Preparation method of porous loading material for preparing solar fuel

By loading Ni0.8Co0.2Fe2O4 powder combined with Co2+ and Ni2+ and Fe3+ on the porous ceramic skeleton, the problem of low CO2 conversion rate and poor circulation ability of oxygen carrier materials at high temperatures is solved, and efficient CO2 conversion and thermal Chemical stability improves energy conversion efficiency.

CN118767959AActive Publication Date: 2024-10-15HARBIN INST OF TECH

Patent Information

Application Number
CN202410750768.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-15
Estimated Expiration
2044-06-12

AI Technical Summary

Technical Problem

Existing oxygen carrier materials have low CO2 conversion rates, poor circulation capabilities, and low energy conversion efficiency at high temperatures. Direct filling in the reactor can easily lead to sintering, which reduces the stability of the material.

Method used

Using porous load materials combined with Co2+ and Ni2+ and Fe3+, by preparing porous silicon carbide as the skeleton material, combined with the combination of Ni0.8Co0.2Fe2O4 powder and porous ceramic skeleton, the microscale heat transfer, mass transfer and circulation of ferrite are improved. performance.

Benefits of technology

It significantly improves the CO2 conversion rate and thermochemical stability, enhances the material's recycling capability and energy conversion efficiency, and extends the material's service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767959A_ABST
    Figure CN118767959A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a porous loading material for preparing solar fuel, and belongs to the field of fuel synthesis by cracking CO2 and H2O. The invention aims to provide the porous oxygen carrier-loaded composite material for synthesizing the solar thermochemical fuel, which is high in cycling stability and CO2 conversion rate. A porous ceramic framework material is synthesized through a template impregnation method, and an oxygen carrier material is loaded. The Ni < 0.8 > Co < 0.2 > Fe < 2 > O < 4 > synthesized by doping the Co element has relatively high stability in solar thermal chemical reduction of CO2.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of solar thermal chemistry and solar photothermal chemical cracking of CO2 and H2O to synthesize fuels, and in particular, relates to a method for preparing a porous support material for preparing solar fuels. Background Art

[0002] Oxygen carrier materials can decompose CO2 and H2O into CO and H2 at high temperatures, so they have great application prospects in the fields of solar thermal utilization, recycling of high-temperature exhaust gas, etc., effectively alleviating the greenhouse effect and energy crisis. Thermochemical conversion of CO2 under concentrated solar energy can decompose CO2 in industrial waste gas into CO fuel, and the temperature of CO2 decomposition in the two-step method is much lower than the temperature of direct conversion. However, the existing oxygen carrier material systems usually have problems such as low CO2 conversion rate, poor recycling capacity, and low energy conversion efficiency. Researchers have proposed many performance enhancement methods. Common materials are perovskite or spinel oxygen carriers, which improve the recycling capacity or reduce the temperature required for thermal reduction by doping or lattice substitution. Among them, nickel-based ferrite has high performance in fuel production and chemical stability, but the characteristic mechanism of various transition metal elements synergistically participating in the thermochemical CO2 conversion process, especially the thermal redox (reduction and oxidation) performance of Fe-Ni-Co nanocomposite oxide materials under different ratios and preparation methods has not been further studied.

[0003] Directly filling the oxygen carrier material into the reactor is prone to sintering, resulting in a large amount of material being unable to perform as expected and reducing stability. Summary of the invention

[0004] The object of the present invention is to provide a porous oxygen carrier composite material for solar thermochemical fuel synthesis with high cycle stability and high CO2 conversion rate. 2+ and Ni 2+ with Fe 3+ When used in combination for CO2 conversion, the micro-scale heat transfer, mass transfer and cycle performance of ferrite are significantly improved. The porous silicon carbide prepared by the method of the present invention has high thermal conductivity, high solar light absorption performance and high thermal stability, and is the best skeleton material for preparing shaped load materials.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0006] The present invention provides a method for preparing a porous support material for preparing solar fuel, comprising the following steps:

[0007] Step 1: Follow Ni 0.8 Co 0.2The stoichiometric ratio of Fe2O4 is as follows: Fe(NO3)3, Ni(NO3)2 and Co(NO3)2 hydrates are weighed respectively, deionized water is added, stirred evenly, and then a chelating agent is added, stirred evenly, and then stirred at 95°C for a period of time, a gel accelerator is poured in, and stirring is continued at 95°C until a colloid is formed, and then heated at 110°C until the gel becomes clear and deepens in color, and then heated at 110°C until a large number of pores appear, and then calcined until the gas is completely discharged, crushed, and ground to obtain Ni 0.8 Co 0.2 Fe2O4 powder;

[0008] Step 2: Soak the polyurethane foam in sodium hydroxide solution for 3 hours, and heat it in a water bath at 60°C to remove the diaphragm in the middle of the reticular polyurethane foam. (The diaphragm is a diaphragm in the middle of the polyurethane foam skeleton that blocks some of the holes and needs to be removed. Heating and soaking are performed simultaneously.)

[0009] Add SiC or Si3N4 powder into the binder solution to make slurry.

[0010] The treated polyurethane foam is immersed in the slurry, and then squeezed repeatedly, and the excess slurry is blown out to ensure that the pores are visible and the slurry does not flow out, and then dried, sintered in stages, and cooled to room temperature with the furnace to obtain a porous ceramic skeleton material;

[0011] Step 3: Ni obtained in step 1 0.8 Co 0.2 Fe2O4 powder is added into water, stirred continuously to form a suspension, impregnated and loaded on the porous skeleton, and dried to obtain the porous loading material;

[0012] Wherein, in step 2, the binder solution is composed of 10% (mass) aluminum dihydrogen phosphate, 0.5% (mass) PVA, 0.5% (mass) CMC and water.

[0013] It is further defined that the chelating agent is citric acid and the gel accelerator is polyethylene glycol PEG-400.

[0014] It is further defined that in step 1, calcination is performed at 950° C. for 4 hours.

[0015] It is further defined that in step 1, the molar ratio of the total molar number of cations of the three metal ions to the chelating agent is 1:2.5.

[0016] It is further defined that the pore size of the polyurethane foam in step 2 is 10 PPI, and the mass percentage concentration of the sodium hydroxide solution is 20%.

[0017] It is further defined that in step 2, the slurry is prepared in a ratio of 60 g SiC (or Si3N4) powder to 34 mL binder solution.

[0018] It is further defined that in step 2, the solid-liquid mass ratio is 7:4 and the treated polyurethane foam is immersed in the slurry.

[0019] It is further defined that the sintering process in step 2 is divided into stages: 1°C / min to 600°C for 60 minutes, 3°C / min to 1050°C, 1°C / min to 1300°C for 30 minutes, and 4°C / min to 1500°C for 120 minutes.

[0020] Further defined, step 3, the Ni obtained in step 1 is mixed at a solid-liquid ratio of 1:2 x Co 1-x Fe2O4 powder was added into water.

[0021] The method is used to prepare porous support materials for solar thermochemistry and solar photothermal chemical decomposition of CO2 and H2O.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] (1) A stable porous ceramic skeleton material is used to load an oxygen carrier material that can react with CO2 and is filled in a reactor for experimental testing.

[0024] (2) Improve the thermochemical stability of oxygen carrier materials for CO2 reduction. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is the temperature and product variation curve of solar thermochemical reduction of CO2 experiment with cobalt-doped nickel ferrite oxygen carrier material;

[0026] Figure 2 This is the temperature and product variation curve of the solar thermal chemical reduction of CO2 experiment with nickel ferrite oxygen carrier material over time;

[0027] Figure 3 This is a comparison of CO production in solar thermochemical experiments using oxygen carrier materials synthesized by the sol-gel method and the solid-state grinding method. DETAILED DESCRIPTION

[0028] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention.

