Magnetic separation-electric separation process for complex refractory iron ore
Through the all-dry separation process combined with staged dry grinding, magnetic separation and electric separation, the problem of separation of siderite, limonite and chlorite in complex and difficult-to-separate iron ore is solved, and the recovery of high-grade iron concentrate is realized. The process is simplified and environmental protection costs are reduced, and tailings wet discharge and environmental pollution are avoided.
Patent Information
- Application Number
- CN202410645129.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-10-10
- Filing Date
- 2024-05-23
- Publication Date
- 2024-10-15
AI Technical Summary
It is difficult for the existing technology to effectively process complex and difficult-to-separate iron ores with low grade, complex composition, and fine particle size, especially siderite, limonite, chlorite and other easily muddy minerals, resulting in poor flotation effect, and Traditional processes have problems with high energy consumption, carbon emissions and pollution.
The fully dry separation process is adopted to separate magnetite and weakly magnetic minerals through a combination of staged dry grinding, magnetic separation and electric separation. The difference in magnetic and electrical properties is used to achieve high-grade recovery of iron concentrate and avoid floating. The use of selection technology simplifies the process and reduces environmental protection costs.
It achieves the separation of high-grade iron concentrate, shortens the process flow, avoids wet discharge of tailings, reduces environmental protection costs, improves the pelletizing performance of iron concentrate, and solves the problems of poor flotation indicators and environmental pollution in traditional processes. question.
Smart Images

Figure CN118768079A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of mineral processing, and in particular to a magnetic separation-electric separation process for complex and difficult-to-separate iron ore. Background Art
[0002] With the continuous exploitation of iron ore resources around the world, the quality of ore has been declining year by year, showing the pattern of lower grade, more complex composition, and finer embedded particle size. At present, there are many complex and difficult-to-select iron ore belts in the world, such as Liaoning and Shanxi in China, the Appalachian geosyncline iron ore belt in North America, the Lorraine-Germany Salkangit belt in France, the Kachkanal iron ore belt in Russia, and the Carrara area in Australia. The iron ore in these production areas is of low grade and complex type, mainly magnetite or hematite, and also contains a variety of iron-containing minerals such as siderite, limonite, chlorite, and gangue such as quartz and calcite. In addition, the above minerals often coexist with each other and need to be ground to very fine particle size before they can be completely separated into monomers.
[0003] Among the above-mentioned minerals, siderite (FeCO3), limonite and chlorite are weakly magnetic minerals with low hardness and easy to be muddied (Mohs hardness <4.0). In the traditional wet "grinding-magnetic separation-flotation" process, they cannot be separated by strong magnetic separation and enter the flotation operation, resulting in a large amount of fine mud and calcium and magnesium ions in the ore pulp, reducing the selectivity of the reagent, seriously deteriorating the flotation process, and making it difficult for the flotation process to obtain better sorting indicators.
[0004] Taking the iron ore produced in Anshan, China as an example, its FeCO3 content is constantly increasing, and in some mining areas it has reached more than 10%. However, the current ore dressing plant adopts a combined process of "stage grinding, coarse and fine grading, gravity separation-magnetic separation-anion reverse flotation" that is difficult to handle such iron ore with high carbonate content. The flotation index has dropped seriously, and even the phenomenon of indistinguishability between the concentrate and the tail has occurred. The mining site has to blend the iron ore from each mining area to reduce the ferrous carbonate content in the selected material to below 3%.
[0005] For example, the patent document with publication number CN106944248A discloses a "method for beneficiating mixed iron ore containing high carbonate". This method grinds the raw ore, performs weak magnetic separation and strong magnetic separation, obtains weak magnetic separation iron concentrate and strong magnetic separation iron concentrate, and screens the strong magnetic separation iron concentrate through a fine screen to obtain qualified iron concentrate under the screen; the product on the screen is fed into a pre-classification-regrinding-strong magnetic separation process to obtain a strong magnetic separation coarse concentrate; the strong magnetic separation coarse concentrate is fed into a positive flotation operation to obtain a positive flotation iron concentrate. The patent document with publication number CN104014416B discloses a "method for separating carbonate-containing iron ore". This method crushes the carbonate-containing iron ore, performs staged ball milling, and performs strong-weak magnetic separation to obtain a magnetic separation mixed concentrate, and then performs classification to obtain coarse and fine products, and finally performs reverse flotation to obtain a coarse-grained concentrate and a fine-grained concentrate. Both of the above methods use flotation combined with magnetic separation or gravity separation to process mixed iron ore. When the content of weak magnetic minerals such as siderite, limonite, chlorite and other easily sludged iron ore raw materials is high, the above methods cannot obtain good flotation indicators. The "micro-fine iron mineral collector and carbonate-containing iron ore coarse and fine asynchronous flotation method" disclosed in the publication number CN113680534A, this method coarsely and finely classifies the mixed magnetic concentrate obtained by strong magnetic separation and weak magnetic separation to obtain coarse and fine products, and then uses different collectors to reverse float the coarse particle level, and performs positive flotation on the fine particle level, and obtains flotation concentrates respectively. This method can obtain better indicators than the conventional magnetic separation-flotation process, but the steps are complicated, the process is long, the amount and type of flotation reagents are large, and the siderite content treated by this method is less than 6%, and other complex components such as chlorite and limonite are not found in the embodiment. For example, the “ore dressing method for high-carbonate refractory iron ore” disclosed in publication number CN113877851A, and the “low-temperature hydrogen reduction magnetic roasting process for refractory iron ore” disclosed in publication number CN108950179A, both use the method of magnetic roasting to convert weakly magnetic siderite into strongly magnetic hematite, and then perform magnetic separation and recovery to prevent it from entering the flotation operation and affecting the indicators. Although the above methods can effectively process iron ore with high iron carbonate content, they have problems such as high energy consumption and carbon emissions. At the same time, they cannot process refractory iron ore containing other complex components such as chlorite.
