Preparation of IL (at) MOF composite material simulating novel rapid transfer system and application of IL (at) MOF composite material in carbon capture

By using IL@ZIF-8 composite material as a filler in the mixed matrix membrane, the problem of CO2 separation in natural gas is solved, efficient CO2 transfer and selective separation are achieved, the problem of CO2 separation in natural gas is solved, and the quality of natural gas is improved. and economical.

CN118767706APending Publication Date: 2024-10-15SHIHEZI UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410925251.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing technology is difficult to effectively and economically separate CO2 from natural gas, leading to pipeline corrosion and reduced calorific value, affecting the quality and sales price of natural gas.

Method used

The IL@MOF composite material IL@ZIF-8, which imitates a new rapid delivery system, is used as a filler to form a mixed matrix film with the self-polymerized constrained Pebax/PEG-MEA base material, using the self-adhesive properties of ionic liquids and Zn2+ carrier promotion The rapid transfer of CO2 forms an efficient CO2/CH4 mixed gas separation system.

Benefits of technology

Efficient transfer and selective separation of CO2 are achieved, with a maximum CO2 flux of 807.8±8 Barrer and a CO2/CH4 selectivity of 17.5±0.2. This simplifies the preparation process, reduces costs, and improves the gas separation performance of the membrane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004937940270000011
    Figure HDA0004937940270000011
  • Figure HDA0004937940270000012
    Figure HDA0004937940270000012
  • Figure HDA0004937940270000021
    Figure HDA0004937940270000021
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of mixed matrix membrane materials, in particular to preparation of an IL (at) MOF composite material simulating a novel rapid transfer system and application of the IL (at) MOF composite material in carbon capture. The invention provides a preparation method of an IL (at) MOF composite material simulating a novel rapid transfer system. The prepared IL (at) ZIF-8 is taken as a filling agent and is physically blended with auto-polymerization constrained Pebax / PEG-MEA (SPM) to form a mixed matrix membrane. The SPM / IL-coated ZIF-8 mixed matrix membrane prepared by the method has the advantages of simple preparation process, controllable reaction, cheap and easily available raw materials and mild conditions, and can powerfully promote advantage complementation of a metal organic framework and a polymer matrix. By utilizing the inherent characteristic of self-bonding of the ionic liquid, the ZIF-8 is effectively connected through the ionic liquid, so that the IL (at) ZIF-8 can play a role in simulating a novel rapid transfer system. Wherein CO2 can be quickly transferred from the ZIF-8 to the adjacent ZIF-8, which is mainly benefited from the'conveyor belt effect 'of the CO2 carrier ([Tf2N]-) of the ionic liquid itself, and effectively provides a continuous CO2 transfer path between MOF regions. In addition, a Zn < 2 + > carrier in an IL (at) ZIF-8 directional ordered pore channel can promote rapid transfer of CO2 in multiple directions. The prepared mixed matrix membrane has an efficient imitated novel rapid transfer system, and the transfer of CO2 in the membrane can be enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mixed matrix membrane material preparation, and in particular to the preparation of an IL@MOF composite material imitating a novel rapid transmission system and its application in carbon capture. Background Art

[0002] The global energy demand is mainly met by burning fossil fuels such as coal, oil, and natural gas. The excessive consumption of non-renewable fossil fuels has caused serious energy crises and environmental problems, while the excessive emission of greenhouse gases has led to an increasingly serious global warming problem. It is a consensus in the mainstream scientific community that greenhouse gas emissions bring about global climate change. Global climate change has led to rising sea levels, frequent extreme weather disasters on the earth, and serious impact on biodiversity. Global climate change has brought serious adverse effects on human society. It is generally believed internationally that greenhouse gas emissions have serious negative impacts on the environment (such as global warming) and the sustainable development of the economy. Among greenhouse gases, carbon dioxide is the most abundant, accounting for 75% of global greenhouse gases. Large-scale emissions of carbon dioxide have led to serious environmental problems such as global warming, ocean acidification, extreme weather and species extinction. Extensive and profound economic and social systemic changes require the successful transformation of the economic system, energy system, and technological system of the whole society, which requires a green and low-carbon lifestyle. CCUS (Carbon Capture Utilization Storage), that is, carbon capture, utilization and storage, is one of the key technologies to address global climate change and has received widespread attention from the whole society. Therefore, reducing emissions and lowering atmospheric CO2 concentrations are urgent tasks that need to be given high priority. Since fossil fuels will remain the main energy source for the foreseeable future, the most direct strategy to reduce anthropogenic CO2 emissions is to eliminate CO2 at the source. Therefore, in order to alleviate the sharply increasing global energy demand and environmental problems, there is a high demand for sustainable energy storage technologies.

