MIG welding and butt joint PF one-side welding and double-side forming welding process for aluminum alloy medium and thick plates
Through MIG welding butt welding of aluminum alloy medium and thick plates, PF single-sided welding and double-sided forming welding process solves the problems of burn-through, welding beads, cracks and other problems when welding aluminum alloy medium and thick plates, improves the welding quality and efficiency, and achieves 95% one-time pass rate.
Patent Information
- Application Number
- CN202411133607.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-10-15
AI Technical Summary
Defects such as burn-through, welding nodules, cracks, and incomplete welding often occur during the welding of V-shaped groove butt joint structures of aluminum alloy medium-thick plates, resulting in poor weld quality and low production efficiency. Existing technologies cannot effectively solve these problems.
The aluminum alloy medium-thick plate MIG welding butt PF single-sided welding and double-sided forming welding process includes pre-processing the arc starting plate and the arc closing plate, leaving a lateral anti-deformation gap, using argon shielding gas with a purity higher than 99.999%, and pre-processing the arc starting plate and the arc closing plate. hot The aluminum alloy plate adopts the "flexible massage" technique of drawing a large circle on the outer ring to a small circle on the inner ring for bottom welding. The middle filling layer adopts an anti-arc technique, and the cover layer adopts a pull-down oblique triangle technique to control longitudinal deformation. and wrong words.
Significantly improves the welding quality of V-shaped groove butt jointing of aluminum alloy medium-thick plates with PF single-sided welding and double-sided forming, reduces welding defects, increases the one-time pass rate to 95%, and reduces the man-hours and material consumption of welding repairs.
Smart Images

Figure CN118768697A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum alloy welding, and in particular to a MIG welding butt PF single-sided welding and double-sided forming welding process for aluminum alloy medium and thick plates. Background Art
[0002] Aluminum alloy has the advantages of light weight, corrosion resistance, and high specific strength. It has been widely used in rail transportation, aerospace, shipbuilding, automobile and other industries. When welding the V-groove butt joint structure of aluminum alloy medium and thick plates (above 12mm), in order to ensure that the weld does not produce defects such as cracking, welding penetration, and incomplete welding, single-sided welding and double-sided forming are usually used to ensure the quality of the weld. Taking the 12mm+12mm V-butt PF joint as an example, in actual production, welders usually use MIG welding. There are three common welding methods for the base welding of the V-groove butt joint PF of aluminum alloy medium and thick plates: straight line pulling method, up and down swing method, and high voltage and low current method.
[0003] At present, these three welding process methods are very likely to cause welding defects such as burn-through, weld nodules, cracks, and incomplete penetration in actual welding production. The one-time qualified rate is only about 65%, which affects the quality of the weld. At the same time, due to a large amount of rework, the production cost is high and the production efficiency is low. How to control the quality of the base, filling and cover welds of the V-shaped PF butt joint of aluminum alloy medium and thick plates has become a problem that needs to be solved.
[0004] Currently, no effective solution has been proposed for the problems in the related technologies. Summary of the invention
[0005] In view of the problems in the related technology, the present invention proposes a MIG welding butt PF single-sided welding and double-sided forming welding process for aluminum alloy medium and thick plates to solve the problems of poor welding quality and low efficiency such as burn-through, weld nodules, cracks, incomplete penetration, etc. in the welds in the above-mentioned background technology.
[0006] To this end, the specific technical solution adopted by the present invention is as follows: Aluminum alloy medium and thick plate MIG welding butt PF single-sided welding double-sided forming welding process, the aluminum alloy medium and thick plate MIG welding butt PF single-sided welding double-sided forming welding process includes the following steps: S1. When welding aluminum alloy medium and thick plates, pre-treated arc starting plates and arc ending plates are placed at the arc starting and ending points; S2. When assembling the aluminum alloy medium and thick plate with the arc starting plate and arc closing plate, a transverse anti-deformation gap should be reserved; S3. When spot welding thick and medium aluminum alloy plates, according to the thickness of the blunt edge of the groove, the method of no gap at the welding start end and reserved gap at the arc end is adopted to prevent deformation and misalignment in the longitudinal direction.
