Titanium alloy thin-wall hemisphere machining method
By using the design of perforations and through-holes in the processing of titanium alloy thin-walled hemispheres, combined with hot isostatic pressing technology and mechanical vibration, the problems of dimensional accuracy and processing difficulty in the processing of titanium alloy thin-walled hemispheres are solved, achieving high efficiency and Precise thin-walled hemisphere forming and production.
Patent Information
- Application Number
- CN202410938753.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-14
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-14
AI Technical Summary
It is difficult to effectively process titanium alloy thin-walled hemispheres with existing technology, resulting in poor dimensional accuracy and high processing difficulty. Especially when manufacturing spherical or ellipsoidal thin-walled shell structures of fire tanks, conventional methods are difficult to obtain consistent thickness and high precision.
A titanium alloy thin-walled hemispherical processing method is adopted, by setting perforations and through holes on the square plate, combined with mechanical vibration and hot isostatic pressing technology, to ensure that the titanium alloy powder is fully filled and sintered, and the cooperation of the mold and the package is used A hemispherical filling cavity is formed to reduce voids and improve density, and then a high-precision thin-walled hemisphere is obtained through machining and grinding.
It improves the dimensional accuracy and production efficiency of titanium alloy thin-walled hemispheres, reduces the processing difficulty, ensures the consistency of arc surface thickness, simplifies the operating process, and improves production efficiency.
Smart Images

Figure HDA0004943358820000011 
Figure HDA0004943358820000021 
Figure HDA0004943358820000031
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of titanium alloy processing, and in particular relates to a method for processing a titanium alloy thin-walled hemispherical body. Background Art
[0002] The density of titanium alloy is only 60% of that of steel, but its strength can reach the level of many alloy steels. Titanium alloy also has excellent corrosion resistance and heat resistance. In recent years, it has become an important structural metal and is widely used in aerospace, marine engineering, energy and chemical industry, automobile manufacturing and other fields.
[0003] In order to achieve firefighting in super-high-rise buildings, the country has vigorously promoted the development of rotor-structured fire-fighting drones, but the carrying capacity of such drones is limited. Therefore, if the weight of the fire tank can be reduced, it will help the drone to carry more fire extinguishing agents. Therefore, titanium and titanium alloys are currently the best manufacturing materials for this type of fire tank.
[0004] Fire tanks are usually spherical or ellipsoidal thin-walled shell structures. The manufacturing of metal thin-walled spherical shell structures is more complicated than that of other conventional structural parts. In particular, due to the unique physical and chemical properties of titanium alloys, their plasticity is poor and their rebound is large, resulting in poor processability. Conventional metal plastic processing methods make it difficult to obtain titanium alloy thin-walled hemispheres with high dimensional accuracy.
[0005] For example, a hot isostatic pressing method for a titanium alloy gas cylinder hemisphere disclosed in application number CN201810898438.4 utilizes hot isostatic pressing (HIP) technology to sinter and form titanium alloy powder, and adopts a method of cooperating internal molds and external sheaths to achieve partial features of formed parts and reduce post-processing. In this technical scheme, the internal mold, base plate, and sheath form a storage space for the powder. The prepared spherical titanium alloy powder is loaded into the space and compacted by mechanical vibration. The titanium alloy powder below the top is restricted by the internal mold, base plate, and sheath and can form a regular hemispherical shape. However, an opening is provided at the upper end of the sheath and is used to connect to the exhaust pipe. There is a lack of restriction on the titanium alloy powder there. After mechanical vibration, only the titanium alloy powder at the top can be made planar (see Figure 1 ), the tightness here is poor, and there is a certain difference between the thickness of the top of the arc surface of the titanium alloy thin-walled hemisphere obtained by sintering and the thickness of other parts of the arc surface, which needs to be processed by mechanical finishing. However, mechanical finishing is more difficult for the processing of the arc surface, so there is still room for improvement. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a titanium alloy thin-walled hemispherical body processing method, which can improve dimensional accuracy, reduce processing difficulty and improve production efficiency by optimizing the processing technology.
