, silicon oxide, silicon carbon compound, silicon nitrogen compound, and silicon alloy material. The tin-based material may include at least one of simple tin, tin oxide, and tin alloy material.

[0159] The present application has no particular limitation on the type of the isolation membrane 30 , and any porous isolation membrane with good chemical stability and mechanical stability may be selected.

[0160] As an example, the main material of the separator 30 may include at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, ceramic and polyvinylidene fluoride. The number of layers of the separator 30 is not particularly limited, and the separator 30 may be a single-layer film or a multi-layer composite film. When the separator 30 is a multi-layer composite film, the materials of each layer are not particularly limited, and the materials of each layer may be the same or different. The separator 30 may be a separate component located between the positive electrode sheet 10 and the negative electrode sheet 20, or it may be attached to the surface of the positive electrode sheet and / or the negative electrode sheet.

[0161] As an example, the present application has no particular limitation on the shape of the battery, which may be cylindrical, square, or any other shape. Figure 2 The square structure battery 5 is used as an example. Figure 3 The outer package of the battery 5 may include a shell 51 and a top cover assembly 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the top cover assembly 53 can be covered on the opening to close the receiving cavity.

[0162] As an example, the positive electrode sheet 10, the negative electrode sheet 20 and the separator 30 can be wound or laminated to form an electrode assembly 52. ​​The electrode assembly 52 is encapsulated in the receiving cavity, and the gel polymer electrolyte impregnates the electrode assembly 52. ​​The number of electrode assemblies 52 included in the battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0163] As an example, batteries may be assembled into a battery module. The number of batteries contained in the battery module may be one or more. The specific number may be selected by those skilled in the art according to the application and capacity of the battery module. Figure 4 4 is an example of a battery module. Figure 4 In the battery module 4, the multiple batteries 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. The multiple batteries 5 may further be fixed by fasteners. The battery module 4 may also include a housing having a storage space, and the multiple batteries 5 are stored in the storage space.

[0164] As an example, the above-mentioned battery modules can also be assembled into a battery pack. The number of battery modules contained in the battery pack can be one or more, and the specific number can be selected by those skilled in the art according to the application and capacity of the battery pack. Figure 5 and Figure 6 1 is a battery pack 1 as an example. Figure 5 and Figure 6The battery pack 1 may include a battery box and a plurality of battery modules 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 can be arranged in the battery box in any manner.

[0165] In the fifth aspect of the present application, the present application proposes an electrical device, comprising the aforementioned gel polymer electrolyte and / or the aforementioned battery. Therefore, the electrical device has all the features and advantages of the aforementioned gel polymer electrolyte and battery, which will not be described in detail here.

[0166] Batteries, battery modules, or battery packs can be used as power sources for electrical devices, or as energy storage units for electrical devices. Electrical devices may include mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto. Electrical devices may select batteries, battery modules, or battery packs according to their usage requirements.

[0167] As an example, Figure 7 The power consumption device is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the high power and high energy density requirements of the power consumption device for the battery, a battery pack or a battery module can be used.

[0168] As an example, the power-consuming device may also be a mobile phone, a tablet computer, a laptop computer, etc. Such a device is usually required to be light and thin, and a battery may be used as a power source.

[0169] The scheme of the present application is described below by specific examples. It should be noted that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If no specific technology or conditions are specified in the examples, the technology or conditions described in the literature in this area or the product instructions are used. The reagents or instruments used are not specified by the manufacturer, and are all conventional products that can be obtained commercially.

[0170] Example 1

[0171] The polymer shown in the synthetic formula Ⅰ-1 is:

[0172] Take 1.5g of bis(vinylsulfone)methane and 32mg of azobisisobutyronitrile (AIBN) 25mL and place them in a single-mouth bottle, place the single-mouth bottle in liquid nitrogen to solidify the reactant, and use an oil pump to evacuate to maintain vacuum for 10 minutes, then melt the reactant and fill it with argon, repeat this 4 times, finally place the single-mouth bottle in an oil bath, and heat and stir the reactant at 70°C for 20h. After the reaction is completed, add the product dropwise to 20mL of n-hexane for precipitation, and solid precipitate appears, which is filtered to obtain a solid product, namely polymer I-1.

[0173] The polymerization reaction is shown in reaction formula I-1.