[0003] Natural gas (NG) can provide higher calorific value and lower CO2 emissions compared to other hydrocarbon fuels such as coal and oil. About 30% of the energy currently consumed worldwide is produced by natural gas, and in addition, a large part of natural gas is transported around the world in liquid form. Natural gas (NG) has become one of the most useful, cleanest and cheapest energy sources in the world. It is estimated that global natural gas consumption will increase at an average annual rate of 2.3% from 2002 to 2025. It is estimated that one-third of the proven natural gas reserves are acidic. In its raw form, it is mainly composed of methane (CH 4 ), different amounts of heavier gaseous hydrocarbons, acid gases, water vapor, mercury, radioactive gases and other gases. 2The content is about 20%, and NG needs further purification. Optimal separation of carbon dioxide from natural gas is necessary because it reduces the calorific value of combustion of natural gas and affects the sales price of natural gas. High carbon dioxide content in natural gas promotes the formation of carbonic acid and dry ice, and even worse, it can cause pipeline corrosion and increase the volume of gas transported by pipeline. Carbon dioxide concentrations above 2% or 3% will significantly reduce the BTU value (heat capacity) of the gas, making it economically unfeasible. Therefore, from an industrial perspective, in the natural gas industry (NG) for specific liquefied natural gas processing (LNG), industry standards require CO 2 The concentration is lower than 50ppm to solve the problem of CO 2 The presence of CO causes problems such as pipeline corrosion and reduced calorific value of natural gas. Therefore, CO is removed from natural gas through purification process. 2 It is essential to improve product quality. A prerequisite for achieving this goal is the adoption of low-cost and energy-efficient carbon capture and storage technology. Summary of the invention

[0004] In order to solve the problems existing in the prior art, the present invention provides a preparation of an IL@MOF composite material imitating a new rapid delivery system and its application in carbon capture. The IL@MOF composite material IL@ZIF-8 imitating a new rapid delivery system prepared by the present invention is used as a filler to construct an efficient new rapid delivery system in a mixed matrix membrane, thereby improving the gas separation performance and being used to separate CO 2 / CH 4 Mixed gases.

[0005] In order to achieve the above-mentioned invention object, the present invention adopts the following technical solutions:

[0006] In a specific embodiment, the present invention provides a method for preparing an IL@MOF composite material for a novel rapid delivery system, the method comprising the steps of:

[0007] (1) 1-Methylimidazole and 3-chloropropyltriethoxysilane in N 2 The mixture was heated under atmosphere and stirred under reflux. After the reaction, the obtained suspension was extracted with an appropriate amount of petroleum ether. The product was rotary evaporated to remove the remaining petroleum ether, and then further dried in a vacuum oven to obtain an ionic liquid intermediate.

[0008] (2) LiTf 2 N is dissolved in deionized water, and then the ionic liquid intermediate synthesized in step (1) is slowly added to the above solution, stirred at room temperature, and washed with deionized water. The resulting suspension is separated by a separatory funnel, then rotary evaporated, and dried in a vacuum oven to obtain IL.

[0009] (3) The IL prepared in step (2) was dispersed in acetone to obtain solution A, and Zn(NO 3 ) 2 6H 2 O and 2-Hmim were dissolved in solution A respectively and stirred thoroughly until the solution was clear and uniform. Then the IL solution containing Zn salt was added to the 2-Hmim solution and stirred continuously at room temperature. After the reaction was completed, the solution was collected by centrifugation and washed with acetone and an appropriate amount of methanol. Finally, it was dried in a vacuum oven to obtain IL@ZIF-8.

