NiCr catalyst, preparation thereof and application of NiCr catalyst in hydrogen production through methane cracking

By using NiCr catalyst in methane cracking technology and constructing special Ni-O-Cr chemical bonds and acidic surface sites, the problems of easy catalyst deactivation and high reaction temperature are solved, and efficient preparation of hydrogen and carbon nanotubes is achieved, improving Improve the stability of the catalyst and methane conversion rate.

CN118767930APending Publication Date: 2024-10-15CENT SOUTH UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310321661.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing methane cracking hydrogen production technology has problems such as easy catalyst deactivation, high reaction temperature, and difficult separation of by-products, which limits its industrial application.

Method used

Using the preparation method of NiCr catalyst, the NixCr2O4 compound is roasted and modified in a reducing atmosphere to construct special Ni-O-Cr chemical bonds and acidic surface sites to improve the stability of the catalyst and methane cracking performance.

Benefits of technology

It achieves efficient catalytic methane cracking under relatively low temperature conditions to generate high-quality hydrogen and carbon nanotubes, significantly improving the stability of the catalyst and methane conversion rate. The hydrogen concentration can reach 95vol%, and the quality of the by-product carbon nanotubes is better than that of commercial products. product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767930A_ABST
    Figure CN118767930A_ABST
Patent Text Reader

Abstract

The invention relates to the field of methane catalytic cracking, in particular to a preparation method of a NiCr catalyst, which comprises the following steps: obtaining a NixCr2O4 compound, and roasting and modifying the NixCr2O4 compound in a reducing atmosphere to obtain the NiCr catalyst, wherein x ranges from 0.4 to 2. The invention also provides preparation of the catalyst and application of the catalyst in hydrogen production by methane cracking, and the carbon nanotube with high added value can be produced by methane cracking under the action of the catalyst. The catalyst provided by the invention has excellent effect of catalyzing methane cracking to produce hydrogen and capability of preparing carbon nanotubes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical fields of functional materials, energy conversion and environmental protection, and in particular to a catalyst for catalyzing methane cracking to produce hydrogen. Background Art

[0003] At present, the existing hydrogen production pathways mainly include methane steam reforming, methane dry reforming, methane partial oxidation and methane cracking. At present, methane steam reforming is the most commonly used methane hydrogen production technology in industry because of its mature technology and low cost. However, since this technology needs to go through methane reforming, high / low temperature water gas shift, methanation coupled with carbon dioxide removal or pressure swing adsorption and other steps, it is not only complicated in process and energy-consuming, but also the catalyst is very easy to deactivate. It is particularly important to explore new ways of methane hydrogen production. Methane partial oxidation uses methane, oxygen or appropriately active catalysts as raw materials. Although it has low energy consumption, high methane conversion rate and synthesis gas selectivity, it also has problems such as easy catalyst deactivation and low mechanical strength. Methane dry reforming technology uses methane and carbon dioxide as raw materials, and realizes the utilization of methane and carbon dioxide under the condition of catalyst, which can greatly reduce energy consumption and realize the conversion of two greenhouse gases. However, the main reason restricting its development is the many side reactions such as reverse water gas shift. Compared with the above, methane cracking can not only produce hydrogen in one step and simplify the process, but also produce high concentration of hydrogen. The by-product is carbon nanotubes with low graphitization degree, which can be directly separated from hydrogen. At the same time, because it not only has the same hardness as diamond, but also has good flexibility, can be stretched, is extremely light, has strong conductivity, and has the properties of both metal and semiconductor, it has broad application prospects. However, at present, methane cracking hydrogen production is still in the initial stage of laboratory research and development, and there are still certain technical problems that need to be solved. First, methane cracking is a strong endothermic reaction, and the cracking temperature is usually higher than 1000°C under the condition of no catalyst; secondly, if a catalyst is added, although the reaction temperature and methane cracking rate can be reduced, the catalyst is very prone to coking and deactivation, and the stability is poor. Summary of the invention

[0004] In order to solve the deficiencies of the prior art, the first object of the present invention is to provide a method for preparing a NiCr catalyst, aiming to prepare a new catalyst having special structural characteristics and excellent catalytic activity and stability for methane cracking to produce hydrogen.

[0005] The second object of the present invention is to provide a NiCr catalyst prepared by the preparation method, aiming to obtain a NiCr catalyst having special physical and chemical characteristics and excellent hydrogen production capacity based on the preparation method.