[0007] Further, the pre-processing includes: Use organic solvent to remove oil and dust from the arc starting plate and arc ending plate; Use mechanical methods to remove oxide film impurities on the arc starting plate and arc ending plate.
[0008] Furthermore, when the aluminum alloy medium and thick plates are butt-welded, the welding machine and the shielding gas switch are turned on, and the shielding gas is argon gas with a purity greater than 99.999%, and the gas flow rate of the shielding gas is 20 L / min.
[0009] Furthermore, the angle of the lateral reverse deformation is 3°, and when the aluminum alloy medium and thick plate, the arc-starting plate and the arc-ending plate are assembled, a flame or a hot air gun is used to preheat the aluminum alloy medium and thick plate, the arc-starting plate and the arc-ending plate, and the preheating temperature is 70°C-90°C.
[0010] Furthermore, the spot welding of the aluminum alloy medium and thick plates includes welding of a base weld, welding of an intermediate filling layer and welding of a cover layer.
[0011] Furthermore, the welding base weld includes: performing base welding of the weld from a large circle drawn on the outer circle to a small circle drawn on the inner circle.
[0012] Furthermore, the intermediate filling layer welding includes: using a reverse arc technique to perform filling layer welding.
[0013] Furthermore, the cover layer welding includes: welding by a downward inclined triangle method to fill the weld groove.
[0014] Furthermore, the reserved gap at the arc closing end is 0.5mm-1.5mm.
[0015] Furthermore, the thickness of the arc starting plate and the arc ending plate is greater than 5 mm or an aluminum alloy with the same thickness as the base material.
[0016] The beneficial effects of the present invention are: 1. The present invention can avoid the problems of poor welding quality, low efficiency, and a one-time qualified rate of only 65% such as burn-through, weld nodules, cracks, and incomplete penetration in the weld during the welding process, and improve the welding quality of the base, filling, and cover layers of the 70° V-groove butt joint PF single-sided welding and double-sided forming of the aluminum alloy medium and thick plates, while reducing the time and materials for repairing welding defects, and the one-time qualified rate reaches about 95%, thereby improving the production quality.
[0017] 2. When welding with innovative operation methods, the base welding of the weld is carried out using the "flexible massage" technique of drawing a large circle from the outer circle to a small circle from the inner circle, so that the heat is concentrated within a certain range rather than on one point, which can ensure that the base weld is penetrated and that no holes are produced by welding; the intermediate filling layer is welded using the "reverse arc" technique, which can prevent the weld metal from sagging and dripping, making the weld too thick or producing weld nodules that affect the welding and quality of the subsequent cover layer; the last cover layer is welded using the "pull-down oblique triangle" technique, which can fill the weld groove and make the weld beautiful, significantly reducing the probability of welding defects such as undercut and dripping that are prone to occur in conventional ordinary welding techniques. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0019] Figure 1 Flow chart of a MIG welding butt PF single-sided welding and double-sided forming welding process for aluminum alloy medium and thick plates according to an embodiment of the present invention; Figure 2 It is a schematic diagram of the base layer welding in the PF single-sided welding and double-sided forming welding process of the aluminum alloy medium and thick plate MIG welding according to an embodiment of the present invention; Figure 3 It is a schematic diagram of the welding of the filling layer in the PF single-sided welding and double-sided forming welding process of the aluminum alloy medium and thick plate MIG welding according to an embodiment of the present invention; Figure 4 It is a schematic diagram of the welding of the cover layer in the PF single-sided welding and double-sided forming welding process of the aluminum alloy medium and thick plate MIG welding according to an embodiment of the present invention; Figure 5 It is a schematic diagram of the macroscopic metallographic weld structure after welding in the PF single-sided welding and double-sided forming welding process of MIG welding of aluminum alloy medium and thick plates according to an embodiment of the present invention.