[0174]

[0175] Preparation of positive electrode:

[0176] The positive electrode active material lithium nickel cobalt manganese oxide (NMC), the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 98:1:1, and the solvent N-methylpyrrolidone (NMP) was added and stirred until the system was uniform to obtain a positive electrode slurry; the positive electrode slurry was evenly coated on both sides of the positive electrode current collector aluminum foil, dried at room temperature, transferred to an oven for further drying, and then cut into 40mm×50mm rectangles as positive electrode sheets. The surface capacity of the positive electrode sheet is 3.5mAh / cm 2 .

[0177] Preparation of negative electrode sheet:

[0178] A 50 μm lithium foil was rolled onto a 12 μm copper foil and then cut into a 41 mm×51 mm rectangle for use as a negative electrode.

[0179] Preparation of gel polymer electrolyte:

[0180] Weigh 10g of the aforementioned polymer accurately, dissolve it in 150ml of acetonitrile solvent, and heat and stir for 24h to fully disperse and dissolve the polymer, then cast it on a glass plate, and transfer it to a vacuum drying oven at 120℃, keep it for 24h, and after the solvent is completely volatilized, cool it down, take it out, and cut it into a 43mm×53mm rectangular polymer matrix film. Then soak the cut polymer matrix film in 10mL of 4M lithium bis(fluorosulfonyl)imide sulfolane (SL) solution, fully swell it, and obtain a gel polymer electrolyte membrane.

[0181] Battery assembly: Take a cut positive electrode sheet and match it with two cut negative electrode sheets. Set the above-mentioned gel polymer electrolyte membrane between the positive electrode sheet and the negative electrode sheet to isolate the positive electrode sheet and the negative electrode sheet, and wrap them in an aluminum-plastic film bag to form a stacked battery cell. The aluminum-plastic film bag is vacuum hot-pressed and sealed. After standing at room temperature for at least 6 hours, the cycle test can be started. The rated capacity of the stacked battery is 140mAh.

[0182] Example 2

[0183] Example 2 is consistent with Example 1, except that a polymer shown in Formula Ⅰ-5 is synthesized and used as a polymer matrix, wherein bis(vinylsulfone)methane is replaced by bis(vinylsulfone)ethane when synthesizing the polymer.

[0184] The polymerization reaction is shown in reaction formula I-5.

[0185]

[0186] Example 3

[0187] Example 3 is consistent with Example 1, except that a polymer shown in Formula Ⅰ-29 is synthesized and used as a polymer matrix, wherein bis(vinylsulfone)methane is replaced by 1,4-bis(vinylsulfonyl)butane (CAS: 3088-17-3) when synthesizing the polymer.

[0188] Example 4

[0189] Example 4 is consistent with Example 1, except that the polymer shown in Formula I-2 is synthesized and used as the polymer matrix. Specifically, 0.172g of sodium hydride (NaH, 60%) and 20mL of anhydrous THF are placed in a 50mL three-necked flask, protected by argon, and the reactant is cooled to 0°C in an ice-water bath, and 1.0g of 2,2'-[methylenebissulfonyl]diethanol in tetrahydrofuran (5mL) solution is added dropwise, and the reaction is stirred at 0°C for 1h after the addition is complete, and 1.0g of 2,2'-[methylenebissulfonyl]diethanol in tetrahydrofuran (5mL) solution is added dropwise again, and the reaction is stirred at room temperature for 1h after the addition is complete, and finally the three-necked flask is placed in an oil bath pot to react and stir the reactant at 70°C for 10h. After the reaction is completed, the THF is removed by concentration under reduced pressure, and the product is then added dropwise to 20mL of n-hexane for precipitation, and a solid precipitate appears, which is filtered to obtain a solid product, namely polymer I-2.

[0190] The polymerization reaction is shown in reaction formula I-2.

[0191]

[0192] Reaction formula I-2.

[0193] Example 5

[0194] Example 5 is consistent with Example 1, except that dimethyl sulfone (DMS) is used as a plasticizer.

[0195] Example 6

[0196] Example 6 is consistent with Example 1, except that ethyl methyl sulfone (EMS) is used as a plasticizer.

[0197] Example 7

[0198] Example 7 is consistent with Example 1, except that ethyl isopropyl sulfone (EiPS) is used as a plasticizer.

[0199] Comparative Example 1

[0200] Comparative Example 1 is consistent with Example 1, except that the structure of the polymer is as follows:

[0201] The CAS number is 25608-63-3 and the manufacturer is McLean.

[0202] Comparative Example 2

[0203] Comparative Example 2 is consistent with Example 1, except that the structure of the polymer is as follows:

[0204] The CAS number is 25135-51-7 and the manufacturer is McLean.