[0006] The third object of the present invention is to provide a method for using the NiCr catalyst in hydrogen production from methane.

[0007] A method for preparing a NiCr catalyst to obtain Ni x Cr2O4 compound is then subjected to a calcination modification treatment in a reducing atmosphere to obtain the product; wherein x is 0.4 to 2.

[0008] In the present invention, Ni is prepared in advance x The compound of the Cr2O4 phase is further calcined and modified under the reducing atmosphere, and further coordinated with the control of x, so that a catalyst with new characteristics of special Ni-O-Cr chemical bonds, active surface, acidic sites and oxygen vacancies can be unexpectedly obtained, and the catalyst prepared by the preparation method has excellent catalytic activity and stability in methane cracking and hydrogen production, and high-quality carbon nanotubes can be obtained.

[0009] In the present invention, Ni x Calcination modification of Cr2O4 compound materials under a reducing atmosphere is the key to successfully preparing the catalyst, constructing special Ni-O-Cr chemical bonds, acidic surfaces and oxygen vacancies, and improving the surface dispersion distribution of active sites, thereby improving the methane cracking hydrogen production performance and stability of the catalyst.

[0010] In the present invention, further controlling the Ni / Cr molar ratio helps to further improve the performance of the material. Preferably, x is 0.8-1.6; preferably 1-1.2 (that is, the Ni / Cr molar ratio is 0.8-1.6:2, preferably 1-1.2:2), and better preparation performance can be obtained.

[0011] In the present invention, the Ni x The Cr2O4 compound can be prepared based on existing methods, preferably by a sol-gel method to synthesize the Ni x Cr2O4 compounds.

[0012] More preferably, the nickel source, the chromium source and the complexing agent are subjected to a sol-gel reaction, followed by drying to obtain a precursor, and then the precursor is calcined in an oxygen-containing atmosphere to obtain the Ni x Cr2O4 compounds.

[0013] Preferably, the nickel source and the chromium source are water-soluble salts of the respective metals, preferably at least one of chlorides, sulfates, nitrates, and organic acid salts;

[0014] In the present invention, there is no special requirement for the complexing agent, and it can be, for example, conventional citric acid.

[0015] Preferably, the molar ratio of the total metal of the nickel source and the chromium source to the complexing agent is 1:1 to 1.5;

[0016] Preferably, the temperature of the sol-gel reaction is 50 to 90°C;

[0017] There is no particular requirement for the sol-gel reaction time, for example, 40 to 100 minutes;

[0018] In the present invention, the precursor can be obtained by drying by evaporation or freeze drying. There is no special requirement for the drying time, for example, 5 to 10 hours.

[0019] Preferably, the oxygen-containing atmosphere is an atmosphere containing air and / or oxygen;

[0020] The calcination temperature is not particularly required, for example, 800 to 900°C, preferably 800 to 860°C;

[0021] Preferably, the calcination time is 3 to 6 hours, preferably 4 to 5 hours.

[0022] In the present invention, the reducing atmosphere is an atmosphere containing hydrogen;

[0023] Preferably, in the hydrogen-containing atmosphere, the volume content of hydrogen is greater than or equal to 1v%, preferably 5-25v%, and more preferably 10-20v%.

[0024] In the present invention, controlling the calcination temperature is helpful to further improve the microscopic characteristics of the product and the cracking hydrogen production performance. Preferably, the calcination temperature is 500-850° C., more preferably 650-750° C., and more preferably 700-720° C. Studies have found that at the preferred temperature, it is more conducive to obtaining products with better cracking ability.

[0025] Preferably, the calcination time is 1 to 8 hours, more preferably 2 to 4 hours.

[0026] The present invention also provides a method for preparing the NiCr catalyst, comprising the following steps:

[0027] 1) Mixing nitrate precursors of nickel and chromium with citric acid; the metal raw material is a water-soluble compound that can provide the nickel and chromium, preferably chloride, nitrate and sulfate of the metal. The molar amount of citric acid added is 1.0 to 1.5 times the total molar amount of metal atoms in the metal raw material.

[0028] 2) Add deionized water and stir to obtain a solution; the stirring temperature is preferably 50 to 80° C., the stirring time is 40 to 60 minutes, and the drying time is, for example, 5 to 10 hours.