[0006] Therefore, it is urgent to develop new separation process flow for complex and difficult-to-separate iron ore to achieve its green and efficient utilization. Summary of the invention
[0007] In view of the problems of complex and difficult-to-select iron ore with fine embedded particle size, containing easily muddy minerals, and poor flotation effect, the present invention provides a magnetic separation-electric separation process for complex and difficult-to-select iron ore, which utilizes the magnetic difference of the ore to separately select magnetite through weak magnetic separation; utilizes the differences in electrical properties such as dielectric constant, electrical conductivity, and rectification of the ore to separate siderite, limonite, chlorite and other minerals that are easily muddy but have poor conductivity among weakly magnetic minerals from hematite, so as to obtain high-grade iron concentrate.
[0008] To achieve the above object, the present invention adopts the following technical solutions:
[0009] A magnetic separation-electric separation process for complex and difficult-to-separate iron ore adopts a "staged dry grinding, magnetic separation-electric separation" fully dry separation process flow, specifically, the complex mixed iron ore is crushed and roller-milled to obtain a magnetic separation feed product, the magnetic separation feed product is subjected to dry weak magnetic separation I, and the concentrate is subjected to grinding operation dry grinding a, wind classification operation, and multi-stage dry weak magnetic separation operation to obtain a magnetite concentrate; the dry weak magnetic separation I tailings are fed into a coarse-grained dry strong magnetic operation dry strong magnetic I, and the obtained coarse-grained strong magnetic concentrate is further subjected to grinding operation dry grinding b, wind classification, and dry strong magnetic operation, and the concentrate enters a multi-stage electric separation operation to obtain a hematite concentrate; the complex mixed iron ore contains magnetite, hematite, siderite, limonite, and chlorite.
[0010] The specific steps include:
[0011] 1) The complex mixed ore crushing product is fed into the high pressure roller mill as the raw ore, and forms a closed-circuit grinding system with the screening operation to obtain the magnetic separation feed product.
[0012] 2) The magnetic separation product of step 1) is fed into the coarse-grained dry weak magnetic separation operation dry weak magnetic I, wherein the concentrate enters the next grinding operation dry grinding a; the tailings are fed into the coarse-grained dry strong magnetic operation dry strong magnetic I, the coarse-grained strong magnetic tailings are discarded, and the obtained coarse-grained strong magnetic concentrate enters the next grinding operation dry grinding b.
[0013] Dry weak magnetic I tailings contain iron-containing weak magnetic minerals, including hematite, siderite, limonite and chlorite.
[0014] 3) Dry grinding a and wind classification operation form a closed-circuit grinding system to obtain fine-grained products with a particle size of -200 mesh accounting for more than 60%, and the specific fineness depends on the degree of ore dissociation. Then several stages of dry weak magnetic separation operations are carried out to obtain high-grade magnetite concentrate with TFe ≥ 66.5%; the middlings of each stage of dry weak magnetic separation operation are returned to the previous stage in turn, and the tailings are merged and discarded.
[0015] Dry grinding methods include dry ball milling, dry autogenous grinding, and dry stirred milling; the number of dry weak magnetic separation stages, magnetic field strength, etc. should be determined according to the actual ore properties and concentrate grade requirements. Generally, wind-powered dry magnetic separators are used, with 3 to 5 process stages.
[0016] 4) Combine dry grinding b with wind classification operation to form a closed-circuit grinding system to obtain fine-grained products with a particle size of -200 mesh accounting for more than 60%, and the specific fineness depends on the degree of ore dissociation. Then carry out several stages of dry strong magnetic operation, in which the concentrate enters the electric separation operation and the tailings are discarded.
[0017] Dry grinding methods include dry ball milling, dry autogenous grinding, and dry stirred milling; the number of dry high-intensity magnetic separation operation stages, magnetic field strength, etc. should be determined according to the actual ore properties and concentrate grade requirements. Generally, a dry vibrating high-gradient magnetic separator is used, with 1 to 3 stages of operation.
[0018] 5) The dry strong magnetic concentrate of step 4) is subjected to several stages of electrostatic separation to obtain a high-grade hematite concentrate with TFe≥65%; the middlings of each stage of electrostatic separation and the tailings of the next stage of electrostatic separation are returned to the feed ore in sequence.
[0019] The total content of siderite, limonite and chlorite in the hematite concentrate is less than 1% by weight.