[0007] The technical solution adopted by the present invention to solve the above technical problems is: a method for processing a titanium alloy thin-walled hemispherical body, comprising the following steps:
[0008] S1. Prepare square plates and spheres;
[0009] S2. A perforation is formed on the end surface of the square plate, the perforation passes through the two end surfaces of the square plate, and a through hole is formed on one side surface of the square plate, the through hole is connected to the middle of the perforation;
[0010] S3, cutting the sphere into two halves to obtain two hemispheres, fixing the two hemispheres to two end faces of the square plate, with the hemispheres staggered from the perforations;
[0011] S4, preparing two sleeves, the two sleeves corresponding to the two hemispheres one by one, fixing the two sleeves to the two end surfaces of the square plate to obtain a mold, the sleeves, the corresponding hemispheres and the square plate cooperate to form a hemispherical filling cavity, and the perforation is connected to the filling cavity;
[0012] S5, placing the mold vertically so that the package sleeve and the hemisphere are located on both sides of the square plate in the horizontal direction, and the through hole is located on the upper part of the square plate, and the through hole extends in the up-down direction;
[0013] S6. preparing spherical titanium alloy powder;
[0014] S7, injecting titanium alloy powder into the filling cavity through the through hole and the perforation, and keeping the titanium alloy powder in the filling cavity, the perforation and the through hole dense by mechanical vibration;
[0015] S8, connecting one end of the exhaust pipe to the through hole, and connecting the other end of the exhaust pipe to the exhaust device;
[0016] S9, placing the mold filled with titanium alloy powder in a heating furnace for heating, and extracting the air in the filling cavity through an exhaust device, and after completion, clamping off the exhaust pipe and sealing it with welding;
[0017] S10, placing the mold in a hot isostatic pressing furnace, sintering the spherical titanium alloy powder under high temperature and high pressure, and forming two titanium alloy thin-walled hemispherical semi-finished products, a first connecting column located in the through hole, and a second connecting column located in the through hole under the action of the mold;
[0018] S11, using mechanical processing equipment to remove the sheath, cut off the first connecting column, and take out the two titanium alloy thin-walled hemispherical semi-finished products;
[0019] S12, grinding the end faces of the semi-finished products of the two titanium alloy thin-walled hemispheres using a grinding device to obtain titanium alloy thin-walled hemispheres.
[0020] Preferably, in step S6, the material of the titanium alloy powder is Ti-6Al-4V, and the particle size range is 40±5 μm.
[0021] Preferably, in step S9, the temperature of the heating furnace is 400-480°C, the heating time is 2-4 hours, and the vacuum degree of the filling cavity is less than 1.0×10 -3 Pa.
[0022] Preferably, in step S10, the hot isostatic pressing parameters are: temperature range is 1000-1100°C, holding time is 4h-6h, argon is filled into the hot isostatic pressing furnace during the heating process, and the mold is pressed by argon at a pressing pressure of 150-300MPa.
[0023] Preferably, the heating rate is 8-12°C / min.
[0024] Preferably, after the holding time is over, the mold is cooled with the furnace at a cooling rate of 8-12°C / min, and the mold is depressurized and released after the temperature drops below 50°C.
[0025] Preferably, the sleeve has an outer convex arc surface, an inner concave arc surface and a bottom surface, and the perforation is tangent to or intersects with the inner edge of the bottom surface of the sleeve.
[0026] Preferably, the square plate and the hemisphere, and the square plate and the sleeve are fixed by welding.
[0027] Preferably, the square plate and the hemisphere, and the square plate and the sheath are fixed by brazing.
[0028] Preferably, the square plate, the sphere and the sleeve are all made of 304 stainless steel.