[0029] 3) The solution obtained in step 2) is foamed and dried at a temperature range of 120-180° C., and the obtained solid sample is crushed and ground; in step 2), the particle size of the crushed and ground material is less than or equal to 0.3 mm.

[0030] 4) The sample ground in step 3) is oxidatively calcined at 800-900° C., and the calcined solid powder is ground to obtain fresh Ni x Cr2O4 product; in step 3), the calcination time is 3 to 6 hours. The heating rate is 2 to 5°C / min. In step 3), the muffle furnace calcination is carried out under oxygen or air atmosphere. In step 4), the particle size of the ground sample is controlled between 0.10 and 0.25 mm.

[0031] 5) The sample ground in step 4) is calcined at 650-750° C. for 2-4 hours in a hydrogen atmosphere to finally obtain a NiCr catalyst. In step 5), the particle size of the reduced sample is controlled to be between 0.10 and 0.25 mm.

[0032] The invention also provides a NiCr catalyst prepared by the preparation method, which has Ni-O-Cr action bonds and has acidic sites and oxygen vacancies.

[0033] In the present invention, thanks to the special preparation method, a special Ni-O-Cr interaction bond can be constructed, with acidic sites and oxygen vacancies, which improves the surface dispersion distribution of active sites and further improves the methane cracking hydrogen production capacity.

[0034] Preferably, the NiCr catalyst has a nanosheet morphology; the grain size is preferably 10 to 50 nm, preferably 10 to 30 nm; and Ni, Cr and O are preferably evenly distributed on the catalyst surface.

[0035] The present invention also provides an application of the NiCr catalyst (that is, a method for producing hydrogen from methane), which is used for catalyzing methane cracking to produce hydrogen.

[0036] Preferably, the temperature of the methane cracking process for producing hydrogen is 650-900° C., preferably 750-800° C. At the preferred cracking temperature, there is a synergistic effect with the preparation process of the catalyst of the present invention, and the catalytic ability of the catalyst of the present invention can be fully exerted.

[0037] Preferably, the cracking starting atmosphere is a mixed gas containing methane and protective gas, wherein the methane content is 5-50v%, preferably 10-40v%, and more preferably 10-20v%. The protective gas is at least one of nitrogen and inert gas.

[0038] Preferably, methane is contacted with the catalyst and reacted at 650-900° C., preferably 750-800° C., to produce hydrogen and high-quality carbon nanotubes.

[0039] More preferably, the carbon nanotubes D / I G Less than or equal to 1 and I G' / I G More preferably, the carbon nanotubes have an I D / I G It can be 0.4 to 0.8, and I G' / I G It is 1 to 1.2.

[0040] The technical solution of the present invention, through the use of the NiCr catalyst, can not only convert methane into hydrogen with a high conversion rate, but also convert the carbon element therein into high-quality CNTs.

[0041] Preferably, the methane can be replaced by other alkanes of C1 to C4.

[0042] Beneficial effects:

[0043] 1) In the present invention, Ni x The Cr2O4 compound is calcined in a reducing atmosphere, and with the control of x, a special Ni-O-Cr strong bond can be constructed. In addition, an acid site is constructed, and the surface dispersion distribution effect of the active site is regulated. In addition, it is also conducive to the construction of oxygen vacancies, which can unexpectedly improve the performance of the prepared material. On this basis, the present invention also found that the sol-gel method is used to form Ni x The Cr2O4 compound, combined with the calcination treatment under the reducing atmosphere, helps to further synergistically improve the structure, phase and performance of the material.

[0044] The preparation method of the present invention can achieve a strong interaction force between Ni metal and Cr metal, construct a catalytic system for efficient methane cracking to produce hydrogen, and can greatly improve the methane conversion rate under relatively low temperature conditions; high-purity hydrogen can be directly obtained.

[0045] Research has found that the methane conversion rate of the present invention can reach up to more than 100%, and the concentration of hydrogen can reach 95 vol%.

[0046] 2) The NiCr catalyst prepared by the preparation method of the present invention has oxygen vacancies, strong interactions between metals and acidic sites, which are conducive to the formation of high-quality carbon nanotube by-products and have certain commercial utilization value.

[0047] 3) The present invention modulates the structure of Cr-O-Ni, which is analyzed to be beneficial to the efficient methane cracking hydrogen production reaction, and can realize methane conversion at a relatively low temperature and the production of hydrogen.