[0020] In the figure: 1. Center line of weld; 2. Fusion line of weld; 3. Groove line; 4. Arc starting plate; 5. Arc ending plate; 6. Base layer; 7. Filling layer; 8. Cap weld; 9. Filling weld; 10. Base weld; 11. Weld root forming. DETAILED DESCRIPTION
[0021] To further illustrate each embodiment, the present invention provides drawings, which are part of the disclosure of the present invention and are mainly used to illustrate the embodiments and can be used in conjunction with the relevant descriptions in the specification to explain the operating principles of the embodiments. With reference to these contents, ordinary technicians in the field should be able to understand other possible implementations and advantages of the present invention. The components in the figures are not drawn to scale, and similar component symbols are generally used to represent similar components.
[0022] According to an embodiment of the present invention, a MIG welding butt PF single-sided welding and double-sided forming welding process for aluminum alloy medium and thick plates is provided.
[0023] The present invention is further described with reference to the accompanying drawings and specific embodiments. Figure 1-5 As shown, according to the MIG welding butt PF single-sided welding and double-sided forming welding process for aluminum alloy medium and thick plates in an embodiment of the present invention, the MIG welding butt PF single-sided welding and double-sided forming welding process for aluminum alloy medium and thick plates includes the following steps: S1. When welding aluminum alloy medium and thick plates, the arc starting and ending positions are provided with pre-treated arc starting plates 4 and arc ending plates 5; S2. When assembling the aluminum alloy medium and thick plate with the arc-starting plate 4 and the arc-ending plate 5, a lateral anti-deformation gap is reserved; S3. When spot welding thick and medium aluminum alloy plates, according to the thickness of the blunt edge of the groove and the position of the groove line 3, the method of no gap at the welding start end and reserved gap at the arc end is adopted to prevent deformation and misalignment in the longitudinal direction.
[0024] In one embodiment, the pre-processing includes: Use organic solvent to remove oil and dust from the arc starting plate 4 and the arc ending plate 5; Mechanical methods are used to remove oxide film impurities on the arc starting plate 4 and the arc ending plate 5.
[0025] In one embodiment, when the aluminum alloy medium and thick plates are butt welded, to ensure welding quality, the welding machine and the shielding gas switch are turned on, and the shielding gas is argon with a purity greater than 99.999%, and the gas flow rate of the shielding gas is 20L / min.
[0026] In one embodiment, transverse reverse deformation needs to be reserved during assembly. The gap between the two aluminum alloy medium and thick plates is the weld center line 1, and the weld fusion line 2 is distributed around the weld center line 1. The angle of the transverse reverse deformation is about 3°. The reverse deformation can prevent the inward transverse shrinkage deformation caused by welding and increase the accessibility during welding. When the aluminum alloy medium and thick plates are assembled with the arc-starting plate 4 and the arc-ending plate 5, a flame or a hot air gun is used to preheat the aluminum alloy medium and thick plates, the arc-starting plate 4 and the arc-ending plate 5, and the preheating temperature is 70°C-90°C.
[0027] In one embodiment, the spot welding of the aluminum alloy medium and thick plate includes welding of a base weld, welding of an intermediate filling layer and welding of a cover layer.
[0028] In one embodiment, the welding base weld includes: performing base welding of the weld by a "flexible massage" technique from a large circle in the outer circle to a small circle in the inner circle, so that the heat is concentrated within a certain range rather than at one point, which can ensure that the base weld is penetrated and that no holes are produced by the weld.
[0029] In one embodiment, the intermediate filling layer welding includes: welding the filling layer 7 using a reverse arc technique, which can prevent the weld metal from sagging and causing the weld to be too thick or produce weld nodules that affect the subsequent welding and quality of the cover layer.
[0030] In one embodiment, the cover layer welding includes: welding by pulling down an oblique triangle to fill the weld groove and make the weld shape beautiful, which significantly improves the probability of welding defects such as undercut and slippage caused by conventional ordinary welding techniques.
[0031] Specifically, multi-layer and multi-pass welding is adopted, and the original commonly used straight-line pulling welding method, up and down swinging method or high voltage and low current welding are abandoned to perform base layer 6 welding, and an innovative operation method is adopted.
