Fe-doped SBA-15 / Y 2 O 3 Composite catalyst and its preparation method and application

By doping Fe-doped SBA-15/Y2O3 composite catalyst, the Schottky barrier and Z-scheme heterojunction are formed, which solves the problem of low efficiency of existing photocatalysts and electrocatalysts in wastewater treatment, and realizes the High-efficiency wastewater treatment improves the redox capacity and photocatalytic activity of the catalyst.

CN118767971BActive Publication Date: 2024-11-19WEIFANG UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411268864.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-19
Estimated Expiration
2044-09-11

AI Technical Summary

Technical Problem

The existing photocatalysts and electrocatalysts have problems such as poor visible light response and easy recombination of photogenerated electron-hole pairs in wastewater treatment, which limits their efficiency. The effectiveness of electrocatalytic technology is highly dependent on the selection of electrode materials, resulting in practical applications. Not effective.

Method used

Fe-doped SBA-15/Y2O3 composite catalyst is used to form Schottky barrier and Z-scheme heterojunction through Fe doping, which improves the redox capacity and photocatalytic efficiency of the catalyst, and utilizes the high specific surface area of ​​SBA-15 and The pore structure serves as a carrier to achieve effective separation of photogenerated carriers.

Benefits of technology

The efficiency of wastewater treatment is significantly improved under visible light, better visible light response and photogenerated carrier separation efficiency are achieved, the redox capacity of the catalyst is enhanced, and the separation of photoelectrons and holes in semiconductors is promoted.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767971B_ABST
    Figure CN118767971B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of composite catalysts and their preparation and application, and particularly relates to Fe-doped SBA-15 / Y 2 O 3 Composite catalyst and its preparation method and application. The Fe-doped SBA-15 / Y 2 O 3 The preparation method of the composite catalyst comprises the following steps: firstly, Fe(NO 3 ) 3 •9H 2 O is dissolved in an organic solvent, and then SBA‑15 molecular sieve is added, stirred, the organic solvent is evaporated, ground, and calcined at elevated temperatures to obtain Fe-doped SBA‑15, and then the Fe-doped SBA‑15 is dissolved in an organic solvent, and finally Y(NO 3 ) 3 6H 2 O, stirring, evaporating the organic solvent, grinding, heating and calcining to obtain Fe-doped SBA‑15 / Y 2 O 3 Composite catalyst. The present invention provides Fe-doped SBA-15 / Y 2 O 3 The composite catalyst can degrade wastewater under visible light and has good treatment effect. The invention also provides a preparation method thereof.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite catalysts and preparation and application thereof, and specifically relates to an Fe-doped SBA-15 / Y2O3 composite catalyst and a preparation method and application thereof. Background Art

[0002] With the acceleration of industrialization, water pollution is becoming increasingly serious, and the presence of organic pollutants poses a serious threat to the ecological environment and human health. Among the many water pollution treatment technologies, photocatalytic degradation and electrocatalytic technologies have attracted widespread attention due to their significant process advantages and practical value. As a green and efficient wastewater treatment method, photocatalytic technology has attracted widespread attention because it can use light energy to drive chemical reactions under mild conditions to degrade or mineralize organic pollutants. However, traditional photocatalysts such as TiO2 have problems such as poor visible light response and easy recombination of photogenerated electron-hole pairs, which limits their efficiency in practical applications. Electrocatalysis refers to a catalytic effect that accelerates the reaction by charge transfer at the interface of electrodes and electrolytes. This technology has the advantages of avoiding secondary pollution and not requiring the addition of external reagents, and can react at room temperature and pressure. However, the effectiveness of electrocatalytic technology is highly dependent on factors such as the selection of electrode materials and the overpotential applied to the electrodes. Therefore, the research and improvement of electrode materials still needs to be carried out in depth.