[0020] The number of electrostatic separation operation stages, voltage (electric field) intensity, etc. should be determined according to the actual ore properties and concentrate grade requirements. Generally, a high-voltage electrostatic separator is used, with 2 to 4 process stages.
[0021] 6) Combine the tailings from dry weak magnetic separation operations, dry strong magnetic tailings, and electrostatic separation tailings into comprehensive tailings.
[0022] A magnetic separation-electric separation process for complex and difficult-to-separate iron ore adopts a "magnetic-electric-flotation" combined separation process flow, specifically, the complex mixed iron ore is crushed and roller-milled, and then subjected to grinding and screening to obtain a graded overflow product, the overflow product is fed to a weak magnetic pre-separation operation, and the resulting concentrate enters a weak magnetic concentration operation to obtain a magnetite concentrate; the tailings from the weak magnetic pre-separation operation enter a strong magnetic separation operation, and the resulting strong magnetic concentration concentrate is fed to an electric separation operation after drying, and the electric separation operation concentrate is subjected to reverse flotation and scavenging operations to obtain a magnetic-hematite mixed concentrate; the tailings from the weak magnetic concentration operation and the concentrate from the electric separation operation are combined and entered into reverse flotation and scavenging operations; the complex mixed iron ore contains magnetite, hematite, siderite, limonite, and chlorite.
[0023] The specific steps include:
[0024] 1) The product of the complex mixed iron ore after crushing roller mill is fed into the grinding and screening operation as the raw ore to obtain a fine-grained overflow product with a particle size of -200 mesh accounting for more than 60%. The specific fineness depends on the degree of ore dissociation. The grinding methods of the grinding and screening operation include single grinding or a combination of multiple grinding methods among high-pressure roller mill, ball mill and stirred mill.
[0025] 2) The overflow product is fed into the weak magnetic pre-selection process, the resulting concentrate enters the multi-stage weak magnetic concentration process, and the tailings enter the strong magnetic separation process.
[0026] The weak magnetic pre-selection equipment is a wet drum magnetic separator, and the magnetic field strength should be determined according to the specific properties of the material and the concentrate grade requirements.
[0027] The weak magnetic concentration equipment selects one or more combinations of wet drum magnetic separators, elutriators, and magnetic vibration machines. The magnetic field strength during sorting should be determined according to the specific properties of the material and the concentrate grade requirements; the number of stages for weak magnetic concentration operations can be determined according to the actual ore properties, and generally 3 to 5 stages are set.
[0028] 3) The concentrated ore obtained from the high-intensity magnetic separation operation is dried and then fed into the electric separation operation, and the tailings are discarded.
[0029] For high-intensity magnetic separation, a high-gradient magnetic separator (such as the SLon series) is selected. Parameters such as the magnetic field strength should be determined according to the specific properties of the material and the concentrate grade requirements. The number of sections for high-intensity magnetic separation can be determined according to the actual ore properties, and is generally set to 1 to 2 sections.
[0030] A high-voltage drum-type electric separator is selected for electric separation operations. Parameters such as voltage (electric field) intensity should be determined according to the specific properties of the material and the concentrate grade requirements. The number of sections for electric separation operations can be determined according to the actual properties of the ore, and is generally set to 1 to 3 sections.
[0031] 4) The concentrate obtained from the electrostatic separation operation is fed into the reverse flotation operation, the tailings are discarded or subjected to magnetization roasting and other treatments, and the middlings are returned to the electrostatic separation operation for re-selection. The total content of siderite, limonite and chlorite in the electrostatic separation concentrate is less than 3% by weight.
[0032] 5) After multiple weak magnetic concentration operations, the ore is demagnetized by a demagnetizer between each weak magnetic concentration to obtain a magnetite concentrate with a grade of not less than 66%. The tailings of the multiple weak magnetic concentration operations are combined and fed into the reverse flotation operation.
[0033] 6) The tailings of the multi-stage weak magnetic concentration operation are combined with the concentrate of the electrostatic separation operation, and then subjected to reverse flotation operation to obtain a mixed maghemitic concentrate, the iron grade of which is not less than 67.5%.
[0034] The tailings from the multi-stage weak magnetic concentration operation and the concentrate from the electrostatic separation operation are combined and mixed and then concentrated to control the reverse flotation feed concentration at 40% to 45%.
[0035] The recovery rate of reverse flotation operation shall not be less than 80%.
[0036] 7) Combine the strong magnetic separation tailings, electrostatic separation tailings and reverse flotation sweeping tailings into comprehensive tailings.
[0037] The reagent system for reverse flotation, such as the type and dosage of collectors, depressants and activators, should be determined according to the specific properties of the material and the concentrate grade requirements; the number of reverse flotation operation sections can be determined according to the actual ore properties, generally one coarse, one fine and three sweeps.
[0038] In the iron phase composition of the complex mixed iron ore, FeCO3 is ≥ 3% by weight.
[0039] Compared with the prior art, the present invention has the following beneficial effects:
[0040] 1) The present invention discloses a magnetic separation-electric separation process for complex and difficult-to-separate iron ore. The magnetic difference of the ore is used to first separate the magnetite by weak magnetic separation; then the difference in electrical properties such as the dielectric constant, conductivity, and rectification of the ore is used to separate the siderite, limonite, chlorite and other minerals that are easy to be muddied but have poor conductivity from the hematite in the weak magnetic minerals, and finally a high-grade iron concentrate is obtained.