[0032] When using this new welding technique, the current and voltage can be appropriately increased according to the metal characteristics of the large thermal conductivity of aluminum alloy. For example, when the plate thickness is 12mm, the double-sided groove is 70°, the blunt edge is 0.5mm, the assembly gap at the arc start is 0mm, and the arc end is 1mm, 190A-210A is used for welding each layer of the weld (the above parameters for each layer can be adjusted by yourself).
[0033] In one embodiment, the reserved gap at the arc closing end is 0.5 mm-1.5 mm.
[0034] Specifically, in order to prevent longitudinal shrinkage deformation during welding, during spot welding, according to the thickness of the blunt edge of the groove, the welding deformation in the longitudinal direction can be controlled by adopting a method of no gap at the welding start end and a gap of 0.5mm-1.5mm reserved at the arc end.
[0035] In addition, a 0.5mm assembly gap is reserved at the arc end when the blunt edge is small, the current is small, and the welding speed is fast; a 1-1.5mm assembly gap is reserved at the arc end when the blunt edge is large, the current is large, and the welding speed is slow. This reserved gap method can prevent the occurrence of misalignment caused by large shrinkage.
[0036] In one embodiment, the arc starting plate 4 and the arc ending plate 5 have a thickness of more than 5 mm or an aluminum alloy with the same thickness as the base material.
[0037] Specifically, an aluminum alloy arc-starting plate 4 and an arc-ending plate 5 with a thickness of more than 5 mm or the same as that of the parent material are installed at the arc-starting and arc-ending positions of the weld, and the arc-starting plate 4 and the arc-ending plate 5 may or may not have welding grooves.
[0038] In order to facilitate understanding of the above technical solutions of the present invention, the working principle or operation mode of the present invention in the actual process is described in detail below.
[0039] In actual application, multi-layer and multi-pass welding is adopted, and the original three methods of straight-line pulling welding, up and down swinging method or high voltage and low current are abandoned for the base layer 6 welding. An innovative operation method is adopted: the "flexible massage" technique of drawing a large circle from the outer circle to the small circle inside is used for the base welding of the weld, and the "reverse arc" technique is used for the middle filling layer welding 7 to prevent the weld from sagging and dripping. Finally, the cover layer is welded by the "downward oblique triangle" technique, and the arc attenuation current is used for arc welding at the arc closing point.
[0040] Aluminum alloy arc-starting plates 4 and arc-ending plates 5 with a thickness of more than 5mm or the same as that of the parent material are installed at the arc-starting and arc-ending places of the weld, and the workpiece is preheated with a flame or a hot air gun at a preheating temperature of 70℃-90℃. In order to prevent longitudinal shrinkage deformation during welding, according to the thickness of the blunt edge of the groove, the method of no gap at the welding start end and a gap of 0.5mm-1.5mm at the arc-ending end can be used to control the deformation in the longitudinal direction and prevent the occurrence of misalignment. When assembling, transverse reverse deformation is also reserved, which can prevent the inward transverse shrinkage deformation caused by the lack of reverse deformation and increase the accessibility during welding. Multi-layer and multi-pass welding is adopted, and the original conventional straight-line pulling welding method, up and down swinging method or high voltage and low current method are abandoned for the base layer 6 welding. An innovative operation method is adopted: the "flexible massage" technique of drawing a large circle from the outer circle to the small circle inside is used for the base welding of the weld, and the "reverse arc" technique is used for the middle filling layer welding 7 to prevent the weld from sagging and dripping. Finally, the cover layer is welded by the "downward oblique triangle" technique, which can effectively prevent the occurrence of defects.
[0041] To sum up, with the help of the above-mentioned technical scheme of the present invention, the present invention can avoid the problems of poor welding quality, low efficiency, and a one-time qualified rate of only 65% such as burn-through, weld nodules, cracks, incomplete penetration, etc. in the weld during the welding process, and improve the welding quality of the base, filling and covering layers of the 70° V-groove butt PF single-sided welding and double-sided forming of aluminum alloy medium and thick plates, while reducing the working hours and materials for repairing welding defects, and the one-time qualified rate reaches about 95%, thereby improving the production quality. When welding with the innovative operation method, the base welding of the weld is carried out using a "flexible massage" technique of drawing a large circle from the outer circle to a small circle from the inner circle, so that the heat is concentrated within a certain range rather than on one point, which can ensure that the base weld is penetrated while not being welded through to produce holes; the intermediate filling layer welding adopts the "reverse arc" technique to weld the filling layer 7, which can prevent the weld metal from sagging and causing the weld to be too thick or to produce weld nodules that affect the welding and quality of the subsequent cover layer; the last cover layer is welded using the "pull-down oblique triangle" technique, which can fill the weld groove and make the weld beautiful at the same time, significantly reducing the probability of welding defects such as undercut and slippage that are easily produced by conventional ordinary welding techniques.