[0003] In recent years, improving the performance of photocatalysts by doping transition metals and constructing semiconductor composite structures has become a research hotspot. For example, patent CN106719817A discloses that a yttrium oxide-ferric oxide (Y2O3-Fe2O3) nanocomposite material based on yttrium oxide is prepared by a hydrothermal method, so that Fe2O3 particles are evenly dispersed on the surface of Y2O3. During the photocatalytic reaction, the Y2O3-Fe2O3 nanomaterial can promote the separation of photogenerated electron-hole pairs, thereby improving the reduction rate of Cr(VI) and having good antibacterial properties under visible light, but its visible light separation efficiency is low.

[0004] For example, patent CN103230802A discloses a method for preparing a composite photocatalyst that responds to visible light and a method for removing arsenic from it. The method mainly adopts a sol-gel method to load the active ingredients yttrium and chromium on magnetic expanded perlite to obtain a catalyst that has a good catalytic effect on arsenic and is easy to recycle. Although the response to visible light is enhanced, the degradation effect on organic pollutants in wastewater is poor.

[0005] Therefore, the development of a green, stable and efficient composite catalyst is of great significance for promoting the practical application of photocatalysis and electrocatalysis technologies in wastewater treatment. Summary of the invention

[0006] The technical problem to be solved by the present invention is to overcome the above-mentioned defects of the prior art, provide an Fe-doped SBA-15 / Y2O3 composite catalyst, degrade wastewater under visible light, and have a good treatment effect. The present invention also provides a preparation method thereof.

[0007] The preparation method of the Fe-doped SBA-15 / Y2O3 composite catalyst described in the present invention comprises the following steps: firstly dissolving Fe(NO3)3·9H2O in an organic solvent, then adding SBA-15 molecular sieve, stirring, evaporating the organic solvent, grinding, heating and calcining to obtain Fe-doped SBA-15, then dissolving the Fe-doped SBA-15 in an organic solvent, and finally adding Y(NO3)3·6H2O, stirring, evaporating the organic solvent, grinding, heating and calcining to obtain the Fe-doped SBA-15 / Y2O3 composite catalyst.

[0008] The organic solvent is one of ethanol, methanol, isopropanol and ether.

[0009] The mass ratio of Fe(NO3)3•9H2O to SBA-15 molecular sieve is (1:30)-(1:5).

[0010] In the Fe-doped SBA-15 / Y2O3 composite catalyst, Y2O3 accounts for 2wt%-10wt% of the Fe-doped SBA-15 / Y2O3 composite catalyst.

[0011] The grinding is performed to an average particle size of 100-500 μm.

[0012] The calcination process before obtaining Fe-doped SBA-15 is: heating to 500-650°C at 5°C / min-10°C / min and calcining for 3h-6h; the calcination process before obtaining Fe-doped SBA-15 / Y2O3 composite catalyst is: heating to 500-650°C at 5°C / min-10°C / min and calcining for 3h-8h.

[0013] The SBA-15 molecular sieve is added and stirred for 30 min-60 min.

[0014] Add Y(NO3)3·6H2O and stir for 1h-4h.

[0015] The Fe-doped SBA-15 / Y2O3 composite catalyst is prepared by the preparation method of the Fe-doped SBA-15 / Y2O3 composite catalyst.

[0016] Application of the Fe-doped SBA-15 / Y2O3 composite catalyst: using it to prepare a working electrode to electrochemically degrade wastewater, or adding it to wastewater to degrade the wastewater under photocatalysis.

[0017] The Fe-doped SBA-15 / Y2O3 composite catalyst is used to prepare a working electrode, and wastewater is degraded by electrochemistry. The specific steps are: the prepared Fe-doped SBA-15 / Y2O3 composite catalyst is coated on indium tin oxide glass (ITO: 75×25×1.1mm, 15-25Ω, Sigma-Aldrich Canada) to prepare a working electrode, and the working electrode is used on an electrochemical analyzer. A standard three-electrode cell is used, and the working electrode, calomel reference electrode and platinum wire are used as counter electrodes to study the electrochemical properties of the sample. A 5mV sine wave is used to measure the electrochemical impedance, and the electrolyte is Na2SO4 with a concentration of 0.1mol / L.