[0010] Furthermore, in step (1), the amount of 1-methylimidazole and 3-chloropropyltriethoxysilane used is in the ratio of (0.25 mol): (0.25 mol); the stirring temperature is 90-100° C., and the stirring time is 20 h to 24 h.

[0011] In step (2), LiTf 2 The dosage of N, ionic liquid intermediate and deionized water is 0.2 mol: 0.2 mol: 260 mL.

[0012] The solution A in step (3) is prepared by dispersing the IL prepared in step (2) in acetone, and the concentration thereof is 10 wt.%. The Zn(NO 3 ) 2 6H 2 The dosage relationship of O, 2-Hmim and acetone is 1.798g:4.000g:54g.

[0013] In a specific embodiment, the present invention also provides an IL@MOF composite material for a novel rapid delivery system prepared by the above-mentioned preparation method.

[0014] In a specific embodiment, the present invention also provides the application of the IL@MOF composite material imitating the novel rapid delivery system in carbon capture.

[0015] In a specific embodiment, the present invention also provides a mixed matrix membrane, wherein the mixed matrix membrane uses the IL@ZIF-8 composite material imitating the new rapid delivery system as a filler and the self-polymerization constrained Pebax / PEG-MEA (SPM) as a base material, and the filler and the base material are physically blended at room temperature to form the mixed matrix membrane; the thickness of the mixed matrix membrane is 160 to 187 μm; the mass percentage of the filler in the mixed matrix membrane is 1% to 7%.

[0016] Furthermore, the present invention also provides the mixed matrix membrane in CO 2 / CH 4 Application in the field of mixed gas separation.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] The present invention provides a method for preparing an IL@ZIF-8 composite material for a novel rapid delivery system, and the prepared IL@ZIF-8 is used as a filler and physically blended with an SPM matrix to form a mixed matrix membrane. The SPM / IL@ZIF-8 mixed matrix membrane prepared by the method of the present invention has a simple preparation process, controllable reaction, and cheap and readily available raw materials. By utilizing the inherent self-adhesive properties of ionic liquids, the ZIF-8 can be effectively connected through ionic liquids, so that IL@ZIF-8 can play the role of a novel rapid delivery system. Among them, CO 2 It can be quickly transferred from ZIF-8 to the adjacent ZIF-8, which is mainly due to the CO 2 Carrier ([Tf 2 N] - ) has a "conveyor belt effect" that effectively provides continuous CO between MOF regions. 2 In addition, Zn in the oriented and ordered channels of IL@ZIF-8 2+ The carrier can promote CO 2 Rapid transmission in multiple directions. The prepared mixed matrix membrane has a highly efficient novel rapid transmission system, which can enhance CO 2 Transport in membranes.

[0019] The present invention combines the advantages of IL and ZIF-8 fillers to achieve a synergistic effect; the preparation process of the mixed matrix membrane is simple, the reaction is controllable, the raw materials are cheap and readily available, and the conditions are mild, which can promote the complementary advantages of inorganic fillers and polymer matrices. 2 / CH 4 Permselectivity of mixed gases CO 2 The highest flux was 807.8±8Barrer, CO 2 / CH 4 The selectivity is 17.5±0.2. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:

[0021] Figure 1 This is a transmission electron microscope image of the IL@ZIF-8 material prepared in Example 1.

[0022] Figure 2 This is a scanning electron microscope cross-sectional image of the SPM / IL@ZIF-8(1) mixed matrix membrane prepared in Example 1.

[0023] Figure 3 This is a scanning electron microscope cross-sectional image of the SPM / IL@ZIF-8(3) mixed matrix membrane prepared in Example 2.

[0024] Figure 4 This is a scanning electron microscope cross-sectional image of the SPM / IL@ZIF-8(5) mixed matrix membrane prepared in Example 3.

[0025] Figure 5 This is a scanning electron microscope cross-sectional image of the SPM / IL@ZIF-8(7) mixed matrix membrane prepared in Example 4.

[0026] Figure 6 This is a scanning electron microscope cross-sectional image of the SPM film prepared in Comparative Example 1.