[0048] 4) This method effectively inhibits the sintering and agglomeration of the catalyst, and greatly improves the stability and catalytic activity of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 The surface microstructure of the Ni1.2Cr2 catalyst obtained in step 6 of Example 1

[0050] Figure 2 The microscopic morphology (carbon nanotube image) of the Ni1.2Cr2 catalyst after reaction obtained in step 6 of Example 1;

[0051] Figure 3 This is a test graph of hydrogen content and methane conversion rate of the Ni1.2Cr2 catalyst prepared in Example 1 under reference test A;

[0052] Figure 4 I is the by-product carbon nanotubes obtained by the Ni1.2Cr2 catalyst prepared in Example 1 under reference test A D / I G Test chart;

[0053] Figure 5 This is a test graph of hydrogen content and methane conversion rate of the Ni1.2Cr2 catalyst prepared in Example 1 under reference test B;

[0054] Figure 6 The Ni1.2Cr2 catalyst prepared in Example 1 (cracking temperature of 750°C, methane content of 20 vol%) was subjected to a long-term cyclic reaction under reference test C;

[0055] Figure 7 Phase diagrams of different Ni / Cr ratios of Example 1, Example 2 and Comparative Example 1;

[0056] Figure 8 The specific surface area diagram of the catalysts with different Ni / Cr ratios in Example 1 and Example 2;

[0057] Fig. 9 NH3-TPD analysis of catalysts with different Ni / Cr ratios in Example 1 and Example 2

[0058] Fig.10 H2-TPR analysis of catalysts with different Ni / Cr ratios in Example 1 and Example 2

[0059] Fig.11 H2-TPD analysis of catalysts with different Ni / Cr ratios in Example 1 and Example 2

[0060] Fig.12 Phase analysis of NiCr catalyst after catalytic methane cracking reaction for 1 to 2 hours and Raman analysis of carbon nanotubes produced after cracking;

[0061] Fig.13 The graphs are the test graphs of hydrogen content and methane conversion rate of the catalysts prepared in Examples 1 to 2 and Comparative Example 1;

[0062] Fig.14 is a phase diagram of the newly prepared catalyst obtained in Example 3;

[0063] Fig.15 The hydrogen content and methane conversion rate test diagram of the catalyst prepared in Example 3;

[0064] Fig.16 XPS and Raman images of the newly prepared catalysts prepared in Comparative Example 2 and Example 1;

[0065] Fig.17 It is the cracking gas content diagram of the catalyst of Comparative Example 2; DETAILED DESCRIPTION

[0066] Example 1

[0067] 1) mixing nickel nitrate, chromium nitrate and citric acid, wherein the molar amount of citric acid added is 1.3 times the total molar amount of all metal atoms, wherein the ratio of nickel to chromium is 1.2:2.0;

[0068] 2) adding deionized water to prepare a solution (wherein the molar concentration of Ni is 1.2 M);

[0069] 3) Stir the prepared solution at 80° C. for 60 minutes;

[0070] 4) placing the solution obtained in step 3) in a drying oven, foaming and drying at a temperature range of 150° C. for 6 hours, and crushing and grinding the obtained solid sample;

[0071] 5) The ground sample in step 4) is placed in a muffle furnace and calcined at 850° C. in an air atmosphere for 4 hours with a heating rate of 2° C. / min. The calcined solid powder is ground to a particle size of less than 0.3 mm to obtain fresh Ni 1.2 Cr2O4 product, grind the catalyst to a particle size not greater than 0.25 mm.

[0072] 6) Ni obtained in step 5) 1.2 The Cr2O4 product was reduced by introducing 20v% hydrogen-Ar mixed gas (total flow rate of 50mL / min) at 700℃ for 2 hours to obtain modified Ni 1.2Cr2O4 catalyst, marked as Ni1.2Cr2 catalyst.

[0073] 7): 0.3 g of the catalyst was loaded into a tubular furnace reactor, into which methane diluted with nitrogen with a volume fraction of 20 vol% was introduced, wherein the nitrogen flow rate was 40 mL / min, and the methane flow rate was 10 mL / min, and the reaction was carried out at 750°C (cracking temperature). After the reaction, the reaction tail gas was collected, and the methane conversion rate, hydrogen concentration of the product gas and carbon deposition properties were determined.