[0041] 2) The "stage dry grinding, magnetic separation-electric separation" fully dry separation process in the present invention is to separate the strongly magnetic magnetite in the mixed iron ore through weak magnetic separation; and then separate the siderite, limonite, chlorite and other minerals that are easy to mud but have poor conductivity from the weak magnetic minerals through several electric separation operations, and recover the high-grade iron concentrate. The flotation process is not set in the whole process flow, which is a fully dry separation process, and the problems of poor flotation operation indicators, affecting the ball-forming performance of iron concentrate, and polluting the environment are eliminated as a whole. At the same time, through the fully dry operation, the process flow is shortened, the wet discharge of tailings is avoided, the pressure of the tailings pond is relieved, and the environmental protection cost is saved.
[0042] 3) The "magnetic-electric-flotation" combined separation process of the present invention is to separate the strongly magnetic magnetite in the mixed iron ore through weak magnetic separation by "magnetic-electric-flotation" combined separation; then the siderite, limonite, chlorite and other minerals that are easy to be muddy but have poor conductivity in the weak magnetic minerals are pre-separated and discarded by electric separation, and the selected materials are subjected to strong magnetic separation and drying before the electric separation operation. The combined separation process retains the traditional flotation process equipment flow, but reduces the content of easily muddy minerals in the iron ore entering the float, and improves the flotation operation index.
[0043] 4) Compared with the existing process, the method used in the present invention can process more types of minerals in the ore, especially iron ore with a ferrous carbonate content greater than 10%, and can still be effectively processed, thereby achieving efficient development and utilization of complex and difficult-to-select mixed iron ore. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 This is a process flow chart of the "stage dry grinding, magnetic separation-electric separation" fully dry separation process of the present invention (Example 1).
[0045] Figure 2 This is a process flow chart of the "magnetic-electric-floatation" combined separation process of the present invention (Example 5). DETAILED DESCRIPTION
[0046] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only for illustration and are not intended to limit the present invention.
[0047] Embodiment 1:
[0048] like Figure 1 As shown, the complex and difficult-to-select iron ore selected in this implementation case is taken from Anshan, Liaoning, China, with a total iron grade of 24.06%, of which magnetite contains 20.66%, hematite contains 10.15%, siderite (FeCO3) contains 4.15%, chlorite contains 3.12%, and the gangue is mainly quartz and a small amount of mica. The process of the present invention is used for separation, which specifically includes the following steps:
[0049] 1) The complex mixed ore is crushed into fine products of 0-12 mm as raw ore and fed into the high pressure roller mill, and a closed-circuit grinding system is formed with the screening operation to obtain the undersize product with a particle size of P80 = 2.55 mm;
[0050] 2) Feed the under-screen product into the coarse-grained dry weak magnetic separation operation dry weak magnetic I, where the concentrate enters the dry grinding a; and forms a closed-circuit grinding system with the wind classifier to obtain a fine-grained product with a particle size of -200 mesh accounting for 85%;
[0051] 3) The wind-force classified product in step 2) is fed into three-stage dry weak magnetic separation operations (dry weak magnetic II, III, IV), and demagnetized by a demagnetizer between each stage of weak magnetic separation to obtain a magnetite concentrate with a grade of 66.9%;
[0052] 4) Feed the dry weak magnetic I tailings into the dry strong magnetic I, discard the coarse strong magnetic tailings, and the obtained coarse strong magnetic concentrate enters the dry grinding b; together with the wind classification operation, a closed-circuit grinding system is formed to obtain a fine-grained product with a particle size of -200 mesh accounting for 85%, followed by a dry strong magnetic operation (dry strong magnetic II), the obtained concentrate enters the electric separation operation, and the tailings are discarded;
[0053] 5) The concentrate of dry strong magnetic II is subjected to two-stage electrostatic separation to obtain a hematite concentrate with a grade of 67.5%; the total content of siderite, limonite and chlorite in the hematite concentrate is less than 1%.
[0054] 6) Combine the tailings from the dry weak magnetic sections II, III, and IV, the dry strong magnetic tailings, and the electrostatic separation tailings into comprehensive tailings.