[0029] Compared with the prior art, the advantages of the present invention are:
[0030] 1. By setting perforations and through holes on the square plate, the perforations are connected to the filling cavity, and the exhaust pipe is connected to the through hole, so as to avoid setting openings on the package. The complete package and the hemisphere can be fully and closely contacted with the filled titanium alloy powder, ensuring the integrity of the arc surface of the titanium alloy thin-walled hemisphere obtained by sintering, that is, the thickness of the top of the arc surface of the titanium alloy thin-walled hemisphere is highly consistent with the thickness of other parts of the arc surface, and the dimensional accuracy is good;
[0031] 2. By setting perforations and through holes on the square plate and placing the mold vertically, injecting titanium alloy powder and performing mechanical vibration, if there is a gap in the filling cavity, the titanium alloy powder in the perforations and through holes will be filled into the filling cavity. The injection process only needs to confirm whether the titanium alloy powder in the through hole is decreasing, and the operation is relatively simple;
[0032] 3. The conventional filling cavity is short and wide, and the width of the filling cavity along the horizontal direction is wider as a whole. The density between the injected titanium alloy powders is relatively general. However, the mold in this scheme is placed vertically, the filling cavity is slender, and the width of the filling cavity along the horizontal direction is narrow as a whole. After the titanium alloy powder is injected and mechanically vibrated, the density between the titanium alloy powders is higher;
[0033] 4. The titanium alloy thin-walled hemisphere processing method can obtain two titanium alloy thin-walled hemispheres at one time, and compared with the conventional titanium alloy gas cylinder hemisphere hot isostatic pressing forming method, the production efficiency is higher;
[0034] 5. By cutting a sphere into two hemispheres and fixing the two hemispheres to the two end faces of a square plate, the inner diameters of the two titanium alloy thin-walled hemispheres prepared are well consistent, which facilitates the subsequent manufacture of a high-precision spherical thin-walled shell structure;
[0035] 6. After sintering, use mechanical processing equipment to remove the sleeve, cut off the first connecting column, and take out the semi-finished products of the two titanium alloy thin-walled hemispheres. Although there is a cut first connecting column on the semi-finished product, the first connecting column is located on the plane of the semi-finished product, and it can be cut and polished flat. Compared with the processing of the curved surface, the processing difficulty is low and the processing efficiency is high;
[0036] 7. The design of the square plate, after being connected with the hemisphere and the sleeve, the four corners of the square plate extend outside the sleeve, which can be used to cooperate with the machine and positioning tooling to keep the mold in a vertical state, and has good applicability. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 Schematic diagram of the structure of a titanium alloy thin-walled hemisphere Figure 1 ;
[0038] Figure 2 Schematic diagram of the structure of a titanium alloy thin-walled hemisphere Figure 2 ;
[0039] Figure 3 It is a structural schematic diagram of the mold in the present invention;
[0040] Figure 4 It is a schematic diagram of the cross-sectional structure of the mold in the present invention.
[0041] In the figure: 1, square plate; 11, perforation; 12, through hole; 2, hemispherical body; 3, sleeve; 4, exhaust pipe. DETAILED DESCRIPTION
[0042] The present invention is further described in detail below with reference to the accompanying drawings.
[0043] In the description of the present invention, it should be noted that the directions or positional relationships indicated by the terms "center", "upper", "lower", "left", "right", "inner", "outer", etc. are based on the directions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.