[0205] The ionic conductivity of the gel polymer electrolytes in Examples 1-7 and Comparative Examples 1-2 was tested, and the test results are shown in Table 1:

[0206] Test method for ionic conductivity: The AC impedance method is used for testing. Specifically, a gel polymer electrolyte with a diameter of 1.6 cm is placed in a stainless steel fixture to construct a blocking cell with a stainless steel / gel polymer electrolyte / stainless steel structure. The impedance of the blocking cell is measured using an electrochemical workstation, using the formula: σ = L / SR b The ionic conductivity of the gel polymer electrolyte was calculated, where σ is the ionic conductivity of the gel polymer electrolyte, L is the thickness of the gel polymer electrolyte, S is the area of ​​the gel polymer electrolyte, and R b is the impedance of the gel polymer electrolyte at room temperature

[0207] The cycle performance, low temperature cycle performance and rate performance of the batteries in Examples 1-7 and Comparative Examples 1-2 were tested. The test results are shown in Table 1:

[0208] Cycle performance test method: The ambient temperature is set at 25°C, and the charge and discharge cycles are performed using a charge rate of 0.5C (i.e. 70mA) and a discharge rate of 0.5C (i.e. 70mA). The charge cut-off voltage is set at 4.3V, and the discharge cut-off voltage is set at 2.8V. When the discharge capacity decays to 80% of the first cycle discharge capacity, the battery life is considered to be terminated, and the number of cycles at this time is recorded.

[0209] Test method for rate performance: The ambient temperature is set to 25°C, and three cycles of charge and discharge are performed using a charge rate of 0.2C (i.e. 28mA) and a discharge rate of 0.5C (i.e. 70mA). The charge cut-off voltage is set to 4.3V, and the discharge cut-off voltage is set to 2.8V. Then, while keeping the charge rate at 0.2C unchanged, increase the discharge rate to 4C, and after the cycle is stable, record the discharge capacity under the 4C high rate condition.

[0210] Test method for low temperature cycle performance: Set the ambient temperature to -30℃ (for example, place the battery in a low temperature oven), use a charge rate of 0.2C (i.e. 28mA) and a discharge rate of 0.2C (i.e. 28mA) for charge and discharge cycles. Set the charge cutoff voltage to 4.3V and the discharge cutoff voltage to 2.8V. After the cycle is stable, record the discharge capacity at low temperature of -30℃.

[0211] Table 1

[0212]

[0213]

[0214] In Example 1, 1.23 g of solid product was obtained, and the product yield was 82%. In Example 4, 0.94 g of solid product was obtained, and the product yield was 47%.

[0215] The polymer in Example 1 was subjected to elemental analysis, and the calculated values ​​were: C, 30.29; H, 5.08; O, 32.28; S, 32.35. The tested values ​​were: C, 31.02; H, 5.21; O, 31.58; S, 32.19. The obtained polymer was subjected to a number average molecular weight test, and the measured number average molecular weight was 38,000, and the polymer dispersity index was 1.9.

[0216] The polymer in Example 2 was subjected to elemental analysis, and the calculated values ​​were: C, 33.95; H, 5.70; O, 30.15; S, 30.21. The tested values ​​were: C, 33.65; H, 5.98; O, 31.45; S, 28.92. The obtained polymer was subjected to a number average molecular weight test, and the measured number average molecular weight was 35,000, and the polymer dispersity index was 1.7.

[0217] The polymer in Example 4 was subjected to elemental analysis, and the calculated values ​​were: C, 28.03; H, 4.70; O, 37.34; S, 29.93. The measured values ​​were: C, 29.02; H, 4.51; O, 38.58; S, 27.89. The obtained polymer was subjected to a number average molecular weight test, and the measured number average molecular weight was 31000, and the polymer dispersity index was 2.0.

[0218] In the description of this specification, the description of reference terms "one embodiment", "another embodiment", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment are included in at least one embodiment of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art can combine and combine different embodiments or examples described in this specification and the features of different embodiments or examples without contradiction.

[0219] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.

Claims

1. A polymer, characterized in that The general formula of the polymer is shown in formula (1): Wherein, R1 includes a substituted or unsubstituted C1-C4 alkyl group, R2 and R3 each independently include an alkyl group and / or an alkoxy group having a carbon number less than or equal to 3, and the value of n is 200-1000.

2. The polymer according to claim 1, characterized in that The number of carbon atoms between adjacent sulfone groups is less than or equal to 4. Optionally, the number of carbon atoms between adjacent sulfone groups is 1 or 2.