[0055] Embodiment 2:
[0056] The complex and difficult-to-select iron ore selected in this implementation case is taken from Anshan, Liaoning Province, with a total iron grade of 33.52%, of which magnetite contains 17.65%, hematite contains 25.11%, siderite (FeCO3) contains 6.55%, chlorite contains 2.36%, and the gangue is mainly quartz and a small amount of feldspar. The process of the present invention is used for separation, which specifically includes the following steps:
[0057] 1) The complex mixed ore is crushed into fine products of 0-12 mm as raw ore and fed into the high pressure roller mill, and a closed-circuit grinding system is formed with the screening operation to obtain the undersize product with a particle size of P80 = 2.55 mm;
[0058] 2) Feed the under-screen product into the coarse-grained dry weak magnetic separation operation dry weak magnetic I, where the concentrate enters the dry grinding a; and forms a closed-circuit grinding system with the wind classifier to obtain a fine-grained product with a particle size of -200 mesh accounting for 85%;
[0059] 3) The wind-force classified product in step 2) is fed into four-stage dry weak magnetic separation operations (dry weak magnetic II, III, IV, V), and demagnetized by a demagnetizer between each stage of weak magnetic separation to obtain a magnetite concentrate with a grade of 67.8%;
[0060] 4) Feed the dry weak magnetic I tailings into the dry strong magnetic I, discard the coarse strong magnetic tailings, and the obtained coarse strong magnetic concentrate enters the dry grinding b; together with the wind classification operation, a closed-circuit grinding system is formed to obtain a fine-grained product with a particle size of -200 mesh accounting for 85%, and then enters two stages of dry strong magnetic operations (dry strong magnetic II, III), the obtained concentrate enters the electric separation operation, and the tailings are discarded;
[0061] 5) The concentrate of dry strong magnetic III is subjected to three-stage electrostatic separation to obtain a hematite concentrate with a grade of 67.7%; the total content of siderite, limonite and chlorite in the hematite concentrate is less than 1%.
[0062] 6) Combine the tailings of dry weak magnetic sections II, III, IV, and V, dry strong magnetic tailings, and electrostatic separation tailings into comprehensive tailings.
[0063] Embodiment 3:
[0064] The complex and difficult-to-select iron ore used in this implementation case was taken from Yuanjia Village, Shanxi Province, China, with a total iron grade of 34.48%, of which magnetite contained 35.78%, hematite contained 8.63%, siderite (FeCO3) contained 5.25%, and chlorite contained 3.74%. The gangue was mainly quartz, containing a small amount of dolomite and calcite, and was selected using the process flow of the present invention.
[0065] 1) The finely crushed product crushed to 0-12 mm is fed into a high-pressure roller mill as the raw ore, and a closed-circuit grinding system is formed with a dry vibrating screen to obtain an undersize product with a particle size of P80 = 2.70 mm;
[0066] 2) Feed the high pressure roller mill product into the dry weak magnetic I, and feed the concentrate of the dry weak magnetic I into the dry mill a, and form a closed-circuit grinding system with the wind classifier to obtain a fine-grained product with a particle size of -200 mesh accounting for 85%;
[0067] 3) The wind-force classified product in step 2) is fed into five-stage dry weak magnetic separation operations (dry weak magnetic II, III, IV, V, VI), and demagnetized by a demagnetizer between each stage of weak magnetic separation to obtain a magnetite concentrate with a grade of 67.7%;
[0068] 4) Feed the tailings of dry weak magnetic I into dry strong magnetic I, discard the coarse strong magnetic tailings, feed the concentrate of dry strong magnetic I into dry grinding B, and form a closed-circuit grinding system with the wind classifier to obtain a fine-grained product with a particle size of -200 mesh accounting for 85%; then enter the dry strong magnetic II, the obtained concentrate enters the electric separation operation, and the tailings are discarded;
[0069] 5) The dry strong magnetic II concentrate is fed into the three-stage electrostatic separation operation to obtain a hematite concentrate with a grade of 66.5%; the total content of siderite, limonite and chlorite in the hematite concentrate is less than 1%.
[0070] 6) The tailings of dry weak magnetic sections II, III, IV, V, VI, dry strong magnetic tailings, and electrostatic separation tailings are combined into comprehensive tailings with a grade of 11.8%.
[0071] Embodiment 4:
[0072] The complex and difficult-to-select iron ore used in this implementation case was taken from Yuanjia Village, Shanxi Province, China, with a total iron grade of 37.09%, of which magnetite contained 11.25%, hematite contained 36.88%, siderite (FeCO3) contained 6.50%, and chlorite contained 4.05%. The gangue was mainly quartz, containing a small amount of dolomite and calcite, and was selected using the process flow of the present invention.
[0073] 1) The finely crushed product crushed to 0-12 mm is fed into a high-pressure roller mill as the raw ore, and a closed-circuit grinding system is formed with a dry vibrating screen to obtain an undersize product with a particle size of P80 = 2.75 mm;
[0074] 2) Feed the high pressure roller mill product into the dry weak magnetic I, and feed the concentrate of the dry weak magnetic I into the dry mill a, and form a closed-circuit grinding system with the wind classifier to obtain a fine-grained product with a particle size of -200 mesh accounting for 85%;
[0075] 3) The wind-force classified product in step 2) is fed into three-stage dry weak magnetic separation operations (dry weak magnetic II, III, IV), and demagnetized by a demagnetizer between each stage of weak magnetic separation to obtain a magnetite concentrate with a grade of 67.5%;
[0076] 4) Feed the tailings of dry weak magnetic I into dry strong magnetic I, discard the coarse strong magnetic tailings, feed the concentrate of dry strong magnetic I into dry grinding b, and form a closed-circuit grinding system with the wind classifier to obtain a fine-grained product with a particle size of -200 mesh accounting for 85%; then enter the three-stage dry strong magnetic operation (dry strong magnetic II, III, IV), the obtained concentrate enters the electric separation operation, and the tailings are discarded;
[0077] 5) The dry strong magnetic concentrate is fed into the three-stage electric separation process to obtain a hematite concentrate with a grade of 66.8%; the total content of siderite, limonite and chlorite in the hematite concentrate is less than 1%.