[0042] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. Aluminum alloy medium and thick plate MIG welding butt PF single-sided welding double-sided forming welding process, characterized in that: The aluminum alloy medium and thick plate MIG welding butt PF single-sided welding double-sided forming welding process comprises the following steps: S1. When welding aluminum alloy medium and thick plates, pre-treated arc starting plates and arc ending plates are placed at the arc starting and ending points; S2. When assembling the aluminum alloy medium and thick plate with the arc starting plate and arc closing plate, a transverse anti-deformation gap should be reserved; S3. When spot welding thick and medium aluminum alloy plates, according to the thickness of the blunt edge of the groove, the method of no gap at the welding start end and reserved gap at the arc end is adopted to prevent deformation and misalignment in the longitudinal direction.
2. The MIG welding butt PF single-sided welding and double-sided forming welding process for aluminum alloy medium and thick plates according to claim 1 is characterized in that: The pre-processing includes: Use organic solvent to remove oil and dust from the arc starting plate and arc ending plate; Use mechanical methods to remove oxide film impurities on the arc starting plate and arc ending plate.
3. The aluminum alloy medium and thick plate MIG welding butt PF single-sided welding double-sided forming welding process according to claim 1 is characterized in that: When the aluminum alloy medium and thick plates are butt welded, the welding machine and the shielding gas switch are turned on, and the shielding gas is argon gas with a purity greater than 99.999%, and the gas flow rate of the shielding gas is 20L / min.
4. The aluminum alloy medium and thick plate MIG welding butt PF single-sided welding double-sided forming welding process according to claim 1 is characterized in that: The angle of the transverse reverse deformation is 3°, and when the aluminum alloy medium and thick plate, the arc-starting plate and the arc-ending plate are assembled, a flame or a hot air gun is used to preheat the aluminum alloy medium and thick plate, the arc-starting plate and the arc-ending plate, and the preheating temperature is 70°C-90°C.
5. The aluminum alloy medium and thick plate MIG welding butt PF single-sided welding double-sided forming welding process according to claim 1 is characterized in that: The spot welding of the aluminum alloy medium and thick plate includes welding of a base weld, welding of an intermediate filling layer and welding of a cover layer.
6. The aluminum alloy medium and thick plate MIG welding butt PF single-sided welding double-sided forming welding process according to claim 5 is characterized in that: The welding bottoming weld includes: performing bottoming welding of the weld from a large circle drawn on the outer circle to a small circle drawn on the inner circle.
7. The aluminum alloy medium and thick plate MIG welding butt PF single-sided welding double-sided forming welding process according to claim 5 is characterized in that: The intermediate filling layer welding includes: using a reverse arc technique to perform filling layer welding.
8. The aluminum alloy medium and thick plate MIG welding butt PF single-sided welding double-sided forming welding process according to claim 5, characterized in that: The cover layer welding includes: welding by pulling down an oblique triangle to fill the weld groove.
9. The aluminum alloy medium and thick plate MIG welding butt PF single-sided welding double-sided forming welding process according to claim 1, characterized in that: The reserved gap at the arc closing end is 0.5mm-1.5mm.
10. The aluminum alloy medium and thick plate MIG welding butt PF single-sided welding double-sided forming welding process according to claim 1, characterized in that: The thickness of the arc starting plate and the arc ending plate is more than 5 mm or the same thickness of the base material aluminum alloy.
Citation Information
Cited By
Hot-wire narrow-gap argon tungsten-arc welding method for dissimilar steel connecting pipe
CN121131935A