[0027] Figure 7 This is a scanning electron microscope cross-sectional image of the SPM / ZIF-8(5) mixed matrix membrane prepared in Comparative Example 2. DETAILED DESCRIPTION

[0028] The present invention will be further explained below. These examples are only used to illustrate the present invention and are not used to limit the scope of the present invention. Experimental methods without specific conditions in the examples are all based on conventional conditions. The reagents and materials used, unless otherwise specified, can be obtained from commercial channels.

[0029] Embodiment 1:

[0030] A SPM / IL@ZIF-8 (1) mixed matrix membrane was prepared. The thickness of the mixed matrix membrane was 166 μm. The mixed matrix membrane used SPM as a membrane matrix and IL@ZIF-8 was added to the membrane matrix. The mass ratio of SPM to IL@ZIF-8 was 0.99:0.01. The preparation method of the mixed matrix membrane was as follows:

[0031] Step 1: Preparation of IL@ZIF-8:

[0032] 1-Methylimidazole (0.25 mol) and 3-chloropropyltriethoxysilane (0.25 mol) were reacted at 95 °C in N 2 The mixture was heated under atmosphere and refluxed with stirring for 24 h. After the reaction, the obtained suspension was extracted with an appropriate amount of petroleum ether. The product was rotary evaporated to remove the remaining petroleum ether, and then further dried in a vacuum oven at 40 ° C for 12 h to prepare an ionic liquid intermediate. 2 N (0.2 mol) was dissolved in 260 mL of deionized water and stirred continuously. Then the synthesized ionic liquid intermediate (0.2 mol) was slowly added to the above solution, stirred at room temperature for 2 h, and washed with deionized water for more than 5 times. The obtained IL was separated by a separation funnel. Then the IL was rotary evaporated and dried in a vacuum oven at 60 ° C for 12 h. Zn(NO3 ) 2 6H 2 O (1.798 g) and 2-Hmim (4.000 g) were dissolved in 10 wt.% IL acetone solution (IL: 6 g, acetone: 54 g), and stirred until the two solutions were clear and uniform. Then the IL solution containing Zn salt was added to the 2-Hmim solution, and stirred continuously at room temperature for 24 h. After the reaction was completed, the mixture was collected by centrifugation and washed with 50 mL of acetone and an appropriate amount of methanol. Finally, it was dried in a vacuum oven at 60 ° C for 12 h to prepare IL@ZIF-8.

[0033] Step 2: Preparation of SPM solution:

[0034] Weigh 0.537g of 1657 particles and 0.358 g of PEG-MEA were dissolved in 10 ml of a mixed solution of ethanol and water (the mass ratio of ethanol to water was 70% / 30%), heated in a water bath at 80°C with stirring for 2 h to completely dissolve Pebax and PEG-MEA, and then added with 1 wt.% AIBN to room temperature to prepare a 6 wt.% SPM matrix solution for later use.

[0035] Step 3; Preparation of SPM / IL@ZIF-8 mixed matrix membrane:

[0036] The IL@ZIF-8 (0.009 g) prepared in Step 1 was physically blended with the 6 wt.% SPM solution prepared in Step 2, and stirred at room temperature for 4 h to obtain a casting solution, which was then poured onto a clean culture dish for casting. The mixture was dried at room temperature (25°C) for 48 h, and then vacuum dried at 40°C in a vacuum drying oven to remove the residual solvent on the surface of the mixed matrix membrane, and then thermally initiated at 80°C to fully polymerize the mixture to obtain a SPM / IL@ZIF-8 mixed matrix membrane with a membrane thickness of 166 μm. The weight percentage of IL@ZIF-8 in the SPM / IL@ZIF-8 mixed matrix membrane was 1%, so it was named SPM / IL@ZIF-8 (1) mixed matrix membrane.

[0037] Please refer to Figure 1 As shown: Ionic liquids have unique self-adhesive properties, acting as "adhesives" to cleverly "bond" the nanoparticles together, resulting in a relatively continuous distribution state of IL@ZIF-8. In addition, through mapping, it can be clearly observed that the F, S, and Si elements are evenly distributed on IL@ZIF-8, which indicates that IL not only acts as an "affinity layer" on the surface of ZIF-8 nanoparticles, but also acts as a "conveyor belt" between adjacent ZIF-8. This highly efficient imitation rapid transfer system can enhance CO 2 Transport in membranes.