[0074] The chemical formula of the obtained catalyst is Ni1.2Cr2 catalyst. Its microscopic characterization results are shown in Figure 1 Combined with the microscopic morphology of the catalyst, it is not difficult to know that the catalyst is in the morphology of Ni1.2Cr2 catalyst nanosheets, and the three elements Ni, Cr, and O are evenly distributed on the catalyst surface.

[0075] The microscopic image of the catalyst after 1 h of catalysis is shown in Figure 2 It can be found that the Ni, Cr, and O elements of the Ni1.2Cr2 catalyst are evenly distributed after the reaction, and a large amount of by-product carbon nanotubes are produced, that is, methane is efficiently converted into hydrogen.

[0076] Reference test A: The cracking temperature in step 7) was changed to 650-900°C (methane feed gas content was 20v%). The methane conversion rate and hydrogen concentration of the product gas were measured. The results are shown in Figure 3 .

[0077] After determining the best catalyst, we optimized the reaction temperature range, using hydrogen concentration and methane conversion as indicators. The results are as follows: Figure 3 As shown. The hydrogen concentration result graph in the temperature range of 650-900℃ shows that when the temperature is lower than 700℃, the hydrogen concentration drops significantly. When the temperature is higher than 800℃, it can be found that the catalyst has good performance in the early stage of the reaction, but too high a temperature will cause rapid agglomeration and sintering of the catalyst, resulting in a rapid decline in performance. It is further found that the temperature range of 750-800℃ is the optimal temperature range for catalytic methane cracking, and the hydrogen concentration can be as high as 95% or more. The high methane conversion rate and high hydrogen concentration solve the problem of separation of hydrogen and methane.

[0078] I of carbon materials obtained by catalysis at different temperatures D / I G See Figure 4 and Table 1.

[0079] Table 1 Statistics of Raman characterization results of carbon nanotubes as byproducts of catalysts at different temperatures

[0080]

[0081] Among them, I D / I G Used to characterize the disordered structure of carbon substances, I D / I G The lower the ratio, the lower the degree of disorder. Therefore, it can be seen that as the temperature increases, I D / I G It stabilizes first and then decreases, reaching the maximum at 700℃ and 750℃.

[0082] Reference test B: The content of methane raw gas in step 7) was changed to 10 vol% to 40 vol% (the cracking temperature was 750°C). The methane conversion rate and hydrogen concentration of the product gas were measured. The results are shown in Figure 5 .

[0083] From the hydrogen concentration result graph in the methane concentration range of 10 vol% to 40 vol%, it can be found that when the methane concentration is 10 vol%, the hydrogen concentration is the highest and the methane conversion rate also reaches the highest value. The catalyst performance is good, which is the optimal catalytic methane cracking concentration.

[0084] Reference Test C:

[0085] The prepared catalyst was cycled to step 7) to test its cycle performance (which is specifically divided into a methane cracking stage and a carbon dioxide reduction stage. In the methane cracking stage, the methane content is 20 vol%; the cracking temperature is 750°C; in the carbon dioxide reduction stage, the carbon dioxide content is 20 vol%; the reduction temperature is 850°C). The results are shown in Figure 6 ;pass Figure 6 It can be seen that it has excellent cycle stability.

[0086] Example 2

[0087] Compared with Example 1, the only difference is that the molar ratio of nickel to chromium in step 1 is changed, and the experimental groups are:

[0088] Group A: Ni / Cr molar ratio is 0.8:2.0. Step 6 The final modified product obtained is labeled as Ni0.8Cr2 catalyst.

[0089] Group B: Ni / Cr molar ratio is 1.6:2.0. Step 6 The final modified product obtained is labeled as Ni1.6Cr2 catalyst.

[0090] Group C: Ni / Cr molar ratio is 0.4:2.0. Step 6 The final modified product obtained is labeled as Ni0.4Cr2 catalyst.

[0091] Group D: Ni / Cr molar ratio is 2:2.0. Step 6 The final modified product obtained is labeled as Ni2Cr2 catalyst.

[0092] Comparative Example 1

[0093] Compared with Example 1, the only difference is that in step 1, nickel nitrate is not added, and other operations and parameters are the same as in Example 1. The catalyst finally obtained in step 6 is a Cr2O3 catalyst with oxygen vacancies.