[0029] Example 1: In this example, the oxygen carrier Ni is prepared 0.8 Co 0.2The specific steps of Fe2O4 are as follows: Weigh 0.6893g of Fe(NO3)3·9H2O hydrate, 0.1985g of Ni(NO3)2·6H2O hydrate and 0.0497g of Co(NO3)2·6H2O respectively, and then pour them into a beaker. Add 10mL of deionized water and stir the mixed solution. Then add citric acid monohydrate as a chelating agent and stir to mix, ensuring that the molar ratio of the total cation molar number of the three metal ions to citric acid is about 1:2.5. Stir at 95℃ on the heating table for a period of time, pour polyethylene glycol (PEG-400) as a gel accelerator. If the preparation amount is less than 200mg, ensure that the molar ratio of PEG-400 to citric acid is 1.5:1. If the preparation amount is increased, according to the amount of the prepared sample, appropriately reduce the amount of PEG-400, and still need to ensure that the mixture is stirred at 95℃ for a period of time until the water evaporates to form a colloid. If the sample is prepared in small quantities, it needs to be poured into a crucible, while a large amount of sample is still placed in a beaker. The preset temperature of the heating furnace can be adjusted to 110°C and the preparation is continued until the gel appears clear and dark in color. Then the preset temperature is adjusted to 130°C and the preparation is continued until a large number of pores appear and a dry gel is formed. After that, it is calcined at 950°C in a muffle furnace for 4 hours together with the crucible to ensure that the generated gas is completely discharged. The calcined powder is then crushed and ground to obtain the final Ni x Co 1-x Fe2O4 powder. In addition, physically doped materials are mixed and ground by weighing the specified oxide molar ratio. For example, 20% CoO doped NiFe2O4 is mixed in the ratio of CoO:NiFe2O4=1:4.

[0030] The specific steps for preparing oxygen carrier-loaded porous ceramic materials are as follows: first, take a polyurethane foam with a diameter of 60 mm, a thickness of 40 mm, and 10 PPI, soak it in a 20% sodium hydroxide solution for 3 hours, and heat it in a water bath at 60°C to remove the diaphragm, add 60 g SiC to 34 mL of a binder (10% (mass) aluminum dihydrogen phosphate, 0.5% (mass) PVA, 0.5% (mass) CMC) solution to form a slurry with a solid-liquid mass ratio of 7:4, immerse the polyurethane foam in the slurry, squeeze it repeatedly, and blow out excess slurry to ensure that the pores are visible and no slurry flows out. The block material is placed in a drying oven and dried at 100°C for 24 hours. After drying, it is placed in a muffle furnace and sintered to form a porous ceramic material. The heating process is 1°C / min to 600°C for 60 minutes, 3°C / min to 1050°C, 1°C / min to 1300 degrees for 30 minutes, 4°C / min to 1500 degrees for 120 minutes, and finally cooled to room temperature with the furnace to obtain a porous ceramic skeleton material.

[0031] Nano-iron-cobalt-nickel oxygen carriers were added into water and stirred continuously to form a suspension with a solid-liquid ratio of 1:2. The suspension was impregnated and loaded onto the porous skeleton and placed in a drying oven at 100°C for 24 hours to obtain a porous loading material Ni for solar fuel preparation. 0.8 Co 0.2 Fe2O4@SiC.

[0032] The oxygen carrier-loaded porous ceramics were placed in a solar thermochemical reactor to convert CO2 into CO at high temperature in a two-step process. 0.8 Co 0.2 The test results of Fe2O4 loaded on SiC porous skeleton materials are as follows Figure 1 and 2 As shown, it can be seen that with the increase of the number of cycles, the load Ni 0.8 Co 0.2 The CO yield of Fe2O4 oxygen carrier material does not decrease significantly, and it has a higher CO yield at a high cycle number. Figure 3 The oxidation process of two materials synthesized by physical grinding and sol-gel methods with CO2 after high-temperature reduction is described, and the CO production is calculated by integration. The highest cycle CO production is 312mL, and the average CO2 conversion rate per cycle is 5.2%. Ni 0.8 Co 0.2 The CO production of Fe2O4 materials in each cycle is relatively close, indicating the stability of the oxygen carrier material synthesized by the sol-gel method in thermal catalytic CO2 conversion.