[0018] The Fe-doped SBA-15 / Y2O3 composite catalyst is added to wastewater to degrade the wastewater under photocatalysis. The specific steps are as follows: 200 mL of 20 mg / L toluene is used as the target pollutant solution, and then 50-300 mg of the prepared Fe-doped SBA-15 / Y2O3 composite catalyst is added to the target pollutant solution. After stirring in the dark on a magnetic stirrer for 50-100 minutes, the light source is turned on. The light used is provided by a 300W halogen tungsten floodlight, and the filter filters out ultraviolet rays with a wavelength less than 410nm, and the target pollutant solution is degraded under visible light irradiation. Samples are taken every 60 minutes to detect the toluene concentration until degradation under visible light for 180 minutes.

[0019] Specifically, the preparation method of the Fe-doped SBA-15 / Y2O3 composite catalyst comprises the following steps:

[0020] (1) Dissolve 10-30 mg Fe(NO3)3•9H2O in 200-500 mL organic solvent (ethanol, methanol, isopropanol, ether) under magnetic stirring, then add SBA-15 molecular sieve according to the mass ratio of Fe(NO3)3•9H2O to SBA-15 molecular sieve of (1:30)-(1:5), stir for 30 min-60 min, evaporate the organic solvent, grind to a white solid with an average particle size of 100-500 μm, put it into a semi-closed alumina crucible with a lid, and heat it to 500-650°C in a muffle furnace at 5°C / min-10°C / min for calcination for 3 h-6 h to obtain Fe-doped SBA-15;

[0021] (2) dissolving the Fe-doped SBA-15 in an organic solvent (ethanol, methanol, isopropanol, ether) to obtain a mixed precursor solution of the Fe-doped SBA-15;

[0022] (3) Add Y(NO3)3·6H2O to the mixed precursor solution of Fe-doped SBA-15, stir for 1 h-4 h, evaporate the organic solvent, grind to an average particle size of 100-500 μm, put into a semi-closed alumina crucible with a lid, and heat to 500-650°C in a muffle furnace at 5°C / min-10°C / min for calcination for 3 h-8 h to obtain a Fe-doped SBA-15 / Y2O3 composite catalyst; in the Fe-doped SBA-15 / Y2O3 composite catalyst, Y2O3 accounts for 2wt%-10wt% of the Fe-doped SBA-15 / Y2O3 composite catalyst.

[0023] The doping of Fe element in the present invention can not only promote charge transfer by forming a Schottky barrier, but also construct a Z-scheme heterojunction between SBA-15 and Y2O3, further enhance the redox ability of the catalyst, improve the photocatalytic efficiency, and realize the effective separation of photogenerated carriers by compounding with SBA-15, thereby improving the photocatalytic activity. Among them, SBA-15 (hexagonal mesoporous silica) has become the choice of photocatalyst carrier due to its high specific surface area, good pore structure and chemical stability.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] (1) The Fe-doped SBA-15 / Y2O3 composite catalyst prepared by the method of the present invention is used for wastewater treatment under visible light, achieving the synergistic effect of transition metal doping and semiconductor composite, and having better visible light response and separation efficiency of photogenerated carriers.

[0026] (2) The preparation method of the Fe-doped SBA-15 / Y2O3 composite catalyst of the present invention, the doping of Fe promotes the transfer of charges through the formation of Schottky barriers, and Fe, as an electron medium, is committed to forming a Z-scheme heterojunction between SBA-15 and Y2O3, which effectively improves the redox ability of the catalyst and promotes the separation of photoelectrons and holes in the semiconductor. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is the morphology of the Fe-doped SBA-15 / Y2O3 composite catalyst prepared in Example 1. DETAILED DESCRIPTION

[0028] The present invention will be further described below in conjunction with specific embodiments.