[0038] Please refer to Figure 2 As shown in Figure 2, the SPM / IL@ZIF-8(1) mixed matrix membrane was used for CO 2 CO with a volume fraction of 20% 2 / CH 4 Mixed gas separation test, its CO 2 The flux is 629.39±6 Barrer, CO 2 / CH 4 The selectivity is 14.9±0.3.

[0039] Embodiment 2:

[0040] A SPM / IL@ZIF-8(3) mixed matrix membrane was prepared. The difference from the SPM / IL@ZIF-8(1) mixed matrix membrane in Example 1 is that the thickness of the obtained SPM / IL@ZIF-8(3) mixed matrix membrane is 177 μm, wherein the mass ratio of SPM to IL@ZIF-8 is 0.97:0.03. The preparation method of the mixed matrix membrane is different from that of Example 1 only in that in step 3, 0.027 g of IL@ZIF-8 is weighed instead of 0.009 g; finally, a mixed matrix membrane with a thickness of 177 μm is obtained.

[0041] Please refer to Figure 3 As shown: At 25 °C and 2 bar, the SPM / IL@ZIF-8(3) mixed matrix membrane prepared in Example 2 was used for CO 2 CO with a volume fraction of 20% 2 / CH 4 Mixed gas separation test, its CO 2 The flux is 685.9±3 Barrer, CO 2 / CH 4 The selectivity is 15.8±0.3.

[0042] Embodiment 3:

[0043] A SPM / IL@ZIF-8(5) mixed matrix membrane was prepared. The difference from the SPM / IL@ZIF-8(1) mixed matrix membrane in Example 1 is that the thickness of the obtained SPM / IL@ZIF-8(5) mixed matrix membrane is 182 μm, wherein the mass ratio of SPM to IL@ZIF-8 is 0.95:0.05. The preparation method of the mixed matrix membrane is different from that of Example 1 only in that in step 3, 0.045 g IL@ZIF-8 is weighed instead of 0.009 g IL@ZIF-8; finally, a mixed matrix membrane with a thickness of 182 μm is obtained.

[0044] Please refer to Figure 4As shown: At 25 °C and 2 bar, the SPM / IL@ZIF-8(5) mixed matrix membrane prepared in Example 3 was used for CO 2 CO with a volume fraction of 20% 2 / CH 4 Mixed gas separation test, its CO 2 The flux is 807.8±8 Barrer, CO 2 / CH 4 The selectivity is 17.5±0.2.

[0045] Embodiment 4:

[0046] A SPM / IL@ZIF-8(7) mixed matrix membrane was prepared. The difference from the SPM / IL@ZIF-8(1) mixed matrix membrane in Example 1 is that the thickness of the obtained SPM / IL@ZIF-8(7) mixed matrix membrane is 187 μm, wherein the mass ratio of SPM to IL@ZIF-8 is 0.93:0.07. The preparation method of the mixed matrix membrane is different from that of Example 1 only in that in step 3, 0.063 g of IL@ZIF-8 is weighed instead of 0.009 g; finally, a mixed matrix membrane with a thickness of 187 μm is obtained.

[0047] Please refer to Figure 5 As shown: At 25 °C and 2 bar, the SPM / IL@ZIF-8(7) mixed matrix membrane prepared in Example 4 was used for CO 2 CO with a volume fraction of 20% 2 / CH 4 Mixed gas separation test, its CO 2 The flux was 744.9±9 Barrer, CO 2 / CH 4 The selectivity is 16±0.3.

[0048] Comparative Example 1

[0049] Prepare an SPM film with a thickness of 160 μm. The preparation method is as follows: weigh 0.537 g of 1657 particles and 0.358g of PEG-MEA were dissolved in 10ml of ethanol and water mixed solution (the mass ratio of ethanol to water was 70% / 30%), heated in a water bath at 80°C for 2h with stirring to completely dissolve the Pebax particles and PEG-MEA, and added with 1wt.% AIBN to obtain a 6wt.% SPM casting solution after reaching room temperature. The casting solution was poured on a clean petri dish and cast, dried at room temperature (25°C) for 48h, and then the residual solvent on the surface of the mixed matrix membrane was removed in a vacuum drying oven at 40°C, and then thermally initiated at 80°C to fully polymerize, to obtain a self-polymerized constrained SPM membrane with a membrane thickness of 160μm.