[0094] The phase diagrams of different Ni / Cr ratios of Example 1, Example 2 and Comparative Example 1 are shown in Figure 7 , where the left figure is the XRD graph of the catalyst prepared by the uncoupled hydrogen reduction method; the right figure is the XRD graph of the catalyst prepared by the coupled hydrogen reduction method. It can be seen from the figure that before hydrogen reduction, when the Ni / Cr molar ratio is lower than 1.2:2, the catalyst phases are NiO and NiCr2O4, when it is higher than 1.2:2, the phases are Cr2O3 and NiCr2O4, and when it is equal to 1.2:2, it is just completely displayed as NiCr2O4. After hydrogen reduction, the catalyst phases at each ratio are detected as Ni and Cr2O3.

[0095] According to the X-ray diffraction results, the lattice parameters of the catalysts prepared in step (6) of Examples 1 and 2 were calculated using the Scherrer formula, as shown in Table 2. 1.2 The Cr2 catalyst has a smaller grain size and thus has better catalytic activity.

[0096] Table 2 Grain parameters of different embodiments and comparative examples

[0097]

[0098] Figure 8 The specific surface area diagram of different Ni / Cr ratios of Example 1 and Example 2;

[0099] NH3-TPD, H2-TPR, H2-TPD analysis are shown in Figures 9-11 .

[0100] In the NH3-TPD spectrum, Fig. 9 As shown, a low-temperature peak can be observed at about 280 °C, which is due to the presence of Lewis acid sites due to the ammonia absorbed on the terminal -OH group. In addition, as the Ni / Cr ratio gradually increases, medium and high temperature peaks appear, which are assigned to strong Bronsted acid sites. Example 1 observed that the temperature peak changes to 375 °C, indicating that the binding ability between –OH and ammonia is enhanced. This can be attributed to the formation of Ni-O-Cr structure. In addition, peaks at 575 °C and 670 °C are clearly observed, which may be the main factor leading to the good methane cracking performance.

[0101] H2-TPR can reflect the changes in the reducibility of compounds in multi-component systems and can also clarify the interaction between metal oxides and supports. Fig.10 As shown. The first peak of Example 1 at around 370°C can be attributed to the reduction of NiO, which has a relatively low interaction with Cr2O3. These substances have high lattice oxygen activity and are therefore easily reduced by hydrogen at low temperatures. In addition, the sample of Example 1 shows the highest hydrogen reduction temperature at about 740°C, which can be attributed to the strong interaction between Ni and Cr. The intermediate peaks of both Example 2C group and Example 2A group samples can be explained by the reduction of Cr2O3 without Ni binding. Under the Ni / Cr ratio, the reduction peaks of both the low-temperature and high-temperature reduction peaks show a trend of first increasing and then decreasing, indicating that an appropriate amount of Ni doping can enhance the interaction between Ni and Cr. This can further promote the catalytic stability of the catalyst.

[0102] In addition, the hydrogen adsorption behavior and the dispersion of active components were investigated by H2-TPD measurements, e.g. Fig.11 As shown. With the increase of Ni / Cr ratio, the peak shifts to a higher temperature. This phenomenon may be due to the strong adsorption of hydrogen on the catalyst surface, or the close combination of hydrogen with the catalyst matrix or the desorption of escaped hydrogen, which will increase the hydrogen storage capacity. At the same time, after integrating the catalysts with different ratios, the area of ​​Example 1 is larger than that of the other catalysts, indicating that its surface has a higher nickel dispersion and more surface dissociated hydrogen is formed on the catalyst.

[0103] The methane cracking test was carried out under the conditions of step 7) of Example 1 (the test conditions were: the content of methane feed gas was 20 vol%, and the cracking temperature was 750° C.);

[0104] Fig.12 Phase analysis of NiCr catalyst after catalytic methane cracking reaction for 1 to 2 hours and Raman analysis of carbon nanotubes produced after cracking;

[0105] The results are shown in Table 3:

[0106]

[0107] The carbon nanotubes produced as byproducts after 1 hour of hydrogen production by catalytic methane cracking with different comparative catalysts were analyzed by Raman spectroscopy, and the specific results after peak fitting are shown in Table 3. D / I G Used to characterize the disordered structure of carbon substances, I D / I G The lower the ratio, the lower the degree of disorder. Therefore, it can be seen that as the nickel-chromium ratio increases, I D / I G Increase first and then decrease, at Ni1.2 The maximum value is reached when Cr2O4 is used. G' can be attributed to the two-photon elastic scattering process, and the ratio of carbon nanotubes generated by the catalyst prepared by the method of the present invention after catalyzing methane cracking to produce hydrogen is higher than the ratio of commercial carbon nanotubes, which is 0.69, indicating that the quality of the byproduct carbon nanotubes is better than that of commercial carbon nanotubes.