[0029] The raw materials and additives used in the following examples and comparative examples are all commercially available products.

[0030] Example 1

[0031] The preparation method of the Fe-doped SBA-15 / Y2O3 composite catalyst comprises the following steps:

[0032] (1) 20 mg of Fe(NO3)3•9H2O was dissolved in 300 mL of ethanol under magnetic stirring, and then SBA-15 molecular sieve was added according to the mass ratio of Fe(NO3)3•9H2O to SBA-15 molecular sieve of 1:10, stirred for 40 min, and the organic solvent was evaporated in air. The solid was ground into a white solid with an average particle size of 100-500 μm, placed in a semi-closed alumina crucible with a lid, and heated to 550°C in a muffle furnace at 8°C / min for 4 h to obtain Fe-doped SBA-15;

[0033] (2) Dissolving 10 mg of Fe-doped SBA-15 in 300 mL of ethanol to obtain a mixed precursor solution of Fe-doped SBA-15;

[0034] (3) According to the fact that Y2O3 accounts for 2wt% of the Fe-doped SBA-15 / Y2O3 composite catalyst, Y(NO3)3·6H2O was added to the mixed precursor solution of Fe-doped SBA-15, and the mixture was stirred for 3 h. The organic solvent was evaporated and the mixture was ground to an average particle size of 100-500 μm. The mixture was placed in a semi-closed alumina crucible with a lid, and the temperature was increased to 550°C at 8°C / min in a muffle furnace and calcined for 6 h to obtain a Fe-doped SBA-15 / Y2O3 composite catalyst.

[0035] Example 2

[0036] This embodiment is the same as embodiment 1, except that the Y2O3 content in the Fe-doped SBA-15 / Y2O3 composite catalyst in step (3) is replaced by 4wt% from 2wt%.

[0037] Example 3

[0038] This embodiment is the same as embodiment 1, except that the Y2O3 content in the Fe-doped SBA-15 / Y2O3 composite catalyst in step (3) is replaced by 6wt% from 2wt%.

[0039] Example 4

[0040] This embodiment is the same as embodiment 1, except that the proportion of Y2O3 in the Fe-doped SBA-15 / Y2O3 composite catalyst in step (3) is replaced by 8wt% of the 2wt% of the Fe-doped SBA-15 / Y2O3 composite catalyst.

[0041] Example 5

[0042] This embodiment is the same as embodiment 1, except that the 2 wt % of Y2O3 in the Fe-doped SBA-15 / Y2O3 composite catalyst in step (3) is replaced by 10 wt %.

[0043] Example 6

[0044] The preparation method of the Fe-doped SBA-15 / Y2O3 composite catalyst comprises the following steps:

[0045] (1) 10 mg of Fe(NO3)3•9H2O was dissolved in 200 mL of organic solvent methanol under magnetic stirring, and then SBA-15 molecular sieve was added according to the mass ratio of Fe(NO3)3•9H2O to SBA-15 molecular sieve of 1:20, stirred for 50 min, the organic solvent was evaporated, and the solid was ground into a white solid with an average particle size of 100-500 μm. The solid was placed in a semi-closed alumina crucible with a lid, and the temperature was increased to 650°C in a muffle furnace at 5°C / min and calcined for 3 h to obtain Fe-doped SBA-15;

[0046] (2) dissolving the Fe-doped SBA-15 in an organic solvent, methanol, to obtain a mixed precursor solution of the Fe-doped SBA-15;

[0047] (3) According to the fact that Y2O3 accounts for 2wt% of the Fe-doped SBA-15 / Y2O3 composite catalyst, Y(NO3)3·6H2O was added to the mixed precursor solution of Fe-doped SBA-15, and the mixture was stirred for 4 h. The organic solvent was evaporated and the mixture was ground to an average particle size of 100-500 μm. The mixture was placed in a semi-closed alumina crucible with a lid, and the temperature was increased to 650°C in a muffle furnace at a rate of 5°C / min and calcined for 3 h to obtain a Fe-doped SBA-15 / Y2O3 composite catalyst.