Claims

1. A method for preparing a porous support material for preparing solar fuel, characterized in that: The following steps are involved: Step 1: Follow Ni 0.8 Co 0.2 The stoichiometric ratio of Fe2O4 is as follows: Fe(NO3)3, Ni(NO3)2 and Co(NO3)2 hydrates are weighed respectively, deionized water is added, stirred evenly, and then a chelating agent is added, stirred evenly, and then stirred at 95°C for a period of time, a gel accelerator is poured in, and stirring is continued at 95°C until a colloid is formed, and then heated at 110°C until the gel becomes clear and deepens in color, and then heated at 110°C until a large number of pores appear, and then calcined until the gas is completely discharged, crushed, and ground to obtain Ni 0.8 Co 0.2 Fe2O4 powder; Step 2: Soak the polyurethane foam in sodium hydroxide solution for 3 hours and heat it in a water bath at 60°C to remove the diaphragm in the middle of the reticular polyurethane foam. Add SiC or Si3N4 powder into the binder solution to make slurry. The treated polyurethane foam is immersed in the slurry, and then squeezed repeatedly, and the excess slurry is blown out to ensure that the pores are visible and no slurry flows out, and then dried, sintered in stages, and cooled to room temperature with the furnace to obtain a porous ceramic skeleton material; Step 3: Ni obtained in step 1 x Co 1-x Fe2O4 powder is added into water, stirred continuously to form a suspension, impregnated and loaded on the porous skeleton, and dried to obtain the porous loading material; Wherein, in step 2, the binder solution is composed of 10% (mass) aluminum dihydrogen phosphate, 0.5% (mass) PVA, 0.5% (mass) CMC and water.

2. The method according to claim 1, characterized in that: The chelating agent is citric acid, and the gelling accelerator is polyethylene glycol PEG-400.

3. The method according to claim 1, characterized in that: In step 1, calcination is performed at 950°C for 4 hours.

4. The method according to claim 1, characterized in that: In step 1, the molar ratio of the total cation moles of the three metal ions to the chelating agent is 1:2.

5.

5. The method according to claim 1, characterized in that: The pore size of the polyurethane foam in step 2 is 10 PPI, and the mass percentage concentration of the sodium hydroxide solution is 20%.

6. The method according to claim 1, characterized in that: In step 2, 60 g SiC (or Si3N4) powder is added to 34 mL of binder solution to prepare the slurry.

7. The method according to claim 1, characterized in that: In step 2, the solid-liquid mass ratio is 7:4 and the treated polyurethane foam is immersed in the slurry.

8. The method according to claim 1, characterized in that: The sintering process in step 2 is divided into stages: 1°C / min to 600°C for 60 min, 3°C / min to 1050°C, 1°C / min to 1300°C for 30 min, and 4°C / min to 1500°C for 120 min.

9. The method according to claim 1, characterized in that: Step 3: Ni obtained in step 1 is added at a solid-liquid ratio of 1:2 x Co 1-x Fe2O4 powder was added into water.

10. A porous support material prepared by the method according to any one of claims 1 to 9 for solar thermochemistry and solar photothermochemical decomposition of CO2 and H2O.

Citation Information

Patent Citations

  • Method for preparing Co1-xNixFe2O4 magnetic nano-powder by solvothermal method

    CN101891483A

  • Titanium oxide coating / foam silicon carbide structure catalytic carrier and preparation method thereof

    CN103357443A

  • Foamed ceramic for catalyst carriers and preparation and application methods thereof

    CN109665821A

  • Synthesis method of magnetic triazinyl covalent bond organic framework material and application of magnetic triazinyl covalent bond organic framework material in dye wastewater adsorption

    CN111468075A

  • Processing of high surface area oxides

    US20110152068A1

Cited By

  • Y0. 4Sr0. 6MnO3 perovskite porous loading material as well as synthesis method and application thereof

    CN119588390A

  • Y 0.4 Sr 0.6 MnO3 perovskite porous support material, method of synthesis and use thereof

    CN119588390B

  • Multi-element metal-based catalyst as well as preparation method and application thereof

    CN121016765A