3. The polymer according to claim 1, characterized in that The content of sulfone groups in the polymer is 20%-80%. Optionally, the content of sulfone groups in the polymer is 60%-80%.

4. The polymer according to any one of claims 1 to 3, characterized in that The carbon atom of the alkoxy group is bonded to the sulfur atom of the sulfone group.

5. The polymer according to any one of claims 1 to 4, characterized in that The number of carbon atoms between the oxygen atom of the alkoxy group and the sulfur atom of the adjacent sulfone group is less than or equal to 4. Optionally, the number of carbon atoms between the oxygen atom of the alkoxy group and the sulfur atom of the adjacent sulfone group is 1 or 2.

6. The polymer according to claim 1, characterized in that The polymer comprises at least one of the following:

7. The polymer according to any one of claims 1 to 6, characterized in that The number average molecular weight of the polymer is 40,000-80,000. Optionally, the number average molecular weight of the polymer is 55,000-65,000.

8. The polymer according to any one of claims 1 to 7, characterized in that The polymer has a polymer dispersibility index of 1.5-2.5, and optionally, the polymer has a polymer dispersibility index of 1.7-2.

2.

9. A method for preparing a polymer, characterized in that: include: The monomer and the initiator are added to a solvent and subjected to a heating treatment to obtain the polymer. The monomer includes an alkane substituted with a sulfone group containing an unsaturated bond, the alkane includes a substituted or unsubstituted C1-C4 alkane, and the unsaturated bond includes at least one of a double bond and a triple bond.

10. The method according to claim 9, characterized in that The alkane includes at least two sulfone groups, and the number of carbon atoms between adjacent sulfone substituents is less than or equal to 4.

11. The method according to claim 9 or 10, characterized in that: The alkane further comprises an ether bond, and the number of carbon atoms between the oxygen atom of the ether bond and the sulfur atom of the adjacent sulfone group is less than or equal to 4.

12. The method according to any one of claims 9 to 11, characterized in that: The initiator includes at least one of azobisisoheptanenitrile, 2,2″-azabis(2-imidazoline) dihydrochloride, 2,2′-azobisisobutylamidine dihydrochloride, benzoyl peroxide, tert-butyl benzoyl peroxide, and methyl ethyl ketone peroxide.

13. A gel polymer electrolyte, characterized in that: The invention comprises a polymer matrix and an electrolyte, wherein the polymer matrix comprises the polymer described in any one of claims 1 to 8; and / or a polymer prepared by the method described in any one of claims 9 to 12.

14. The gel polymer electrolyte according to claim 13, characterized in that: The electrolyte includes a plasticizer and a metal salt, and the plasticizer includes a sulfone plasticizer.

15. The gel polymer electrolyte according to claim 14, characterized in that: The sulfone plasticizer includes at least one of sulfolane, dimethyl sulfone, ethyl methyl sulfone, ethyl isopropyl sulfone and 3-methylcyclic sulfone; preferably, the sulfone plasticizer includes sulfolane.

16. The gel polymer electrolyte according to claim 14 or 15, characterized in that: The mass fraction of the polymer matrix in the gel polymer electrolyte is 10%-80%.

17. The gel polymer electrolyte according to any one of claims 14 to 16, characterized in that: The mass fraction of the plasticizer in the gel polymer electrolyte is 20%-60%.

18. The gel polymer electrolyte according to any one of claims 14 to 16, characterized in that: The mass fraction of the metal salt in the gel polymer electrolyte is 5%-30%.

19. A battery, characterized in that: The invention comprises the gel polymer electrolyte according to any one of claims 13 to 18.

20. An electrical device, characterized in that: Comprising the gel polymer electrolyte according to any one of claims 13 to 18, and / or the battery according to claim 19.

Citation Information

Patent Citations

  • Michael addition curing chemistries for sulfur-containing polymer compositions employing bis(sulfonyl)alkanols

    CN105431411A

  • Aliphatic polysulfone, synthetic method, application and aliphatic polysulfone-based solid electrolyte

    CN114854019A

  • Vinyl sulphone-group-containing polymers

    GB1012791A

  • Nonaqueous electrolyte secondary battery

    JP2017174740A

  • Aliphatic polysulfones with improved mechanical integrity

    US20190144611A1

Cited By

  • Stable flame-retardant gel polymer for electrolyte

    CN119875129A

  • Solid polymer electrolyte as well as preparation method and application thereof