[0048] Example 7

[0049] The preparation method of the Fe-doped SBA-15 / Y2O3 composite catalyst comprises the following steps:

[0050] (1) 30 mg of Fe(NO3)3•9H2O was dissolved in 500 mL of organic solvent isopropanol under magnetic stirring, and then SBA-15 molecular sieve was added according to the mass ratio of Fe(NO3)3•9H2O to SBA-15 molecular sieve of 1:5, stirred for 30 min, the organic solvent was evaporated, and the solid was ground into a white solid with an average particle size of 100-500 μm. The solid was placed in a semi-closed alumina crucible with a lid, and the temperature was increased to 500°C in a muffle furnace at 10°C / min and calcined for 6 h to obtain Fe-doped SBA-15;

[0051] (2) dissolving the Fe-doped SBA-15 in an organic solvent, isopropanol, to obtain a mixed precursor solution of the Fe-doped SBA-15;

[0052] (3) According to the fact that Y2O3 accounts for 2wt% of the Fe-doped SBA-15 / Y2O3 composite catalyst, Y(NO3)3·6H2O was added to the mixed precursor solution of Fe-doped SBA-15, and the mixture was stirred for 4 h. The organic solvent was evaporated and the mixture was ground to an average particle size of 100-500 μm. The mixture was placed in a semi-closed alumina crucible with a lid, and the mixture was heated to 500°C at a speed of 10°C / min in a muffle furnace and calcined for 8 h to obtain a Fe-doped SBA-15 / Y2O3 composite catalyst.

[0053] Example 8

[0054] The preparation method of the Fe-doped SBA-15 / Y2O3 composite catalyst comprises the following steps:

[0055] (1) 10 mg of Fe(NO3)3•9H2O was dissolved in 250 mL of organic solvent ether under magnetic stirring, and then SBA-15 molecular sieve was added according to the mass ratio of Fe(NO3)3•9H2O to SBA-15 molecular sieve of 1:30, stirred for 60 min, the organic solvent was evaporated, and the solid was ground into a white solid with an average particle size of 100-500 μm. The solid was placed in a semi-closed alumina crucible with a lid, and the temperature was increased to 600 °C in a muffle furnace at 6 °C / min and calcined for 5 h to obtain Fe-doped SBA-15;

[0056] (2) dissolving the Fe-doped SBA-15 in an organic solvent, ether, to obtain a mixed precursor solution of the Fe-doped SBA-15;

[0057] (3) According to the fact that Y2O3 accounts for 2wt% of the Fe-doped SBA-15 / Y2O3 composite catalyst, Y(NO3)3·6H2O was added to the mixed precursor solution of Fe-doped SBA-15, and the mixture was stirred for 2 h. The organic solvent was evaporated and the mixture was ground to an average particle size of 100-500 μm. The mixture was placed in a semi-closed alumina crucible with a lid, and the temperature was increased to 600°C in a muffle furnace at a rate of 6°C / min and calcined for 6 h to obtain a Fe-doped SBA-15 / Y2O3 composite catalyst.

[0058] Comparative Example 1

[0059] The preparation method of the SBA-15 / Y2O3 composite catalyst comprises the following steps:

[0060] (1) According to the fact that Y2O3 in the SBA-15 / Y2O3 composite catalyst accounts for 2wt% of the SBA-15 / Y2O3 composite catalyst, SBA-15 is dissolved in ether, an organic solvent, to obtain a mixed precursor solution of SBA-15;

[0061] (3) Add Y(NO3)3·6H2O to the mixed precursor solution of SBA-15 and stir for 2 h. Evaporate the organic solvent and grind to an average particle size of 100-500 μm. Place the mixture in a semi-closed alumina crucible with a lid and heat to 600 °C in a muffle furnace at 6 °C / min and calcine for 6 h to obtain an SBA-15 / Y2O3 composite catalyst.