[0108] Fig.13 The graphs are the test graphs of hydrogen content and methane conversion rate of the catalysts prepared in Examples 1 to 2 and Comparative Example 1;

[0109] It shows that when the molar ratio of Ni to Cr is between 0.8 and 1.6, especially between 1 and 1.2, better methane catalytic conversion rate and hydrogen yield can be achieved.

[0110] Embodiment 3:

[0111] Compared with Example 1, the only difference is that the temperature of step (6) is changed. The experimental groups are:

[0112] Group A: reduction temperature is 500°C and time is 4h. The final modified product obtained in step 6 is labeled as Ni1.2Cr2-500°C-4h catalyst;

[0113] Group B: reduction temperature is 850°C and time is 2h. Step 6 obtains the final modified product marked as Ni1.2Cr2-850°C-2h catalyst.

[0114] The physical properties of different newly prepared catalysts are shown in Fig.14 .

[0115] According to the method of Example 1, the methane conversion rate, hydrogen concentration of the product gas and carbon deposition properties were measured (the methane content in the methane feed gas was 20 vol%, and the cracking temperature was 750°C). The results are shown in Fig.15 It can be seen that a better methane cracking hydrogen production effect can be obtained by catalyzing at the above temperature for a suitable time.

[0116] Comparative Example 2

[0117] Compared with Example 1, the only difference is that the NixCr2O4 phase reduction preparation idea of ​​the present invention is not adopted, but nickel nitrate and Cr2O3 are directly reduced (the reduction conditions are the same as step 6 of Example 1), and the preparation is as follows:

[0118] Nickel nitrate and Cr2O3 are impregnated in an aqueous solution at a molar ratio of NI to Cr of 1.2:2.0, and then the solvent is evaporated to remove the solvent, and then the reduction roasting treatment of step (6) of Example 1 is carried out.

[0119] Fig.16XPS and Raman images of the newly prepared catalysts of Comparative Example 2 and Example 1.

[0120] From the XPS graph, we can see that the Ni 2p spectrum is divided into six sub-peaks, among which the sub-peaks at 852.6eV (Ni 2p 3 / 2) and 870.0eV (Ni 2p 1 / 2) belong to Ni 0 This indicates that after hydrogen reduction, the surface Ni species is replaced by Ni 0 The peaks at 855.7 eV and 874.4 eV can be attributed to Ni +δ Ni species (2<δ<3). In addition, the binding energies at 861.2eV and 879.8eV are assigned as satellite peaks of the above Ni species. The sub-peaks at 575.3eV (2p 3 / 2) and 584.6eV (2p 1 / 2) may belong to Cr +(3-ɑ) (0<ɑ<3). This may be due to the reduction of Cr by hydrogen 3+ Combing the XPS spectra of Ni and Cr, it is expected that a strong interaction is formed between Cr and Ni due to the formation of Ni-O-Cr structure, which also confirms the electron transfer from Ni to Cr. The strong peaks at 576.6eV (Cr 2p 3 / 2) and 586.1eV (Cr 2p 1 / 2) in spinel are assigned to Cr 3+ In addition, the peaks at 578.2 eV and 587.3 eV correspond to Cr 6+ The presence of Cr-O may be derived from the unreduced Cr-O octahedral structure. The O 1s spectrum can be divided into three peaks, 529.8 eV (OI), 531.2 eV (OII) and 532.3 eV (OIII), corresponding to the lattice oxygen, oxygen vacancies and surface –OH or CO3 on the catalyst surface, respectively. 2- The abundant oxygen vacancies formed can effectively promote the activation of methane and the surface Ni +δ A moderate amount of lattice oxygen can be provided to synergistically promote methane decomposition.

[0121] After speculating that the Ni-O-Cr structure may appear, Raman was used for further verification. The results are as follows Fig.16 As shown. 303, 350cm -1 and 548,607cm -1 The peak at 548 cm-1 corresponds to the typical Cr2O3 structure. -1 The peak at 350 cm shifts to lower wavenumbers, indicating the evolution of the catalyst structure and the formation of more lattice defects. -1The peak at 548 cm-1 is attributed to the formation of octahedral CrO6 sites, while the peak at 548 cm-1 originates from the tetrahedral NiO4 structure. Two different peaks can be observed in Example 1 relative to Comparative Example 2, located at 500 cm-1 and 527 cm-1, respectively. -1 and 660cm -1 , which is a Ni-O-Cr structure. This is because Ni +δ and Cr +(3-ɑ) The strong interaction between them is ultimately formed by sol-gel synthesis and its hydrogen reduction.