[0078] 6) Combine the tailings from the dry weak magnetic sections II, III, and IV, the dry strong magnetic tailings, and the electrostatic separation tailings into comprehensive tailings.
[0079] In the embodiments 1-4 of the present invention, the processes from grinding, classification to magnetic separation and electrostatic separation are all fully dry processes, which do not consume water and do not produce wet tailings. Compared with the prior art, the process of the present invention can remove the weakly magnetic minerals such as siderite, limonite, chlorite and other easy-to-mudify weak magnetic minerals in the difficult-to-select mixed iron ore through the electrostatic separation process, and obtain high-grade iron concentrate under dry conditions, which cannot be achieved by the prior art process. In addition, the processes of embodiments 1-4 do not involve flotation operations, which can save the energy consumption of slurry heating and greenhouse gas emissions, and at the same time do not produce chemical pollution, which can eliminate the influence of chemical on the subsequent iron concentrate pelletizing process.
[0080] Embodiment 5:
[0081] like Figure 2 As shown, the complex and difficult-to-select iron ore used in this implementation case was taken from Anshan, Liaoning, China, with a total iron grade of 30.05%, of which, calculated by mass percentage, magnetite contained 15.90%, hematite contained 16.87%, siderite (FeCO3) contained 13.95%, chlorite contained 2.13%, and the gangue was mainly quartz and a small amount of feldspar, and was selected using the process flow of the present invention.
[0082] 1) Feed the high pressure roller mill product with a particle size of ≤3 mm into the ball mill and form a closed circuit grinding system with the cyclone to obtain a product with an overflow particle size of 85% to 95% of -200 mesh.
[0083] 2) The overflow product is fed into a weak magnetic pre-selection operation, and the resulting concentrate is subjected to three stages of weak magnetic concentration operations. Between each stage of weak magnetic selection, it is demagnetized by a demagnetizer to obtain a magnetite concentrate with a grade of 66.45%.
[0084] 3) The tailings from the weak magnetic pre-selection operation are fed into a strong magnetic selection operation, and the tailings from the strong magnetic selection operation are discarded; the strong magnetic selection concentrate is dried and fed into an electrostatic separation operation, and the tailings whose main components are siderite, limonite, chlorite and quartz and other gangue are discarded to obtain an electrostatic separation concentrate with a total content of siderite, limonite and chlorite less than 3%; the middlings are returned for re-selection in turn, and the electrostatic separation concentrate enters the reverse flotation operation.
[0085] 4) The weak magnetic concentration tailings and the electrostatic concentration concentrate are combined and fed into the reverse flotation operation (one coarse, one fine and three sweeps) to obtain a mixed maghemitic concentrate with an iron grade of 67.85% and a recovery rate of 82.55%.
[0086] 5) Combine the strong magnetic separation tailings, electrostatic separation tailings and reverse flotation sweeping tailings into comprehensive tailings.
[0087] Embodiment 6:
[0088] The complex and difficult-to-select iron ore used in this implementation case was taken from Anshan, Liaoning, China, with a total iron grade of 25.69%. Calculated by mass percentage, the magnetite content was 21.55%, the hematite content was 9.90%, the siderite (FeCO3) content was 6.55%, and the chlorite content was 1.66%. The gangue minerals were mainly quartz, and the process flow of the present invention was used for separation.
[0089] 1) Feed the high pressure roller mill product with a particle size of ≤3 mm into the ball mill and form a closed circuit grinding system with the cyclone to obtain a product with an overflow particle size of 85% to 95% of -200 mesh.
[0090] 2) The overflow product is fed into a weak magnetic pre-selection operation, and the resulting concentrate is subjected to three stages of weak magnetic concentration operations. Between each stage of weak magnetic selection, it is demagnetized by a demagnetizer to obtain a magnetite concentrate with a grade of 66.8%.
[0091] 3) The weak magnetic pre-selection tailings are fed into a strong magnetic separation operation, and the tailings of the strong magnetic separation operation are discarded; the strong magnetic separation concentrate is dried and fed into an electrostatic separation operation, and the tailings with the main components of siderite, limonite, chlorite and quartz are discarded to obtain an electrostatic separation concentrate with a total content of siderite, limonite and chlorite less than 3%; the middlings are returned for reselection in turn, and the electrostatic separation concentrate enters the reverse flotation operation. 4) The weak magnetic selection tailings and the electrostatic separation concentrate are combined and fed into the reverse flotation operation (one rough, one fine and three sweeps) to obtain a magnetic and hematite mixed concentrate with an iron grade of 67.66% and a recovery rate of 83.75%.
[0092] 5) Combine the strong magnetic separation tailings, electrostatic separation tailings and reverse flotation sweeping tailings into comprehensive tailings.