[0044] Example: Figures 2 to 4 As shown, a method for processing a titanium alloy thin-walled hemispherical body comprises the following steps:
[0045] S1, preparing a square plate 1 and a sphere;
[0046] S2, a through hole 11 is formed on the end surface of the square plate 1, the through hole 11 passes through the two end surfaces of the square plate 1, and a through hole 12 is formed on one side surface of the square plate 1, the through hole 12 is connected to the middle part of the through hole 11;
[0047] S3, cutting the sphere into two halves to obtain two hemispheres 2, and welding the two hemispheres 2 to the two end faces of the square plate 1, with the hemispheres 2 being staggered from the through holes 11;
[0048] S4, prepare two sleeves 3, the two sleeves 3 correspond to the two hemispherical bodies 2 one by one, weld and fix the two sleeves 3 to the two end surfaces of the square plate 1 to obtain a mold, the sleeves 3, the corresponding hemispherical bodies 2 and the square plate 1 cooperate to form a hemispherical filling cavity, and the perforation 11 is connected to the filling cavity;
[0049] S5, placing the mold vertically, so that the sleeve 3 and the hemispherical body 2 are located on both sides of the square plate 1 in the horizontal direction, and the through hole 12 is located on the upper part of the square plate 1, and the through hole 12 extends in the up-down direction;
[0050] S6. Prepare spherical titanium alloy powder, the material of the titanium alloy powder is Ti-6Al-4V, and the particle size range is 40±5 μm;
[0051] S7, injecting titanium alloy powder into the filling cavity through the through hole 12 and the perforation 11, and keeping the titanium alloy powder in the filling cavity, the perforation 11 and the through hole 12 dense by mechanical vibration;
[0052] S8, connecting one end of the exhaust pipe 4 to the through hole 12, and connecting the other end of the exhaust pipe 4 to the exhaust device;
[0053] S9, placing the mold filled with titanium alloy powder in a heating furnace for heating, and extracting the air in the filling cavity through an exhaust device, and after completion, clamping off the exhaust pipe 4 and sealing it with welding;
[0054] S10, placing the mold in a hot isostatic pressing furnace, sintering the spherical titanium alloy powder under high temperature and high pressure, and forming two titanium alloy thin-walled hemispherical semi-finished products, a first connecting column located in the through hole 11, and a second connecting column located in the through hole 12 under the action of the mold;
[0055] S11, using mechanical processing equipment to remove the sheath 3, cut off the first connecting column, and take out the two titanium alloy thin-walled hemispherical semi-finished products;
[0056] S12, grinding the end faces of the two titanium alloy thin-walled hemispherical semi-finished products using grinding equipment to obtain titanium alloy thin-walled hemispherical bodies 2.
[0057] In step S9, the temperature of the heating furnace is 400-480°C, preferably 440°C, the heating time is 2-4 hours, preferably 3 hours, and the vacuum degree of the filling cavity is less than 1.0×10 -3 Pa, preferably 0.8×10 -3 Pa.
[0058] In step S10, the hot isostatic pressing parameters are: temperature range is 1000-1100°C, preferably 1100°C, holding time is 4h-6h, preferably 5h, heating rate is 8-12°C / min, preferably 10°C / min, argon is filled into the hot isostatic pressing furnace during the heating process, and the mold is pressed by argon, and the pressing pressure is 150-300MPa, preferably 200MPa. After the holding time is over, the mold is cooled with the furnace, and the cooling rate is 8-12°C / min, preferably 10°C / min, and the pressure is released and the gas is released after it drops below 50°C.
[0059] In this embodiment, the sleeve has an outer convex arc surface, an inner concave arc surface and a bottom surface, and the perforations are tangent (inscribed) or intersecting with the inner edge of the bottom surface of the sleeve to ensure that the titanium alloy powder is fully filled into the filling cavity.
[0060] In this embodiment, the square plate and the hemisphere, and the square plate and the sleeve are fixed by brazing. The operating temperature is low, which can reduce the thermal impact on the parent material, thereby reducing thermal stress and deformation, maintaining the mechanical properties and structural stability of the parent material, and having high connection strength and good stability. At the same time, it has good air tightness to avoid air leakage during the vacuum process.
[0061] In this embodiment, the square plate, the sphere and the sleeve are all made of 304 stainless steel.
[0062] The present invention is described above by way of example in conjunction with the accompanying drawings. It is obvious that the implementation of the present invention is not limited to the above-mentioned method. As long as various improvements are made using the method concept and technical solution of the present invention, or the concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.