[0122] The catalytic performance of the catalyst of Comparative Example 2 was measured using the method of Example 1. The results are shown in Fig.17 ;pass Fig.17 It can be seen that the performance of the catalyst prepared by the preparation method of Comparative Example 2 is significantly worse than that of the preparation method of the present invention.

Claims

1. A method for preparing a NiCr catalyst, characterized in that: Get Ni x Cr2O4 compound, and then calcining it in a reducing atmosphere to obtain; Among them, x is 0.4~2.

2. The method for preparing the NiCr catalyst according to claim 1, characterized in that: x is 0.8 to 1.6; preferably 1 to 1.2; Preferably, the Ni is synthesized by a sol-gel method. x Cr2O4 compounds.

3. The method for preparing the NiCr catalyst according to claim 2, characterized in that: The nickel source, the chromium source and the complexing agent are subjected to a sol-gel reaction, and then dried to obtain a precursor, and then the precursor is calcined in an oxygen-containing atmosphere to obtain the Ni x Cr2O4 compounds.

4. The method for preparing the NiCr catalyst according to claim 3, characterized in that: The nickel source and chromium source are water-soluble salts of the respective metals, preferably at least one of chloride, sulfate, nitrate, and organic acid salt; Preferably, the complexing agent is citric acid; Preferably, the molar ratio of the total metal of the nickel source and the chromium source to the complexing agent is 1:1 to 1.5; Preferably, the temperature of the sol-gel reaction is 50 to 90°C; Preferably, the oxygen-containing atmosphere is an atmosphere containing air and / or oxygen; Preferably, the calcination temperature is 800-900°C; Preferably, the calcination time is 3 to 6 hours.

5. The method for preparing the NiCr catalyst according to any one of claims 1 to 4, characterized in that: The reducing atmosphere is an atmosphere containing hydrogen; Preferably, in the hydrogen-containing atmosphere, the volume content of hydrogen is greater than or equal to 1v%, preferably 5-25v%.

6. The method for preparing the NiCr catalyst according to any one of claims 1 to 5, characterized in that: The calcination temperature is 500-850°C, more preferably 650-750°C; more preferably 700-720°C; Preferably, the calcination time is 1 to 8 hours, more preferably 2 to 4 hours.

7. A NiCr catalyst prepared by the method according to any one of claims 1 to 6, characterized in that: It has Ni-O-Cr interaction bonds, acidic sites and oxygen vacancies.

8. The NiCr catalyst according to claim 7, characterized in that Nanosheet morphology; Preferably, the grain size is 10-50 nm.

9. Use of a NiCr catalyst prepared by the preparation method according to any one of claims 1 to 6 or a NiCr catalyst according to any one of claims 7 to 8, characterized in that: It is used as a catalyst to catalyze the cracking of methane to produce hydrogen.

10. The use according to claim 9, characterized in that The temperature of the cracking hydrogen production is 650-900°C, preferably 750-800°C; Preferably, the methane content in the cracking starting atmosphere is 5 to 50 v%, preferably 10 to 40 v%; more preferably 10 to 20 v%; Preferably, the methane can be replaced by other alkanes of C1 to C4; Preferably, it is used as a catalyst to catalyze the cracking of methane to produce hydrogen and co-produce carbon nanotubes; Preferably, the carbon nanotubes are high-quality carbon nanotubes; Preferably, the carbon nanotubes D / I G Not higher than 1, I G' / I G Above 0.69.

Citation Information

Patent Citations

  • Process for preparing hydrogen gas and nanometer carbon by catalyzing and cracking methane at low temperature

    CN101337655A

  • CFAN catalyst, preparation method thereof, and application of CFAN catalyst in production of hydrogen from methane

    CN110721691A

  • Catalysts and processes for tunable base-grown multiwalled carbon nanotubes

    CN111372681A

  • Method of producing carbon nanotubes and catalysts therefor

    CN1360558A

  • Carried nanometer bi-metal catalyst, and prepn. method and application thereof

    CN1868591A