[0050] Please refer to Figure 6 As shown: At 25°C and 2 bar, the SPM membrane prepared in the comparative example was used for CO 2 CO with a volume fraction of 20% 2 / CH 4 Mixed gas separation test, its CO 2 Flux is 410.2±10 Barrer, CO 2 / CH 4 The selectivity is 12.2±0.4.

[0051] Comparative Example 2

[0052] The SPM / ZIF-8(5) mixed matrix membrane was prepared. The difference from the SPM / IL@ZIF-8(5) mixed matrix membrane in Example 3 was that in step 3, 0.045 g of IL@ZIF-8 was replaced by 0.045 g of ZIF-8. Finally, a mixed matrix membrane with a thickness of 168 μm was obtained.

[0053] Please refer to Figure 7 As shown: At 25°C and 2 bar, the SPM / ZIF-8(5) mixed matrix membrane prepared in Comparative Example 2 was used for CO 2 CO with a volume fraction of 20% 2 / CH 4 Mixed gas separation test, its CO 2 The flux is 613.2±5 Barrer, CO 2 / CH 4 The selectivity is 14.8±0.4.

[0054] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing an IL@ZIF-8 composite material for a novel rapid delivery system, characterized in that: The preparation method comprises the following steps: (1) 1-Methylimidazole and 3-chloropropyltriethoxysilane are heated under N2 atmosphere and refluxed with stirring. After the reaction, the obtained suspension is extracted with an appropriate amount of petroleum ether. The product is rotary evaporated to remove the remaining petroleum ether, and then further dried in a vacuum oven to obtain an ionic liquid intermediate. (2) LiTf2N was dissolved in deionized water, and then the ionic liquid intermediate synthesized in step (1) was slowly added to the above solution, stirred at room temperature, and washed with deionized water. The resulting suspension was separated by a separatory funnel, then rotary evaporated, and dried in a vacuum oven to obtain IL. (3) The IL prepared in step (2) was dispersed in acetone to obtain solution A, and Zn(NO3)2·6H2O and 2-Hmim were dissolved in solution A respectively, and stirred thoroughly until the solution was clear and uniform. Then, the IL solution containing Zn salt was added to the 2-Hmim solution, and stirred continuously at room temperature. After the reaction was completed, the mixture was collected by centrifugation, and washed with acetone and an appropriate amount of methanol. Finally, it was dried in a vacuum oven to obtain IL@ZIF-8.

2. The preparation method according to claim 1, characterized in that: (1) The amount of 1-methylimidazole and 3-chloropropyltriethoxysilane used in step (1) is (0.25 mol): (0.25 mol); the stirring temperature is 90-100° C. and the stirring time is 20 h to 24 h. (2) In step (2), the amount of LiTf2N, ionic liquid intermediate and deionized water used is in the ratio of 0.2 mol: 0.2 mol: 260 mL. (3) Solution A in step (3) is prepared by dispersing the IL prepared in step (2) in acetone, and its concentration is 10 wt.%. The amount of Zn(NO3)2·6H2O, 2-Hmim, and acetone is in the ratio of 1.798 g: 4.000 g: 54 g.

3. Application of the IL@ZIF-8 composite material imitating the novel rapid delivery system according to claim 1 in carbon capture.

4. A mixed matrix membrane, wherein the mixed matrix membrane uses IL@ZIF-8 composite material imitating a new rapid delivery system as a filler and self-polymerization constrained Pebax / PEG-MEA (SPM) as a base material, and the filler and the base material are physically blended at room temperature to form the mixed matrix membrane; the thickness of the mixed matrix membrane is 166 to 187 μm; the mass percentage of the filler in the mixed matrix membrane is 1% to 7%.

5. Use of the mixed matrix membrane according to claim 4 in the field of CO2 / CH4 mixed gas separation.