[0062] Comparative Example 2

[0063] The preparation method of the Fe-doped SBA-15 composite catalyst comprises the following steps:

[0064] 20 mg of Fe(NO3)3•9H2O was dissolved in 300 mL of ethanol under magnetic stirring, and then SBA-15 molecular sieve was added at a mass ratio of Fe(NO3)3•9H2O to SBA-15 molecular sieve of 1:10, stirred for 40 minutes, and the organic solvent was evaporated in the air. The solid was ground into a white solid with an average particle size of 100-500 μm, placed in a semi-closed alumina crucible with a lid, and heated to 550°C at 8°C / min in a muffle furnace and calcined for 4 hours to obtain an Fe-doped SBA-15 composite catalyst.

[0065] Comparative Example 3

[0066] The preparation method of the Fe-doped Al2O3 / Y2O3 composite catalyst comprises the following steps:

[0067] (1) 20 mg of Fe(NO3)3•9H2O was dissolved in 300 mL of ethanol under magnetic stirring, and then Al2O3 was added according to the mass ratio of Fe(NO3)3•9H2O to alumina of 1:10, stirred for 40 min, and the organic solvent was evaporated in air. The solid was ground into a white solid with an average particle size of 100-500 μm, placed in a semi-closed alumina crucible with a lid, and calcined at 550°C in a muffle furnace at 8°C / min for 4 h to obtain Fe-doped Al2O3;

[0068] (2) Dissolve 10 mg of Fe-doped Al2O3 in 300 mL of ethanol to obtain a mixed precursor solution of Fe-doped Al2O3;

[0069] (3) According to the fact that Y2O3 accounts for 2wt% of the Fe-doped Al2O3 / Y2O3 composite catalyst, Y(NO3)3·6H2O is added to the mixed precursor solution of Fe-doped Al2O3, and the mixture is stirred for 3 h. The organic solvent is evaporated and the mixture is ground to an average particle size of 100-500 μm. The mixture is placed in a semi-closed alumina crucible with a lid, and the mixture is heated to 550°C at a rate of 8°C / min in a muffle furnace and calcined for 6 h to obtain a Fe-doped Al2O3 / Y2O3 composite catalyst.

[0070] The catalysts of Examples 1-8 and Comparative Examples 1-3 were subjected to performance tests, and the test results are shown in Table 1.

[0071] Table 1 Catalyst performance results

[0072]

[0073] The above Examples 1-8 and Comparative Examples 1-3 were subjected to the following two applications:

[0074] (I) The prepared catalyst was used to prepare a working electrode, and the wastewater was degraded by electrochemistry. The specific steps are as follows: the prepared catalyst was coated with ITO glass with dimensions of 8 mm in length, 15 mm in width, and 1.1 mm in thickness. A working electrode was prepared on indium tin oxide glass (ITO: 8×15×1.1 mm, 15-25Ω, Sigma-Aldrich Canada), and the electrochemical analyzer was used to study the electrochemical properties of the sample (degradation of 100 mL 20 mg / L toluene solution C0) using a standard three-electrode cell, a working electrode, a calomel reference electrode, and a platinum wire as a counter electrode. A 5mV sine wave was used to measure the electrochemical impedance, and the electrolyte was Na2SO4 with a concentration of 0.1 mol / L. The concentration of the toluene solution after 3 hours was measured. t According to the degradation rate formula, the degradation rate η is calculated, and the results are shown in Table 2. Degradation rate calculation formula:

[0075] ;

[0076] η is the degradation efficiency of toluene, C0 and C t are the initial concentration of toluene and the concentration at time t (t=3h) respectively.