Claims
1. A method for processing a titanium alloy thin-walled hemispherical body, characterized in that The following steps are involved: S1. Prepare square plates and spheres; S2. A perforation is formed on the end surface of the square plate, the perforation passes through the two end surfaces of the square plate, and a through hole is formed on one side surface of the square plate, the through hole is connected to the middle of the perforation; S3, cutting the sphere into two halves to obtain two hemispheres, fixing the two hemispheres to two end faces of the square plate, with the hemispheres staggered from the perforations; S4, preparing two sleeves, the two sleeves corresponding to the two hemispheres one by one, fixing the two sleeves to the two end surfaces of the square plate to obtain a mold, the sleeves, the corresponding hemispheres and the square plate cooperate to form a hemispherical filling cavity, and the perforation is connected to the filling cavity; S5, placing the mold vertically so that the package sleeve and the hemisphere are located on both sides of the square plate in the horizontal direction, and the through hole is located on the upper part of the square plate, and the through hole extends in the up-down direction; S6. preparing spherical titanium alloy powder; S7, injecting titanium alloy powder into the filling cavity through the through hole and the perforation, and keeping the titanium alloy powder in the filling cavity, the perforation and the through hole dense by mechanical vibration; S8, connecting one end of the exhaust pipe to the through hole, and connecting the other end of the exhaust pipe to the exhaust device; S9, placing the mold filled with titanium alloy powder in a heating furnace for heating, and extracting the air in the filling cavity through an exhaust device, and after completion, clamping off the exhaust pipe and sealing it with welding; S10, placing the mold in a hot isostatic pressing furnace, sintering the spherical titanium alloy powder under high temperature and high pressure, and forming two titanium alloy thin-walled hemispherical semi-finished products, a first connecting column located in the through hole, and a second connecting column located in the through hole under the action of the mold; S11, using mechanical processing equipment to remove the sheath, cut off the first connecting column, and take out the two titanium alloy thin-walled hemispherical semi-finished products; S12, grinding the end faces of the semi-finished products of the two titanium alloy thin-walled hemispheres using a grinding device to obtain titanium alloy thin-walled hemispheres.
2. A method for processing a titanium alloy thin-walled hemispherical body according to claim 1, characterized in that In step S6, the material of the titanium alloy powder is Ti-6Al-4V, and the particle size range is 40±5 μm.
3. A method for processing a titanium alloy thin-walled hemispherical body according to claim 1, characterized in that In step S9, the temperature of the heating furnace is 400-480°C, the heating time is 2-4 hours, and the vacuum degree of the filling cavity is less than 1.0×10 -3 Pa.
4. A method for processing a titanium alloy thin-walled hemispherical body according to claim 1, characterized in that In step S10, the hot isostatic pressing parameters are: temperature range is 1000-1100°C, holding time is 4h-6h, argon is filled into the hot isostatic pressing furnace during the heating process, and the mold is pressed by argon at a pressing pressure of 150-300MPa.
5. A method for processing a titanium alloy thin-walled hemispherical body according to claim 4, characterized in that The heating rate is 8-12℃ / min.
6. A method for processing a titanium alloy thin-walled hemispherical body according to claim 4, characterized in that After the holding time is over, the mold is cooled with the furnace at a cooling rate of 8-12℃ / min. After the temperature drops below 50℃, the pressure is released and the air is released.
7. The method for processing a titanium alloy thin-walled hemispherical body according to claim 1, characterized in that The package sleeve has an outer convex arc surface, an inner concave arc surface and a bottom surface, and the perforation is tangent to or intersects with the inner edge of the bottom surface of the package sleeve.
8. The method for processing a titanium alloy thin-walled hemispherical body according to claim 1, characterized in that The square plate and the hemisphere, as well as the square plate and the sheath are all welded and fixed.
9. A method for processing a titanium alloy thin-walled hemispherical body according to claim 8, characterized in that The square plate and the hemisphere, and the square plate and the sheath are fixed by brazing.
10. The method for processing a titanium alloy thin-walled hemispherical body according to claim 1, characterized in that The square plate, sphere and sleeve are all made of 304 stainless steel.
Citation Information
Patent Citations
Hot isostatic pressing forming method of titanium alloy gas cylinder hemispheroid
CN108971495A
Hot isostatic pressing shape control method for titanium alloy thin-wall part
CN111266588A
Hot isostatic pressing formed high-temperature alloy hemispheroid and preparation method thereof
CN112658253A
Device and method for preparing seamless ceramic hollow floating ball
CN114905618A
Method of manufacturing a metallic component by use of wire winding and hot isostatic pressing