[0093] Embodiment 7:
[0094] The complex and difficult-to-select iron ore used in this implementation case was taken from Yuanjia Village, Shanxi Province, China, with a total iron grade of 32.07%, of which, calculated by mass percentage, magnetite contained 12.66%, hematite contained 26.83%, siderite (FeCO3) contained 8.55%, chlorite contained 5.33%, and the gangue minerals were mainly quartz and a small amount of mica. The process flow of the present invention was used for separation.
[0095] 1) Feed the high pressure roller mill product with a particle size of ≤3 mm into the ball mill and form a closed circuit grinding system with the cyclone to obtain a product with an overflow particle size of 85% to 95% of -200 mesh.
[0096] 2) The overflow product is fed into the weak magnetic pre-selection operation, and the resulting concentrate is subjected to four stages of weak magnetic concentration operations. Between each stage of weak magnetic selection, it is demagnetized by a demagnetizer to obtain a magnetite concentrate with a grade of 66.5%.
[0097] 3) The tailings of weak magnetic pre-selection are fed into two-stage strong magnetic separation operations, and the tailings of strong magnetic selection are discarded; the strong magnetic selection concentrate is dried and fed into two-stage electrostatic separation operations, and the tailings whose main components are siderite, limonite, chlorite and quartz and other gangue are discarded to obtain an electrostatic separation concentrate with a total content of siderite, limonite and chlorite less than 3%; the middlings are returned for re-selection in turn, and the electrostatic separation concentrate enters the reverse flotation operation.
[0098] 4) The weak magnetic tailings and electrostatic concentrate are combined and fed into reverse flotation operation (one coarse, one fine and three sweeps) to obtain a magnetic and red mixed concentrate with an iron grade of 67.88% and a recovery rate of 82.65%.
[0099] 5) Combine the strong magnetic separation tailings, electrostatic separation tailings and reverse flotation sweeping tailings into comprehensive tailings.
[0100] Embodiment 8:
[0101] The ore samples used in this implementation case were mixed and prepared from multiple regions. After testing, the total iron grade was 37.63%, of which, calculated by mass percentage, magnetite contained 20.74%, hematite contained 21.93%, siderite (FeCO3) contained 15.05%, chlorite contained 4.87%, and the gangue minerals were mainly quartz, which were separated by the process flow of the present invention.
[0102] 1) Feed the high pressure roller mill product with a particle size of ≤3 mm into the ball mill and form a closed circuit grinding system with the cyclone to obtain a product with an overflow particle size of 85% to 95% of -200 mesh.
[0103] 2) The overflow product is fed into the weak magnetic pre-selection operation, and the resulting concentrate is subjected to four stages of weak magnetic concentration operations. Between each stage of weak magnetic selection, it is demagnetized by a demagnetizer to obtain a magnetite concentrate with a grade of 67.75%.
[0104] 3) The tailings from the weak magnetic pre-selection are fed into two-stage strong magnetic separation operations, and the tailings from the strong magnetic separation are discarded; the strong magnetic separation concentrate is dried and fed into three-stage electrostatic separation operations, and the tailings whose main components are siderite, limonite, chlorite and quartz and other gangue are discarded to obtain an electrostatic separation concentrate with a total content of siderite, limonite and chlorite less than 3%; the middlings are returned for re-selection in turn, and the electrostatic separation concentrate enters the reverse flotation operation.
[0105] 4) The weak magnetic tailings and electrostatic concentrate are combined and fed into reverse flotation operation (one coarse, one fine and three sweeps) to obtain a magnetic and red mixed concentrate with an iron grade of 67.68% and a recovery rate of 82.75%.
[0106] 5) Combine the strong magnetic separation tailings, electrostatic separation tailings and reverse flotation sweeping tailings into comprehensive tailings.
[0107] In view of the fact that the existing "magnetic separation-anion reverse flotation" process is limited to purifying iron ore with an easily muddy mineral content of less than 3% such as iron carbonate, but is difficult to process high-carbonate and high-chlorite iron ore, Examples 5-8 of the present invention combine the electrostatic separation process with magnetic separation and flotation, and add an electrostatic separation process after the strong magnetic separation operation, so that the siderite, limonite, chlorite and other easily muddy weak magnetic ores in the mixed iron ore can be effectively removed before the mixed iron ore enters the flotation process, thereby reducing their influence on the flotation process, improving the iron ore separation index, and realizing the efficient development and utilization of complex and difficult-to-separate mixed iron ore.
Claims
1. A complex and difficult iron ore magnetic separation-electric separation process, characterized in that: The complex mixed iron ore is crushed and roller-milled to obtain a magnetic separation feed product, and the magnetic separation feed product is subjected to dry weak magnetic separation I. The concentrate is subjected to grinding operation dry grinding a, wind classification operation, and multi-stage dry weak magnetic separation operation to obtain magnetite concentrate; the dry weak magnetic separation I tailings are fed into dry strong magnetic operation dry strong magnetic I, and the obtained strong magnetic concentrate is further subjected to grinding operation dry grinding b, wind classification, dry strong magnetic operation, and the concentrate enters multi-stage electric separation operation to obtain hematite concentrate; the complex mixed iron ore contains magnetite, hematite, siderite, limonite, and chlorite.