[0077] Table 2 Results of electrochemical degradation of wastewater

[0078]

[0079] (ii) Add the catalyst to the wastewater and degrade the wastewater under photocatalysis. The specific steps are as follows: 200mL of toluene with a concentration of 20mg / L is used as the target pollutant solution, and then 50mg of the prepared catalyst is added to the target pollutant solution. After stirring in the dark on a magnetic stirrer for 60min, the light source is turned on. The light used is provided by a 300W halogen tungsten floodlight. The filter filters out ultraviolet rays with a wavelength less than 410nm, and the target pollutant solution is degraded under visible light. Take a sample every 60min to detect its toluene concentration until it degrades under visible light for 180min, and record the first (60min) sampling concentration, the second (120min) sampling concentration, and the third (180min) sampling concentration respectively. The results are shown in Table 3.

[0080] Table 3 Test results

[0081]

[0082] As can be seen from Table 1, the average bulk density, average specific surface area, average pore volume, and average pore size of the composite oxygen carrier prepared by the present invention are all relatively large, the crushing strength is relatively large, and the catalytic performance of the composite oxygen carrier prepared is good. As can be seen from Tables 2 and 3, when the composite oxygen carrier prepared by the present invention is applied to the decomposition of toluene, the decomposition conversion rate is high and the oxidative decomposition performance is strong.

Claims

1. A method for preparing a Fe-doped SBA-15 / Y2O3 composite catalyst, characterized in that: The following steps are involved: First, Fe(NO3)3·9H2O is dissolved in an organic solvent, then SBA-15 molecular sieve is added, stirred, the organic solvent is evaporated, ground, and the temperature is increased to calcine to obtain Fe-doped SBA-15. Then, Fe-doped SBA-15 is dissolved in an organic solvent, and finally Y(NO3)3·6H2O is added, stirred, the organic solvent is evaporated, ground, and the temperature is increased to calcine to obtain a Fe-doped SBA-15 / Y2O3 composite catalyst.

2. The method for preparing the Fe-doped SBA-15 / Y2O3 composite catalyst according to claim 1, characterized in that: The organic solvent is one of ethanol, methanol, isopropanol and ether.

3. The method for preparing the Fe-doped SBA-15 / Y2O3 composite catalyst according to claim 1, characterized in that: The mass ratio of Fe(NO3)3•9H2O to SBA-15 molecular sieve is (1:30)-(1:5).

4. The method for preparing the Fe-doped SBA-15 / Y2O3 composite catalyst according to claim 1, characterized in that: In the Fe-doped SBA-15 / Y2O3 composite catalyst, Y2O3 accounts for 2wt%-10wt% of the Fe-doped SBA-15 / Y2O3 composite catalyst.

5. The method for preparing the Fe-doped SBA-15 / Y2O3 composite catalyst according to claim 1, characterized in that: The grinding is performed to an average particle size of 100-500 μm.

6. The method for preparing the Fe-doped SBA-15 / Y2O3 composite catalyst according to claim 1, characterized in that: The calcination process before obtaining Fe-doped SBA-15 is: heating to 500-650°C at 5°C / min-10°C / min and calcining for 3h-6h; the calcination process before obtaining Fe-doped SBA-15 / Y2O3 composite catalyst is: heating to 500-650°C at 5°C / min-10°C / min and calcining for 3h-8h.

7. The method for preparing the Fe-doped SBA-15 / Y2O3 composite catalyst according to claim 1, characterized in that: The SBA-15 molecular sieve is added and stirred for 30 min-60 min.

8. The method for preparing the Fe-doped SBA-15 / Y2O3 composite catalyst according to claim 1, characterized in that: Add Y(NO3)3·6H2O and stir for 1h-4h.

9. An Fe-doped SBA-15 / Y2O3 composite catalyst, characterized in that: The catalyst is prepared by the preparation method of the Fe-doped SBA-15 / Y2O3 composite catalyst described in any one of claims 1 to 8.

10. An application of the Fe-doped SBA-15 / Y2O3 composite catalyst according to claim 9, characterized in that: It is used to prepare a working electrode to electrochemically degrade wastewater, or it is added to wastewater to degrade the wastewater under photocatalysis.