2. The complex and refractory iron ore magnetic separation-electric separation process according to claim 1 is characterized in that: The specific steps include: 1) The complex mixed ore is crushed and fed into the roller mill, and a closed-circuit grinding system is formed with the screening operation to obtain the magnetic separation feed product; 2) The magnetic separation feed product of step 1) is fed into the dry weak magnetic separation operation dry weak magnetic I, wherein the concentrate enters the next grinding operation dry grinding a; the tailings are fed into the dry strong magnetic operation dry strong magnetic I, the dry strong magnetic I tailings are discarded, and the obtained strong magnetic concentrate enters the next grinding operation dry grinding b; 3) Dry grinding a and wind classification operations form a closed-circuit grinding system to obtain fine-grained products with a particle size of -200 mesh accounting for more than 60%, followed by several stages of dry weak magnetic separation operations to obtain magnetite concentrate with TFe ≥ 66.5%; The intermediate ore from each stage of dry weak magnetic separation is returned to the previous stage in turn, and the tailings are merged and discarded; 4) Dry grinding b and wind classification operation form a closed-circuit grinding system to obtain fine-grained products with a particle size of -200 mesh accounting for more than 60%, followed by several stages of dry strong magnetic operation, in which the concentrate enters the electric separation operation and the tailings are discarded; 5) The dry strong magnetic concentrate of step 4) is subjected to several stages of electrostatic separation to obtain hematite concentrate with TFe≥65%; the middlings of each stage of electrostatic separation and the tailings of the next stage of electrostatic separation are returned to the feed ore in sequence.
3. The complex and difficult iron ore magnetic separation-electric separation process according to claim 2 is characterized in that: In the above step 2), the dry weak magnetic I tailings contain iron-containing weak magnetic minerals, including hematite, siderite, limonite and chlorite.
4. The complex and difficult iron ore magnetic separation-electric separation process according to claim 2 is characterized in that: In the above step 5), the total content of siderite, limonite and chlorite in the hematite concentrate is less than 1% by weight.
5. A complex and difficult iron ore magnetic separation-electric separation process, characterized in that: The complex mixed iron ore is crushed and roller-milled, and then subjected to grinding and screening to obtain a graded overflow product, the overflow product is fed into a weak magnetic pre-selection operation, the obtained concentrate is fed into a weak magnetic concentration operation to obtain a magnetite concentrate; the tailings of the weak magnetic pre-selection operation are fed into a strong magnetic separation operation, the obtained strong magnetic separation concentrate is fed into an electrostatic separation operation after drying, the electrostatic separation concentrate is subjected to a reverse flotation operation to obtain a magnetic hematite mixed concentrate; the tailings of the weak magnetic concentration operation and the concentrate of the electrostatic separation operation are combined and fed into a reverse flotation operation; the complex mixed iron ore contains magnetite, hematite, siderite, limonite and chlorite.
6. A complex and difficult iron ore magnetic separation-electric separation process according to claim 5, characterized in that: The specific steps include: 1) The product of the complex mixed iron ore after crushing and roller milling is fed into the grinding and screening operation as the raw ore to obtain the graded overflow product; 2) The overflow product is fed into the weak magnetic pre-selection process, the resulting concentrate enters the multi-stage weak magnetic concentration process, and the tailings enter the strong magnetic separation process; 3) The concentrated ore obtained from the high-intensity magnetic separation operation is dried and then fed to the electric separation operation, and the tailings are discarded; 4) The concentrate obtained from the electrostatic separation operation is fed into the reverse flotation operation, and the middlings are returned to the electrostatic separation operation for further separation; 5) After multiple weak magnetic concentration operations, a magnetite concentrate with a grade of not less than 66% is obtained, and the multiple weak magnetic concentration operations are combined with tailings to feed reverse flotation operations; 6) The tailings of the multi-stage weak magnetic concentration operation are combined with the concentrate of the electrostatic separation operation, and then subjected to reverse flotation operation to obtain a mixed maghemitic concentrate, the iron grade of which is not less than 67.5%.
7. A complex and difficult iron ore magnetic separation-electric separation process according to claim 6, characterized in that: The above step 1) is to feed the particle product of the complex mixed iron ore after crushing and roller grinding into the grinding and screening operation as the raw ore to obtain the classified overflow product with a fineness of ≤0.075mm accounting for more than 60%.
8. The complex and difficult iron ore magnetic separation-electric separation process according to claim 6 is characterized in that: In the above step 4), the total content of siderite, limonite and chlorite in the electrolytic concentrate is less than 3% by weight.
9. A complex and difficult iron ore magnetic separation-electric separation process according to claim 6, characterized in that: In the above step 6), the tailings from the multi-stage weak magnetic separation operation and the concentrate from the electrostatic separation operation are combined and mixed and then concentrated, so that the reverse flotation feed concentration is controlled at 40% to 45%. The recovery rate of the reverse flotation operation in step 6) is not less than 80%.
10. A complex and refractory iron ore magnetic separation-electric separation process according to any one of claims 1 to 9, characterized in that: In the iron phase composition of the complex mixed iron ore, FeCO3 is ≥ 3% by weight.
Citation Information
Cited By
Dry reselection method for treating high-silicon bauxite
CN120132987A